Process for manufacture of fluoropolymers containing ion exchange groups
The environmental and environmental protection methods of traditional fluoropolymer manufacturing methods are solved by polymerizing ethylenically unsaturated fluorinated monomer emulsions of tetrafluoroethylene and hydrolyzable groups by using free radical initiator and high molecular weight multifunctional dispersant in aqueous media. Toxicological problems have achieved efficient and stable preparation of fluoropolymers, avoiding adverse effects on polymer characteristics.
Patent Information
- Application Number
- CN202380024574.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-15
AI Technical Summary
Perfluorooctanoic acid and its salts used in the existing fluoropolymer manufacturing methods are limited due to environmental and toxicological concerns, and surfactants are often required in traditional methods, which affect the performance and environmental friendliness of the polymer.
Emulsion polymerization of tetrafluoroethylene and hydrolyzable ethylenically unsaturated fluorinated monomers in aqueous media by the presence of free radical initiators and multifunctional dispersants, providing surfactivity using high molecular weight multifunctional dispersants and dispersing ability avoids the impact on polymer properties.
It is achieved efficient and stable production of fluoropolymers with excellent weather resistance and aqueous dispersion without using traditional surfactants, reducing the impact on the environment and improving the performance of the polymer.
Smart Images

Figure BDA0005019190300000061 
Figure BDA0005019190300000071 
Figure BDA0005019190300000121
Abstract
Description
[0001] Citation of Related Applications
[0002] This application claims priority from European patent application EP 22159375.9 filed on March 1, 2022, the entire contents of which are incorporated by reference into this application for all purposes. Technical Field
[0003] The present invention relates to a method for preparing fluoropolymer dispersions using certain multifunctional polymer derivatives, and to fluoropolymers obtained thereby. Background Art
[0004] Fluoropolymers, i.e. polymers with a fluorinated backbone, have long been known and have been used in a variety of applications due to several desirable properties, such as heat resistance, chemical resistance, weathering resistance, UV stability, etc. Fluorinated polymers containing ion exchange groups have been used to make proton exchange membranes, for example for fuel cell applications.
[0005] Frequently used processes for producing fluoropolymers involve aqueous emulsion polymerization of one or more fluorinated monomers, usually involving the use of a fluorinated surfactant. Frequently used fluorinated surfactants include perfluorooctanoic acid and its salts, particularly ammonium perfluorooctanoate.
[0006] Recently, perfluoroalkanoic acids with 8 or more carbon atoms have raised environmental concerns. For example, perfluoroalkanoic acids have been found to show bioaccumulation. As a result, efforts are now being made to phase out such compounds and methods have been developed to manufacture fluoropolymer products using alternative surfactants with more favorable toxicological profiles.
[0007] EP 0341716 A (ASAHI GLASS CO LTD) 15 / 11 / 1989 relates to a process for preparing an aqueous dispersion, which comprises subjecting monomers to emulsion polymerization in an aqueous medium in the presence of a fluorinated copolymer comprising units derived from fluoroolefins and units having hydrophilic side chains having groups which may be (i) carboxylic acid groups or carboxylate groups of formula -COOM, (ii) sulfonic acid groups or sulfonate groups of formula -SO3M, and (iii) phosphonic acid groups or phosphonate groups of formula -PO3M (wherein M is hydrogen, an alkali metal, a quaternary ammonium group, or a quaternary phosphonium group), and (iv) amide groups, and which have a number average molecular weight of the order of 1000 to 500000, in particular 3000 to 400000. The monomer to be polymerized is a fluoroolefin having 2 to 4 carbon atoms, such as hexafluoropropylene, pentafluoropropylene, tetrafluoroethylene, chlorotrifluoroethylene, trifluoroethylene or vinylidene fluoride, and a vinyl compound, an allyl compound, a fluorinated vinyl compound or a fluorinated allyl compound is preferred because their polymerization produces an aqueous dispersion capable of providing a coating having excellent weather resistance.
[0008] WO 2012 / 082707 A1 (3M INNOVATIVE PROPERTIES COMPANY) discloses a microemulsion obtained by mixing water, at least one ethylenically unsaturated fluoromonomer, and at least one oligomeric fluorosulfinic acid compound and / or at least one ethylenically unsaturated polymerizable monomeric fluorosulfinic acid compound and its use for polymerizing at least one ethylenically unsaturated fluoromonomer. These oligomeric and polymerizable monomeric fluorosulfinic acid compounds have a low molecular weight and are characterized by the presence of a sulfinic acid / sulfinate functional group -SO2M, where M is a cation.
[0009] WO 2018 / 167190 A1 (SOLVAY SPECIALTYPOLYMERS ITALY SpA) 28 / 09 / 2018 discloses a process for the manufacture of a fluoropolymer, the process comprising emulsion polymerizing one or more than one fluorinated monomer in an aqueous medium in the presence of at least one free radical initiator and at least one multifunctional dispersant, the at least one multifunctional dispersant:
[0010] - comprises a main chain comprising repeating units derived from one or more ethylenically unsaturated monomers,
[0011] - its molecular weight and its molecular weight distribution are such that the dispersant contains substantially no fractions having a molecular weight of less than 3000,
[0012] -Contains multiple options from -SO3Xa 、-PO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal, the amount of the ionic group is at least 1.75 meq / g relative to the weight of the dispersant, wherein the dispersant is used in an amount of 0.01% by weight and 5.00% by weight based on the total weight of the aqueous medium. WO 2018 / 167190 A1 specifically discloses that in the presence of -SO3X a PTFE is prepared in the presence of a dispersant (D) having an ionic group.
[0013] It has been found that the use of certain multifunctional dispersants disclosed in WO 2018 / 167190 A1 can be advantageously used in an aqueous emulsion polymerization process of monomers comprising hydrolyzable groups to provide a dispersion of polymers comprising hydrolyzable groups in the absence of surfactants. Summary of the invention
[0014] A first object of the present invention is a process for producing a fluoropolymer comprising a plurality of hydrolyzable groups [polymer (P)], said process comprising emulsion polymerizing in an aqueous medium in the presence of at least one free radical initiator and at least one multifunctional dispersant [dispersant (D)]:
[0015] - tetrafluoroethylene, and
[0016] - at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group,
[0017] The dispersant (D):
[0018] - having a weight average molecular weight (M) of at least 15,000 and at most 800,000 w ),
[0019] - comprises a backbone comprising repeating units derived from one or more ethylenically unsaturated monomers, and
[0020] -Contains multiple options from -SO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal.
[0021] The applicant has surprisingly found that despite the high molecular weight of the dispersant (D), due to the presence of ionic groups as pendant groups in the fluorinated chain, the dispersant (D) has sufficient surface activity and dispersing power to ensure efficient stabilization of the fluoropolymer in the aqueous polymerization environment.
[0022] Advantageously, the dispersant (D) has a molecular weight and a molecular weight distribution such that it contains substantially no fractions having a molecular weight of less than 3000.
[0023] The amount of the ionic groups in the dispersant (D) is at least 1.00 meq / g relative to the weight of the dispersant (D).
[0024] The hydrolyzable groups in the polymer (P) are preferably selected from -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group.
[0025] The dispersant (D) is used in an amount of 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
[0026] In an advantageous embodiment of the invention, the ionic groups in the dispersant (D) are obtained from hydrolyzable groups of a polymer (P) which is the product of an emulsion polymerization process. In this embodiment, at the end of the polymerization process, the polymer (P) does not require any purification step to remove the residues of the dispersant (D). In fact, due to similar chemical properties, the presence of the dispersant (D) does not have any adverse effect on the properties of the polymer (P).
[0027] In an even more advantageous embodiment of the invention, the dispersant (D) has the same monomer composition as the polymer (P) obtained at the end of the process, the only difference being the presence of the ionic group -SO3X a and-COOX a , replacing the hydrolyzable groups -SO2X and -COOZ as defined above.
[0028] definition
[0029] The expression "fluorinated monomer" is intended here to mean an ethylenically unsaturated monomer comprising at least one fluorine atom.
[0030] When used in relation to a polymer composition comprising a dispersant (D), the expression "consisting essentially of" is meant to indicate that the polymer contains not more than 1 mol % of terminal groups, impurities, defects and other spurious repeating units other than the listed repeating units, relative to the total moles of repeating units.
[0031] Polymer (P)
[0032] The method of the present invention comprises emulsion polymerization of tetrafluoroethylene and at least one ethylenically unsaturated fluorinated monomer containing at least one hydrolyzable group in an aqueous medium. The hydrolyzable group is selected from the group consisting of -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group.
[0033] The polymer (P) preferably comprises repeating units derived from at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group -SO2X (wherein X is a halogen), hereinafter referred to as [monomer (A)].
[0034] Non-limiting examples of suitable monomers (A) are selected from the group consisting of:
[0035] -sulfonyl halofluoroolefin having the formula: CF2=CF(CF2) p SO2X, wherein X is a halogen, preferably F or Cl, more preferably F, wherein p is an integer between 0 and 10, preferably between 1 and 6, more preferably p is equal to 1, 2 or 3;
[0036] -sulfonyl halide fluorovinyl ether having the formula: CF2=CF-O-(CF2) m SO2X, wherein X is a halogen, preferably F or Cl, more preferably F, wherein m is an integer between 1 and 10, preferably between 1 and 6, more preferably between 2 and 4, even more preferably m is equal to 2;
[0037] -sulfonyl halofluoroalkoxy vinyl ether having the formula: CF2=CF-(OCF2CF(R F1 )) w -O-CF2(CF(R F2 )) y SO2X
[0038] wherein X is halogen, preferably F or Cl, more preferably F, wherein w is an integer between 0 and 2, R F1 and R F2 are the same as or different from each other and are independently F, Cl, or C optionally substituted by one or more ether oxygen atoms. 1- C 10 fluoroalkyl, y is an integer between 0 and 6; preferably, w is 1, R F1 is -CF3, y is 1 and R F2 It is F;
[0039] - a sulfonyl halide aromatic fluoroolefin having the formula CF2=CF-Ar-SO2X, wherein X is a halogen, preferably F or Cl, more preferably F, wherein Ar is C 5- C 15 Aromatic or heteroaromatic groups.
[0040] Preferably, monomer (A) is selected from the group consisting of monomers having the formula CF2=CF-O-(CF2) m The group of sulfonyl fluoride fluorovinyl ethers of -SO2F, wherein m is an integer between 1 and 6, preferably between 2 and 4.
[0041] More preferably, monomer (A) is CF2=CFOCF2CF2-SO2F (perfluoro-5-sulfonyl fluoride-3-oxa-1-pentene).
[0042] During the polymerisation process additional fluorinated monomers may be present and incorporated into the polymer (P).
[0043] Non-limiting examples of suitable ethylenically unsaturated fluorinated monomers are:
[0044] -C2-C8 perfluoroolefins, such as hexafluoropropylene and perfluoroisobutylene;
[0045] - C2-C8 hydrogen-containing fluoroolefins, such as trifluoroethylene, vinylidene fluoride, vinyl fluoride, pentafluoropropylene and hexafluoroisobutylene;
[0046] - C2-C8 fluorinated olefins containing chlorine and / or bromine and / or iodine, such as chlorotrifluoroethylene and bromotrifluoroethylene;
[0047] -Has the formula CF2=CFOR f1 A fluoroalkyl vinyl ether, wherein R f1 is C1-C6 fluoroalkyl, such as -CF3, -C2F5, -C3F7;
[0048] - a fluorooxyalkyl vinyl ether of the formula CF2=CFOX0, wherein X0 is a C1-C2- 12 Fluorooxyalkyl, these fluorooxyalkyl vinyl ethers include in particular those having the formula CF2=CFOCF2OR f2 Fluoromethoxyalkyl vinyl ether, wherein R f2 It is a C1-C3 fluoro(oxy)alkyl group, such as -CF2CF3, -CF2CF2-O-CF3 and -CF3
[0049] - Fluorodioxole having the formula:
[0050]
[0051] Where R f3 , R f4 , R f5 , R f6 Each of them is the same as or different from each other and is independently a fluorine atom, a C1-C6 fluoro(halo)fluoroalkyl group optionally containing one or more oxygen atoms, such as -CF3, -C2F5, -C3F7, -OCF3, -OCF2CF2OCF3.
[0052] In addition to tetrafluoroethylene, preferred fluorinated monomers for use in the process of the present invention include chlorotrifluoroethylene, hexafluoropropylene, vinyl fluoride, vinylidene fluoride.
[0053] The polymer (P) is preferably selected from polymers comprising or essentially consisting of:
[0054] 50 to 99 mol %, preferably 50 to 98 mol %, even 5 to 95 mol %, of repeating units derived from tetrafluoroethylene (TFE), relative to the total moles of polymer (P);
[0055] 1 to 50 mol %, preferably 2 to 50 mol %, even 5 to 50 mol %, relative to the total moles of polymer (P) of recurring units derived from at least one monomer selected from the group consisting of:
[0056] (j) Sulfonyl halide fluorovinyl ether having the formula: CF2=CF-O-(CF2) m SO2X, wherein X is a halogen, preferably F or Cl, more preferably F, wherein m is an integer between 1 and 10, preferably between 1 and 6, more preferably between 2 and 4, even more preferably m is equal to 2;
[0057] (jj) Sulfonyl halide fluoroalkoxy vinyl ether having the formula: CF2=CF-(OCF2CF(R F1 )) w -O-CF2(CF(R F2 )) y SO2X, wherein X is halogen, preferably F or Cl, more preferably F, wherein w is an integer between 0 and 2, R F1 and R F2 are the same as or different from each other and are independently F, Cl, or C optionally substituted by one or more ether oxygen atoms. 1- C 10 fluoroalkyl, y is an integer between 0 and 6; preferably, w is 1, R F1 is -CF3, y is 1 and R F2 is F; and
[0058] (jjj) mixtures thereof; and
[0059] - 0 to 45 mol %, preferably 0 to 40 mol %, even 0 to 25 mol %, relative to the total moles of polymer (P), of recurring units derived from at least one hydrogenated and / or fluorinated monomer, preferably perfluorinated monomer, different from TFE, these monomers being generally chosen from the group consisting of: hexafluoropropylene; monomers having the formula CF2=CFOR' f1 Perfluoroalkyl vinyl ether, wherein R' f1 is a C1-C6 perfluoroalkyl group, such as -CF3, -C2F5, -C3F7; having the formula CF2=CFOR' O1 Perfluoroalkyl vinyl ether, wherein R' O1is a C2-C 12 Perfluoroalkyl groups, including for example those having the formula CF2=CFOCF2OR' f2 Perfluoroalkyl-methoxy-vinyl ether, wherein R' f2 is a C1-C6 perfluoroalkyl group, such as -CF3, -C2F5, -C3F7, or a C1-C6 perfluorooxyalkyl group having one or more ether groups, such as -C2F5-O-CF3; a fluorodioxole having the formula:
[0060]
[0061] Among them, R f3 , R f4 , R f5 , R f6 Each of them is the same as or different from each other and is independently a fluorine atom, a C1-C6 fluoro(halo)fluoroalkyl group optionally containing one or more oxygen atoms, such as -CF3, -C2F5, -C3F7, -OCF3, -OCF2CF2OCF3, preferably -OCF3.
[0062] According to certain embodiments, polymer (P) comprises, consists essentially of, or consists of:
[0063] (1) 50 to 95 mol %, preferably 55 to 93 mol % of repeating units derived from TFE;
[0064] (2) 5 to 50 mol %, preferably 7 to 45 mol %, of repeating units derived from monomer (A) containing -SO2X groups as described in detail above;
[0065] (3) 0 to 25 mol %, preferably 0 to 20 mol %, of repeating units derived from one or more fluorinated monomers other than TFE as detailed above.
[0066] The polymer (P) typically has a weight average molecular weight (M) of at least 50,000, preferably at least 85,000, more preferably at least 100,000 as measured by GPC relative to polystyrene standards using dimethylacetamide as eluent. w ).
[0067] The weight average molecular weight (M) of the polymer (P) as measured by GPC relative to polystyrene standards using dimethylacetamide as eluent w ) is generally at most 700000, preferably at most 600000, more preferably at most 500000. For most applications of polymer (P), a suitable range is, for example, 150000 to 600000, preferably 180000 to 500000.
[0068] Preferably, polymer (P) has a number average molecular weight of at least 50000, preferably at least 90000 and / or advantageously at most 500000, preferably at most 450000 as measured by GPC against polystyrene standards using dimethylacetamide as eluent. The GPC method is described in detail in the experimental part.
[0069] Dispersant (D)
[0070] The multifunctional dispersant (D) comprises a main chain comprising repeating units derived from one or more ethylenically unsaturated monomers; and a plurality of a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal. The dispersant (D) does not contain unsaturated carbon-carbon bonds.
[0071] The dispersant (D) is used in an amount of 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
[0072] The amount of dispersant (D) in the emulsion polymerization process is at least 0.05 wt%, preferably at least 0.10 wt% and advantageously up to 4.00 wt%, preferably up to 3.50 wt%, even more preferably up to 3.00 wt% relative to the total weight of the aqueous medium. A practical range is between 0.10 wt% and 2.75 wt%, preferably between 0.25 wt% and 2.00 wt%, even between 0.50 wt% and 1.75 wt%, relative to the total weight of the aqueous medium. In certain embodiments, the dispersant (D) is present in an amount between 0.25 wt% and 1.50 wt% relative to the total weight of the aqueous medium.
[0073] Although the polymerization is generally initiated in the presence of a dispersant (D), it is not excluded that further dispersants (D) are added during the polymerization, although this is generally not necessary.
[0074] The dispersant (D) has a weight average molecular weight (MW) of at least 15,000 as measured by GPC relative to polystyrene standards using dimethylacetamide as eluent. w ). The GPC method is described in detail in the experimental section.
[0075] The weight average molecular weight (M) of the dispersant (D) as measured by GPC relative to polystyrene standards using dimethylacetamide as the eluent w ) is not particularly critical, provided that the dispersant (D) has an amount of ionic groups per weight of the dispersant which enables the dispersant to have sufficient dispersibility.
[0076] However, it will be appreciated that a practical range of weight average molecular weight of the dispersant (D) is generally up to 800,000, up to 600,000, preferably up to 500,000, more preferably up to 400,000.
[0077] Preferably, the dispersant (D) has a weight average molecular weight of at least 20,000, preferably at least 25,000, advantageously at least 50,000, at least 100,000, or even at least 150,000.
[0078] Particularly good results are obtained with dispersants having a weight average molecular weight of 50,000 to 400,000, or even 150,000 to 400,000.
[0079] The dispersant (D) may advantageously have a number average molecular weight (M) of 7,000 to 500,000, preferably 25,000 to 400,000, or even 50,000 to 250,000. n ).
[0080] Advantageously, the dispersant (D) is a polymer having a molecular weight and a molecular weight distribution such that the dispersant (D) is substantially free of fractions having a molecular weight of less than 3,000.
[0081] The substantial absence of a molecular weight fraction less than 3000 can be determined using GPC techniques relative to polystyrene standards using dimethylacetamide as the eluent. The GPC method is described in detail in the experimental section.
[0082] The expression "substantially free" in relation to dispersant (D) and the fraction with a molecular weight less than 3000 is intended to mean that said fraction is present in an amount of at most 0.03 wt%, preferably at most 0.01 wt%, and more preferably said fraction is not detectable by the GPC technique as detailed above.
[0083] The dispersant (D) comprises a plurality of selected from -SO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal. The monovalent metal is typically selected from the group of alkali metals, preferably it is sodium or potassium.
[0084] Preferably, the dispersant (D) comprises a plurality of selected from -SO3X a The ionic groups composed of X a Selected from H, an ammonium group or a monovalent metal.
[0085] The amount of the ionic groups in the dispersant (D) is typically at least 1.00 meq / g, at least 1.10 meq / g, preferably at least 1.20 meq / g, more preferably at least 1.30 meq / g relative to the weight of the dispersant (D). It is believed that dispersants (D) having ionic groups in an amount less than 1.00 meq / g lack sufficient polarity to dissolve in the aqueous phase and produce a stabilizing / surfactant-like effect. There is no substantial limitation on the maximum amount of the ionic groups in the dispersant (D). It is generally understood that the ionic groups are typically present in an amount of up to 2.50 meq / g, preferably up to 2.20 meq / g, more preferably up to 2.00 meq / g.
[0086] The dispersant (D) comprises the ionic group as a pendant group covalently bonded to a repeating unit derived from an ethylenically unsaturated functional monomer [monomer (X)].
[0087] The dispersant (D) may consist essentially of repeating units derived from one or more than one monomer (X), or it may be a copolymer comprising repeating units derived from one or more than one monomer (X) and repeating units derived from one or more than one additional monomer different from monomer (X).
[0088] Typically, monomer (X) is a fluorinated monomer; the one or more additional monomers different from monomer (X) may be fluorinated monomers.
[0089] According to certain embodiments of the present invention, the dispersant (D) comprises a plurality of -SO3X a Group polymer.
[0090] The dispersant (D) may be substantially derived from one or more than one compound containing -SO3X a Alternatively, the dispersant (D) may comprise a monomer derived from one or more than one compound containing -SO3X a The repeating units of the monomers of the group and derived from one or more than one non-SO3X a The repeating unit of the monomer of the group.
[0091] With the inclusion of -SO3X a The expression "a repeating unit derived from..." in relation to a monomer of a group is intended to encompass i) a repeating unit derived from / obtained directly from polymerizing said monomer, and ii) a repeating unit derived from / obtained from polymerizing a monomer comprising -SO3X a The monomers of the functional group precursors of the group are then modified and / or post-treated (e.g. by hydrolysis) to the polymer. In other words, the monomers comprising the functional group precursors derived from one or more than one group comprising -SO3X aThe dispersant containing repeating units of a monomer containing -SO2X groups can be obtained by polymerizing a monomer containing -SO2X groups and then hydrolyzing it. For the avoidance of doubt, the dispersant (D) contains -SO3X a Ionic groups.
[0092] Contains multiple -SO3X a Suitable dispersants (D) of the group are polymers comprising repeating units derived from:
[0093] - at least one ethylenically unsaturated fluorinated monomer containing at least one -SO2X group, wherein X is a halogen (e.g. F) or -OX a , where X a is H, an ammonium group, or a monovalent metal; and
[0094] - repeating units derived from at least one ethylenically unsaturated fluorinated monomer not containing a -SO2X group (hereinafter [monomer (B)]).
[0095] Ethylenically unsaturated fluorinated monomers containing at least one -SO2X group suitable for preparing the dispersant (D) may be selected from the list consisting of monomers (A) detailed above, wherein X is halogen (e.g. F) or -OX a , where X a =H, ammonium group or monovalent metal.
[0096] With respect to both types of monomers (A) and (B), the phrase "at least one monomer" is used herein to indicate that one or more than one monomer of each type may be present in the dispersant (D). Hereinafter, the term monomer will be used to refer to both one and more than one monomer of a given type.
[0097] Non-limiting examples of suitable ethylenically unsaturated fluorinated monomers of type (B) are:
[0098] -C2-C8 perfluoroolefins, such as tetrafluoroethylene, hexafluoropropylene, and perfluoroisobutylene;
[0099] - C2-C8 hydrogen-containing fluoroolefins, such as trifluoroethylene, vinylidene fluoride, vinyl fluoride, pentafluoropropylene and hexafluoroisobutylene;
[0100] - C2-C8 fluorinated olefins containing chlorine and / or bromine and / or iodine, such as chlorotrifluoroethylene and bromotrifluoroethylene;
[0101] -Has the formula CF2=CFOR f1 A fluoroalkyl vinyl ether, wherein R f1 is C1-C6 fluoroalkyl, such as -CF3, -C2F5, -C3F7;
[0102] - a fluorooxyalkyl vinyl ether of the formula CF2=CFOX0, wherein X0 is a C1-C2- 12 Fluorooxyalkyl, these fluorooxyalkyl vinyl ethers include in particular those having the formula CF2=CFOCF2OR f2 Fluoromethoxyalkyl vinyl ether, wherein R f2 It is a C1-C3 fluoro(oxy)alkyl group, such as -CF2CF3, -CF2CF2-O-CF3 and -CF3
[0103] - Fluorodioxole having the formula:
[0104]
[0105] Where R f3 , R f4 , R f5 , R f6 Each of them is the same as or different from each other and is independently a fluorine atom, a C1-C6 fluoro(halo)fluoroalkyl group optionally containing one or more oxygen atoms, such as -CF3, -C2F5, -C3F7, -OCF3, -OCF2CF2OCF3.
[0106] Preferably, monomer (B) is selected from:
[0107] - C2-C8 perfluoroolefins selected from tetrafluoroethylene and / or hexafluoropropylene;
[0108] - a C2-C8 hydrogen-containing fluoroolefin selected from trifluoroethylene, vinylidene fluoride and vinyl fluoride; and
[0109] - mixtures thereof.
[0110] More preferably, monomer (B) is tetrafluoroethylene.
[0111] In a preferred embodiment, the dispersant (D) is a a A fluorinated polymer having a functional group, and the fluorinated polymer consists essentially of, consists of: derived from at least one containing at least one -SO3X a The present invention relates to an ethylenically unsaturated fluorinated monomer of the present invention and a repeating unit derived from at least one ethylenically unsaturated fluorinated monomer (B).
[0112] According to certain embodiments, at least one monomer (B) of the dispersant (D) is TFE.
[0113] Preferred dispersants (D) are selected from the group consisting of polymers comprising, consisting essentially of:
[0114] 50 to 99 mol %, preferably 50 to 98 mol %, even 50 to 95 mol % of repeating units derived from tetrafluoroethylene (TFE), relative to the total moles of dispersant (D);
[0115] 1 to 50 mol %, preferably 2 to 50 mol %, even 5 to 50 mol %, relative to the total moles of dispersant (D) of repeating units derived from at least one monomer selected from the group consisting of:
[0116] (j) Sulfonyl halide fluorovinyl ether having the formula: CF2=CF-O-(CF2) m SO2X, where X is OX a (Where X a as detailed above), or X is halogen, preferably F or Cl, more preferably F, wherein m is an integer between 1 and 10, preferably between 1 and 6, more preferably between 2 and 4, even more preferably m is equal to 2;
[0117] (jj) Sulfonyl halide fluoroalkoxy vinyl ether having the formula: CF2=CF-(OCF2CF(R F1 )) w -O-CF2(CF(R F2 )) y SO2X
[0118] Where X is OX a (Where X a As described above), or X is halogen, preferably F or Cl, more preferably F, wherein w is an integer between 0 and 2, R F1 and R F2 are the same as or different from each other and are independently F, Cl, or C1-C1 optionally substituted by one or more ether oxygen atoms. 10 fluoroalkyl, y is an integer between 0 and 6; preferably, w is 1, R F1 is -CF3, y is 1 and R F2 is F; and
[0119] (jjj) mixtures thereof; and
[0120] - 0 to 45 mol %, preferably 0 to 40 mol %, even 0 to 25 mol %, relative to the total moles of dispersant (D), of recurring units derived from at least one hydrogenated and / or fluorinated monomer, preferably perfluorinated monomer, different from TFE, these monomers being generally chosen from the group consisting of: hexafluoropropylene; monomers having the formula CF2=CFOR' f1 Perfluoroalkyl vinyl ether, wherein R' f1 is a C1-C6 perfluoroalkyl group, such as -CF3, -C2F5, -C3F7; having the formula CF2=CFOR'O1 Perfluoroalkyl vinyl ether, wherein R' O1 is a C2-C 12 Perfluoroalkyl groups, including for example those having the formula CF2=CFOCF2OR' f2 Perfluoroalkyl-methoxy-vinyl ether, wherein R' f2 It is a C1-C6 perfluoroalkyl group, such as -CF3, -C2F5, -C3F7, or a C1-C6 perfluorooxyalkyl group having one or more ether groups, like -C2F5-O-CF3.
[0121] According to certain embodiments, the preferred dispersant (D) comprises, consists essentially of:
[0122] - 50 to 95 mol %, preferably 55 to 93 mol % of repeating units derived from TFE;
[0123] - 5 to 50 mol %, preferably 7 to 45 mol %, of repeating units derived from one or more monomers containing -SO2X groups (monomer (A));
[0124] 0 to 25 mol %, preferably 0 to 20 mol %, of recurring units derived from one or more fluorinated monomers different from TFE (monomer (B)).
[0125] In an advantageous embodiment of the present invention, both the polymer (P) and the dispersant (D) comprise:
[0126] - 50 to 95 mol %, preferably 55 to 93 mol % of repeating units derived from TFE;
[0127] - 5 to 50 mol %, preferably 7 to 45 mol %, of repeating units derived from one or more monomers containing -SO2X groups (monomer (A));
[0128] 0 to 25 mol %, preferably 0 to 20 mol %, of recurring units derived from one or more fluorinated monomers different from TFE (monomer (B)).
[0129] In certain embodiments of the present invention, the dispersant (D) has the same molar composition as the polymer (P).
[0130] In a very advantageous embodiment of the present invention, after the hydrolysis of the hydrolyzable groups, the polymer (P) is used as a dispersant in a further polymerization process.
[0131] Therefore, the method of the present invention comprises the following steps: recovering the polymer (P), hydrolyzing the hydrolyzable -SO2X groups to obtain -SO3X a group, thereby obtaining a dispersant (D).
[0132] Thus, the process of the present invention comprises the step of preparing the dispersant (D) by emulsion polymerizing in an aqueous medium in the presence of at least one free radical initiator and a dispersant [dispersant (Dx)]:
[0133] - tetrafluoroethylene, and
[0134] - at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group selected from -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group,
[0135] To obtain a polymer containing multiple hydrolyzable groups; hydrolyze these hydrolyzable groups to obtain the corresponding ionic groups -SO3X a and-COOX a , where X a is H, an ammonium group or a monovalent metal.
[0136] The dispersant (Dx) is present in an amount of 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
[0137] The dispersant (D) may be any dispersant known in the art for the preparation of fluoropolymers. Advantageously, the dispersant (Dx) is a dispersant (D).
[0138] Thus, in an advantageous embodiment, the process of the invention comprises the step of preparing the dispersant (D) by emulsion polymerizing in an aqueous medium in the presence of at least one free radical initiator and a dispersant (Dx):
[0139] - tetrafluoroethylene, and
[0140] - at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group selected from -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group,
[0141] The dispersant (Dx) has a weight average molecular weight of 15,000 to 800,000; comprises a main chain comprising repeating units derived from one or more ethylenically unsaturated monomers; and comprises a plurality of selected from -SO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group, or a monovalent metal;
[0142] To obtain a polymer containing multiple hydrolyzable groups; hydrolyze these hydrolyzable groups to obtain the corresponding ionic groups -SO3X a and-COOX a , where X ais H, an ammonium group or a monovalent metal.
[0143] The dispersant (Dx) has a molecular weight and molecular weight distribution such that it is substantially free of fractions having a molecular weight less than 3000 as measured by GPC relative to polystyrene standards using dimethylacetamide as eluent. The GPC method is described in detail in the experimental section.
[0144] The amount of the ionic groups in the dispersant (Dx) is at least 1.00 meq / g relative to the weight of the dispersant (Dx).
[0145] The dispersant (Dx) is present in the emulsion polymerization medium in an amount of 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
[0146] The dispersant (Dx) has the same monomer composition, average molecular weight and molecular weight distribution as the dispersant (D) obtained at the end of the process.
[0147] Dispersant (D) and polymer (P) can be prepared by any polymerization process known in the art. Suitable methods for preparing such polymers are for example those described in US 4940525 (Dow Chemical Company (THE DOW CHEMICAL COMPANY)) 10 / 07 / 1990, EP 1323751A (Solvay Solexis SPA)) 2 / 07 / 2003, EP 1172382 A (Solvay Solexis SPA) 16 / 11 / 2002.
[0148] The aqueous emulsion polymerization may be carried out at a temperature between 10°C and 150°C, preferably between 20°C and 130°C, and a pressure typically between 2 and 60 bar, in particular 5 to 45 bar.
[0149] The reaction temperature can be varied during the polymerization, for example, in order to influence the molecular weight distribution, ie, to obtain a broad molecular weight distribution or to obtain a bimodal or multimodal molecular weight distribution.
[0150] The pH of the polymerization medium may be in the range of pH 1-10, preferably 2-10.
[0151] As described, the method of the present invention is carried out in the presence of at least one free radical initiator (i.e. any initiator known to initiate free radical polymerization of ethylenically unsaturated monomers) in an aqueous medium. Suitable free radical initiators include peroxides and azo compounds and redox-based initiators in particular. Specific examples of peroxide initiators include: hydrogen peroxide, sodium peroxide or barium peroxide, diacyl peroxides such as diacetyl peroxide, disuccinic anhydride peroxide, dipropionyl peroxide, dibutyryl peroxide, dibenzoyl peroxide, di-tert-butyl peroxide, benzoylacetyl peroxide, diglutaric acid peroxide, and dilauroyl peroxide, and other peracids and salts, such as ammonium, sodium or potassium salts. Examples of peracids include peracetic acid. Esters of peracids may also be used and examples thereof include tert-butyl peroxyacetate and tert-butyl peroxypivalate. Examples of inorganic initiators include ammonium salts, alkali metal salts or alkaline earth metal salts of, for example, persulfate, permanganic acid or manganic acid. Persulfate initiators (e.g., ammonium persulfate (APS)) can be used alone or in combination with a reducing agent. Suitable reducing agents include bisulfites such as ammonium bisulfite or sodium metabisulfite, thiosulfates such as ammonium thiosulfate, potassium thiosulfate or sodium thiosulfate, hydrazine, azodicarboxylates and azodicarboxylic acid diamides (ADA). Further, reducing agents that can be used include sodium formaldehyde sulfoxylate (Rongalite) or fluoroalkyl sulfinates, such as those disclosed in US 5285002. Reducing agents typically reduce the half-life of persulfate initiators. In addition, metal salt catalysts such as copper salts, iron salts or silver salts can be added.
[0152] The amount of initiator may be between 0.01% by weight (based on the fluoropolymer to be produced) and 1.00% by weight. Nevertheless, the amount of initiator is preferably between 0.05% and 0.50% by weight and more preferably between 0.05% and 0.30% by weight based on the fluoropolymer to be produced.
[0153] The aqueous emulsion polymerization can be carried out in the presence of other materials such as, inter alia, paraffin waxes, buffers and, if desired, complex-formers or chain transfer agents.
[0154] Examples of usable chain transfer agents include dimethyl ether, methyl tert-butyl ether, alkanes having 1 to 5 carbon atoms, such as ethane, propane and n-pentane, halogenated hydrocarbons, such as CCl4, CHCl3 and CH2Cl2; and hydrofluorocarbon compounds, such as CH2F-CF3 (R134a). In addition, in the method of the present invention, esters such as ethyl acetate and malonate can be effective as chain transfer agents.
[0155] Furthermore, the aqueous emulsion polymerization of the process of the present invention can be carried out in the presence of certain fluorinated fluids without ionic groups, which are typically capable of forming nano-sized droplets (average particle size less than 50 nm, preferably less than 30 nm) and are advantageously stabilized in aqueous dispersions by the presence of a dispersant (D).
[0156] If the process of the invention is carried out in the presence of a fluorinated fluid as detailed above, it may be preferred to firstly mix the dispersant (D) with said fluid homogeneously in an aqueous medium and then feed the aqueous mixture of dispersant (D) and said fluid thus obtained in the polymerization medium. This technique is particularly advantageous since such premixing advantageously enables the manufacture of an emulsion of said fluid in an aqueous phase comprising the dispersant (D), wherein this emulsion comprises dispersed droplets of said fluid having an average size preferably less than 50 nm, more preferably less than 40 nm, even more preferably less than 30 nm.
[0157] The fluid that can be used according to this embodiment is preferably a (per)fluoropolyether comprising a repeating unit (R1) comprising at least one ether bond in the main chain and at least one fluorine atom (fluoropolyoxyalkylene chain). Preferably, the repeating unit R1 of the (per)fluoropolyether is selected from the group consisting of:
[0158] (I) -CFX-O-, wherein X is -F or -CF3; and
[0159] (II) -CF2-CFX-O-, wherein X is -F or -CF3; and
[0160] (III) -CF2-CF2-CF2-O-; and
[0161] (IV) -CF2-CF2-CF2-CF2-O-; and
[0162] (V)-(CF2) j -CFZ-O-, wherein j is an integer selected from 0 and 1, and Z is a fluoropolyoxyalkylene chain comprising 1 to 10 repeating units selected from classes (I) to (IV) above; and mixtures thereof.
[0163] If the (per)fluoropolyether comprises different types of repeating units R1, said repeating units are advantageously distributed randomly along the fluoropolyoxyalkylene chain.
[0164] Preferably, the (per)fluoropolyether is a compound conforming to the following formula (Ip):
[0165] T1-(CFX) p -OR f -(CFX) p’-T2(Ip)
[0166] in:
[0167] - each X is independently F or CF3;
[0168] - p and p' are the same as or different from each other and are integers from 0 to 3;
[0169] -R f is a fluoropolyoxyalkylene chain comprising repeating units R° selected from the group consisting of:
[0170] (i) -CFXO-, where X is F or CF3,
[0171] (ii) -CF2CFXO-, where X is F or CF3,
[0172] (iii) -CF2CF2CF2O-,
[0173] (iv) -CF2CF2CF2CF2O-,
[0174] (v)-(CF2) j -CFZ-O-, wherein j is an integer selected from 0 and 1, and Z is a compound having the general formula -OR f 'T3 group, wherein R f ' is a fluoropolyoxyalkylene chain including from 0 to 10 repeating units, the repeating units being selected from the following items: -CFXO-, -CF2CFXO-, -CF2CF2CF2O-, -CF2CF2CF2CF2O-, wherein each X is independently F or CF3; and T3 is a C1-C3 perfluoroalkyl group, and mixtures thereof;
[0175] - T1 and T2 are the same as or different from each other and are H, a halogen atom, or a C1-C3 fluoroalkyl group which optionally contains one or more H or halogen atoms other than fluorine.
[0176] Generally speaking, the process of the present invention is carried out in the substantial absence of fluorinated emulsifiers having a molecular weight of less than 1000.
[0177] When used in conjunction with fluorinated emulsifiers, the expression "substantially absent" means that no surfactant is intentionally added to the polymerization. Although impurities that may be characterized as fluorinated surfactants having a molecular weight of less than 1000 may be tolerated, their amounts are generally below the detection limit of standard analytical techniques (<1 ppm relative to the aqueous medium).
[0178] More generally, the process of the present invention is carried out in the substantial absence of fluorinated emulsifiers having a molecular weight of less than 3,000.
[0179] More precisely, the process of the invention comprises polymerizing in an aqueous medium substantially free of a fluorinated emulsifier [surfactant (FS)] having the formula:
[0180] R f§ (X - ) j (M + ) j
[0181] Where R f§ It is C3-C 30 (Per)fluoroalkyl chain, (per)fluoro(poly)oxyalkylene chain, X - Yes - COO - 、-PO3 - or -SO3 - , M + Selected from H + NH4 + , alkali metal ion, and j can be 1 or 2.
[0182] As non-limiting examples of surfactants (FS), mention may be made of ammonium and / or sodium (per)fluoro(oxy)carboxylates, and / or (per)fluoropolyoxyalkylenes having one or more carboxyl end groups.
[0183] Examples of fluorinated surfactants, in particular (per)fluorooxyalkylene surfactants are described inter alia in US2007015864 (3M Innovations Ltd.) 8 / 01 / 2007, US 2007015865 (3M Innovations Ltd.) 18 / 01 / 2007, US2007015866 (3M Innovations Ltd.) 18 / 01 / 2007, US2007025902 (3M Innovations Ltd.) 1 / 02 / 2007.
[0184] For example, fluorinated emulsifiers [surfactants (FS)] which are essentially excluded from the process of the invention are, in particular:
[0185] -CF3(CF2) n1 COOM', wherein n1 is an integer ranging from 4 to 10, preferably from 5 to 7, and more preferably equal to 6; M' represents H, NH4, Na, Li or K, preferably NH4;
[0186] -T(C3F6O) n0 (CFXO) m0 CF2COOM", wherein T represents Cl or has the formula C k F 2k+1O, wherein k is an integer from 1 to 3, one F atom is optionally substituted by a Cl atom; n0 is an integer ranging from 1 to 6; m0 is an integer ranging from 0 to 6; M" represents H, NH4, Na, Li or K; X represents F or CF3;
[0187] -F-(CF2CF2) n2 -CH2-CH2-RO3M"', wherein R is P or S, preferably S, M'" represents H, NH4, Na, Li or K, preferably H; n2 is an integer ranging from 2 to 5, preferably n2 = 3;
[0188] -AR f -B bifunctional fluorinated surfactant, wherein A and B are the same or different from each other, is -(O) p CFX-COOM*; M* represents H, NH4, Na, Li or K, preferably M* represents NH4; X=F or CF3; p is an integer equal to 0 or 1; R f is a linear or branched perfluoroalkyl chain, or a (per)fluoropolyether chain, such that AR f - The number average molecular weight of B is in the range of 300 to 1,000;
[0189] -R' f -O-(CF2) r -OL-COOM', where R' f is a linear or branched perfluoroalkyl chain, optionally containing catenary oxygen atoms, M' is H, NH4, Na, Li or K, preferably M' represents NH4; r is 1 to 3; L is a divalent fluorinated bridging group, preferably -CF2CF2- or -CFX-, X=F or CF3;
[0190] -R" f -(OCF2) u -O-(CF2) v -COOM", where R" f is a linear or branched perfluoroalkyl chain, optionally containing catenary oxygen atoms, M" is H, NH4, Na, Li or K, preferably M" represents NH4; u and v are integers from 1 to 3;
[0191] -R"' f -(O) t -CHQ-L-COOM'", its R'" f is a linear or branched perfluoroalkyl chain, optionally containing catenary oxygen atoms, Q=F or CF3, t is 0 or 1, M'" is H, NH4, Na, Li or K, preferably M'" is NH4; L is a divalent fluorinated bridging group, preferably -CF2CF2- or -CFX-, X=F or CF3;
[0192] - a cyclic fluorine compound having the following formula (I):
[0193]
[0194] wherein X1, X2, and X3 are the same or different from each other and are independently selected from H, F, and C optionally containing one or more chain or non-chain oxygen atoms. 1-6 (Per)fluoroalkyl; L represents a bond or a divalent group; R F It is divalent fluorinated C 1-3 A bridging group; Y is a hydrophilic functional group selected from the group consisting of:
[0195]
[0196] Where X a is H, a monovalent metal (preferably an alkali metal) or a compound having the formula -N(R' n )4 ammonium group, wherein R' n The same or different at each occurrence, representing a hydrogen atom or a C 1-6 Hydrocarbon group.
[0197] The process of the invention typically produces an aqueous dispersion of fluoropolymer further comprising a dispersant (D) as detailed above.
[0198] The particle size (volume mean diameter) of the fluoropolymer is typically between 40 nm and 400 nm, with a typical particle size of between 60 nm and about 350 nm being preferred.
[0199] If the fluoropolymer is desired in solid form, the fluoropolymer may be isolated from the dispersion by coagulation or any other suitable technique.
[0200] Advantageously, the present invention may further comprise a step of obtaining the polymer (P) in its ionic form as a powdery material [material (PP)], said powdery material consisting of a plurality of particles of at least one polymer comprising a plurality of a and-COOX a The ionic groups composed of X a is H, an ammonium group or a metal, preferably a monovalent metal, the method comprising:
[0201] (1) providing an aqueous dispersion of particles comprising a polymer (P), wherein the polymer comprises a plurality of X and-COOX y A hydrolyzable group consisting of x is halogen, in particular F or Cl, and X y is C1-C4 alkoxy; and
[0202] (2) contacting the aqueous dispersion with an alkaline hydrolyzing agent to at least partially hydrolyze the group -SO2X X and-COOX y Converted into the corresponding group -SO3X b and-COOX b --where X b is an ammonium group or a monovalent metal, without causing any significant coagulation, so as to obtain an aqueous dispersion of particles of the polymer (P) in ionic form; optionally
[0203] (3) contacting the dispersion obtained at the end of step (2) with at least one ion exchange resin in order to at least partially remove residues of the alkaline hydrolysis agent and / or other contaminants; and
[0204] (4) Spray drying the dispersion obtained at the end of step (2) and optionally step (3) in order to obtain material (PP).
[0205] The at least one ion exchange resin in step (3) can be an anion exchange resin, a cation exchange resin, or both.
[0206] When X a is H, the method comprises the step of: b With cation H + Exchange step. The ion exchange can be performed in step (3) using a cation exchange resin or by any other known method such as electrodialysis on a bipolar membrane.
[0207] A method for recovering a polymer (P) as a powder from an emulsion polymerization latex is described in WO 2020 / 094563 A1, the content of which is incorporated herein by reference.
[0208] The method for obtaining material (PP) may comprise an additional step of purifying the dispersion. Examples of suitable techniques include dialysis, electrodialysis and ultrafiltration. The additional purification step may be performed at any stage, typically between step (2) and step (4). When optional step (3) is present, the additional purification step is performed between step (2) and step (3), or preferably between step (3) and step (4).
[0209] Other methods for recovering polymer (P) as powder from emulsion polymerization latex are disclosed, for example, in WO 22224105 A1, the content of which is incorporated herein by reference.
[0210] Depending on the requirements of the application in which the fluoropolymer is to be used, the fluoropolymer in powder form may be post-fluorinated in order to convert any chemically unstable end groups into stable -CF3 end groups.
[0211] For coating applications, aqueous dispersions of the fluoropolymer are desirable, and thus there is no need to separate or coagulate the fluoropolymer from the dispersion. In order to obtain a fluoropolymer dispersion suitable for use in coating applications (such as, for example, in the impregnation of a fabric or other porous support), it is generally desirable to add additional stabilizing surfactants and / or further increase fluoropolymer solids. For example, a nonionic stabilizing surfactant may be added to the fluoropolymer dispersion.
[0212] The amount of fluoropolymer solids in the dispersion may be increased to an amount between 30 and 70 wt% as needed or desired.Any known concentration technique may be used, including ultrafiltration and thermal concentration.
[0213] In a preferred embodiment of the present invention, the polymer (P) is used for preparing a membrane for use in a polymer electrolyte membrane fuel cell.
[0214] Should the disclosure of any patents, patent applications, and publications incorporated by reference into this application conflict with the description of this application to the extent that a term may be unclear, this description shall take precedence.
[0215] The present invention will now be described in more detail with reference to the following examples, which are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0216] Preparation Example 1 - Preparation of Dispersant (D-1) by Polymerization and Sequential Hydrolysis of Tetrafluoroethylene (TFE) and Perfluoro-5-Sulfonyl Fluoride-3-Oxa-1-Pentene (SFVE)
[0217] Step 1 - Aggregation
[0218] The following reagents were placed in a 5 L autoclave:
[0219] - 1.8L of demineralized water;
[0220] - 533 g of a monomer having the formula: CF2=CF-O-CF2CF2-SO2F (SFVE);
[0221] - 89 g of a 46 wt% aqueous solution of an ammonium salt of a fluorine compound having the formula:
[0222]
[0223] wherein Xa is NH4.
[0224] The autoclave stirred at 650 rpm was heated at 58°C. An amount of 90 mL of an aqueous solution of ammonium persulfate with 16 g / L was added. The pressure was maintained at a value of 8.5 bar (absolute pressure) by 8.2 bar of feed tetrafluoroethylene (TFE). After the initial addition of 83 g, SFVE (23 g) was added in batches of 5 wt% of converted TFE per batch. The reaction was stopped after 200 min by stopping stirring, the autoclave was cooled and the pressure was reduced by venting the TFE; a total of 340 g of TFE was fed into the autoclave. In general, 0.12 g of surfactant was used per gram of converted TFE.
[0225] The latex thus obtained was degassed with a stream of air for 48 h to remove the residues of monomers and then coagulated by freeze-thawing.The powder was washed with deionized water (4 x 1 L) for 30 min and dried in a ventilated oven at 120°C overnight.
[0226] A copolymer was obtained which had an equivalent weight (EW) of 720 g / mol and had the following composition: TFE: 81.5 mol %; SFVE: 18.5 mol %, as determined by FT-IR measurements.
[0227] The polymer has a number average molecular weight (M) of 93,000. n ) and a weight average molecular weight (M w ). Substantially no fraction with a molecular weight lower than 3000 was detected by GPC.
[0228] GPC measurements were performed using an RI detector in dimethylacetamide as solvent against polystyrene standards. The concentration of the copolymer in the test solution was 0.5% wt / vol.
[0229] Step 2 - Stabilization, hydrolysis and dissolution in water
[0230] 250 g of the powder obtained in step 1 was treated with a mixture of 10 L / h of fluorine and 4 L / h of nitrogen at 70° C. for 3 hours to terminate the main chain with -CF3 functional groups and remove unwanted carboxylic acid groups. The powder was treated with 1.5 L of a NaOH / H2O (20 wt%) solution under stirring and heated at 80° C. It was confirmed by solid-state NMR that the initially contained -SO2F groups were completely converted to -SO3 - Ionic groups. The amount of ionic groups in the polymer was 1.39 meq / g. After 10 h, the powder was washed with deionized water (4×1 L) for 30 min under stirring and dissolved in deionized water in a pressurized vessel heated at 250° C.
[0231] Polymerization Example 2: Polymerization of tetrafluoroethylene (TFE) and perfluoro-5-sulfonyl fluoride-3-oxa-1-pentene (SFVE) in the presence of a dispersant (D-1)
[0232] The following reagents were placed in a 5 L autoclave:
[0233] - 1.8L of demineralized water;
[0234] 20 g of a 25 wt % aqueous dispersion of dispersant (D-1) obtained from Preparation Example 1 (ie corresponding to 5 g of dispersant (D-1)), thus corresponding to a concentration of about 1.05 wt % based on the initial aqueous phase.
[0235] The autoclave was heated at 50° C. with stirring at 650 rpm. An amount of 90 mL of a 16 g / L aqueous solution of sodium persulfate was added. The pressure was maintained at a value of 7.6 bar (absolute) by feeding tetrafluoroethylene (TFE).
[0236] 82 g of SFVE were fed into the reactor and the pressure of the autoclave was maintained at a constant value of 7.8 bar by feeding TFE and feeding SFVE (23 g) (5% TFE conversion per batch). After 230 minutes, when an amount of 340 grams of TFE and 443 g of SFVE had been fed, the feed of TFE was stopped. The autoclave was cooled to ambient temperature by maintaining constant stirring at 650 rpm, the latex was discharged after 48 hours under air bubbling to remove residual monomers from the polymerization and then stored in a plastic can. No signs of coagulation / precipitation of the latex were observed.
[0237] The latex so produced was characterized by laser light scattering to determine the average particle size, which was found to be 107 nm.The polymer so obtained had an equivalent weight (EW) of 758 g / mol and the following composition measured by FT-IR: TFE: 82.7 mol%, and SFVE: 17.3 mol%.
Claims
1. A process for producing a fluoropolymer comprising a plurality of hydrolyzable groups [polymer (P)], the process comprising emulsion polymerizing in an aqueous medium in the presence of at least one free radical initiator and at least one multifunctional dispersant [dispersant (D)]: - tetrafluoroethylene, and - at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group, The dispersant (D): - having a weight average molecular weight (M) of at least 15,000 and at most 800,000 as measured by GPC w ); - comprises a backbone comprising repeating units derived from one or more ethylenically unsaturated monomers; and -Contains multiple options from -SO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal.
2. The method of claim 1, wherein: The dispersant (D) has a molecular weight and a molecular weight distribution such that it contains substantially no fraction having a molecular weight of less than 3000 as measured by GPC.
3. The method according to claim 1 or 2, wherein: The dispersant (D) has a weight average molecular weight (M) of 150,000 to 600,000, preferably 180,000 to 500,000 as measured by GPC. w ).
4. A method as claimed in any one of the preceding claims, wherein: The amount of ionic groups in the dispersant (D) is at least 1.00 meq / g and / or at most 2.50 meq / g relative to the weight of the dispersant (D).
5. A method as claimed in any one of the preceding claims, wherein: The amount of the dispersant (D) is 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
6. A method as claimed in any one of the preceding claims, wherein: The dispersant (D) is a polymer comprising repeating units derived from at least one ethylenically unsaturated fluorinated monomer containing at least one group -SO2X, wherein X is -OX a , where X a is H, an ammonium group or a monovalent metal; and a repeating unit derived from at least one ethylenically unsaturated fluorinated monomer not containing a -SO2X group.
7. The method of claim 6, wherein: The at least one ethylenically unsaturated fluorinated monomer not containing a -SO2X group is tetrafluoroethylene.
8. A method as claimed in any one of the preceding claims, wherein The polymer (P) comprises repeating units derived from at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group selected from the group consisting of -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group.
9. A method as claimed in any one of the preceding claims, wherein: The polymer (P) comprises repeating units derived from at least one ethylenically unsaturated fluorinated monomer containing at least one -SO2X group, wherein X is a halogen.
10. A method as claimed in any one of the preceding claims, wherein: The polymer (P) and the dispersant (D) comprise repeating units derived from at least one ethylenically unsaturated fluorinated monomer containing at least one -SO2X group, the ethylenically unsaturated fluorinated monomer being selected from the group consisting of: -sulfonyl halofluoroolefin having the formula: CF2=CF(CF2) p SO2X; wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein p is an integer between 0 and 10, preferably between 1 and 6, more preferably p is equal to 1, 2 or 3; -sulfonyl halide fluorovinyl ether having the formula: CF2=CF-O-(CF2) m SO2X, wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein m is an integer between 1 and 10, preferably between 1 and 6, more preferably between 2 and 4, even more preferably m is equal to 2; -sulfonyl halofluoroalkoxy vinyl ether having the formula: CF2=CF-(OCF2CF(R F1 )) w -O-CF2(CF(R F2 )) y SO2X Wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein w is an integer between 0 and 2, R F1 and R F2 are the same as or different from each other and are independently F, Cl, or C optionally substituted with one or more ether oxygens. 1- C 10 fluoroalkyl, y is an integer between 0 and 6; preferably, w is 1, R F1 is -CF3, y is 1 and R F2 It is F; - a sulfonyl halide aromatic fluoroolefin having the formula CF2=CF-Ar-SO2X, wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein Ar is C5-C 15 Aromatic or heteroaromatic groups.
11. A method as claimed in any one of the preceding claims, wherein: The polymer (P) and the dispersant (D) comprise: - 50 to 99 mol% of repeating units derived from tetrafluoroethylene relative to the total moles of the polymer (P) or the dispersant (D); - 1 to 50 mol % of repeating units, relative to the total moles of the polymer (P) or the dispersant (D), derived from at least one monomer selected from the group consisting of: (j) Sulfonyl halide fluorovinyl ether having the formula: CF2=CF-O-(CF2) m SO2X, wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein m is an integer between 1 and 10, preferably between 1 and 6, more preferably between 2 and 4, even more preferably m is equal to 2; (jj) Sulfonyl halide fluoroalkoxy vinyl ether having the formula: CF2=CF-(OCF2CF(R F1 )) w -O-CF2(CF(R F2 )) y SO2X Where X is OX a , wherein in the dispersant (D), X is OX a , where X a is H, an ammonium group or a monovalent metal, and in polymer (P), X is a halogen, preferably F or Cl, more preferably F, wherein w is an integer between 0 and 2, R F1 and R F2 are the same as or different from each other and are independently F, Cl, or C1-C1 optionally substituted by one or more ether oxygen atoms. 10 fluoroalkyl, y is an integer between 0 and 6; preferably, w is 1, R F1 is -CF3, y is 1 and R F2 is F; and (jjj) mixtures thereof; as well as - 0 to 40 mol % of recurring units derived from at least one hydrogenated and / or fluorinated monomer, preferably a perfluorinated monomer, different from tetrafluoroethylene, with respect to the total moles of polymer (P) or dispersant (D), selected from the group consisting of: hexafluoropropylene; monomers having the formula CF2=CFOR' f1 Perfluoroalkyl vinyl ether, wherein R' f1 Is a C1-C6 perfluoroalkyl group; having the formula CF2=CFOR' O1 Perfluorooxyalkyl vinyl ether, wherein R' O1 is a C2-C 12 Perfluoroalkyl groups, including those having the formula CF2=CFOCF2OR' f2 Perfluoroalkyl-methoxy-vinyl ether, wherein R' f2 is a C1-C6 perfluoroalkyl group, or a C1-C6 perfluorooxyalkyl group having one or more ether groups; a fluorodioxole having the following formula: Where R f3 , R f4 , R f5 , R f6 Each of the same or different from each other is independently a fluorine atom, a C1-C6 fluoro(halo)fluoroalkyl group optionally containing one or more oxygen atoms.
12. A process as claimed in any one of the preceding claims, comprising the steps of preparing the dispersant (D): emulsion polymerizing tetrafluoroethylene and at least one ethylenically unsaturated fluorinated monomer comprising at least one hydrolyzable group selected from -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group, in an aqueous medium in the presence of at least one free radical initiator and a dispersant (Dx) to obtain a polymer comprising a plurality of hydrolyzable groups; and hydrolyzing these hydrolyzable groups to obtain the corresponding ionic groups -SO3X a and-COOX a , where X a is H, an ammonium group or a monovalent metal.
13. The method of claim 12, wherein: The dispersant (Dx) is present in an amount of 0.01 wt% to 5.00 wt% based on the total weight of the aqueous medium.
14. The method according to claim 11 or 12, wherein: Dispersant (Dx) is dispersant (D).
15. An aqueous dispersion of particles of a fluoropolymer comprising a plurality of hydrolyzable groups [polymer (P)], said dispersion comprising at least one dispersant (D), said dispersant (D): - comprises a main chain comprising repeating units derived from one or more ethylenically unsaturated monomers, - having a weight average molecular weight (M) of at least 15,000 and at most 800,000 w ), -Contains multiple options from -SO3X a and-COOX a The ionic groups composed of X a is H, an ammonium group or a monovalent metal.
16. A method for obtaining a polymer (P) in its ionic form as a powdery material [material (PP)], the method comprising: (1): Providing the aqueous dispersion as claimed in claim 15; as well as (2): contacting the aqueous dispersion with an alkaline hydrolyzing agent to at least partially convert the hydrolyzable groups of the polymer (P) into corresponding ionic groups without causing any significant coagulation, so as to obtain an aqueous dispersion of particles of the polymer (P) in ionic form; as well as Optionally (3): contacting the dispersion obtained at the end of step (2) with at least one ion exchange resin in order to at least partially remove the residues of the alkaline hydrolysis agent and / or other contaminants; as well as (4): Spray drying the dispersion obtained at the end of step (2) and the optional step (3) so as to obtain the material (PP).
17. The method of claim 16, wherein: These hydrolyzable groups are the groups -SO2X and -COOZ, wherein X is a halogen atom and Z is a C1-C4 alkoxy group.
18. The method according to claim 16 or 17, comprising an additional purification step between step (2) and step (4), in particular when optional step (3) is present, between step (3) and step (4).
19. The method of claim 18, wherein: The purification step is performed by one selected from dialysis, electrodialysis and ultrafiltration.