Copolymer, molded body, extrusion molded body, and transfer molded body
By adjusting the PPVE content and melt flow rate in tetrafluoroethylene and perfluoro(propyl vinyl ether) copolymer, the wear resistance and permeability of fluorothermoplastics under high temperature and high pressure are solved. A molded body with wear resistance of 135°C and tensile creep resistance of 230°C was achieved.
Patent Information
- Application Number
- CN202380028918.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing fluorothermoplastics are difficult to maintain wear resistance, low permeability and durability of the drug solution under high temperature and high pressure conditions, especially at 230°C.
Using a copolymer containing tetrafluoroethylene and perfluoro (propyl vinyl ether) units, the PPVE unit content, melt flow rate and number of functional groups in the copolymer are adjusted to form a wear resistance of 135°C and a high temperature of 85°C. A molded body with rigidity and tensile creep resistance at 230°C.
It achieves excellent performance of wear resistance of 135°C, low permeability of the drug solution, rigidity at high temperature of 85°C, tensile creep resistance characteristics of 230°C, and is suitable for molded bodies under high temperature and high pressure environments.
Smart Images

Figure BDA0005051314790000041 
Figure BDA0005051314790000151 
Figure BDA0005051314790000181
Abstract
Description
Technical Field
[0001] The present invention relates to copolymers, molded bodies, extrusion molded bodies and transfer molded bodies. Background Art
[0002] Patent Document 1 describes fluorine thermoplastics from (a) to (c).
[0003] (a) Tetrafluoroethylene
[0004] (b) a perfluorinated olefin containing at least one of hexafluoropropylene, perfluorinated vinyl ether or perfluorinated allyl ether
[0005] (c) Formula: F 2 C=CF(CF 2 ) a (O)RfH Modifier
[0006] In the formula, a is 0 or 1, and Rf is a linear or branched fluorinated alkylene group containing 1 to 5 carbon atoms, optionally containing at least one ether bond, and optionally containing 1 or 2 hydrogen atoms.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: U.S. Patent Application Publication No. 2021 / 189031 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The object of the present invention is to provide a copolymer capable of obtaining a molded product having excellent abrasion resistance at 135°C, low permeability to chemical solutions, rigidity at a high temperature of 85°C, durability against repeated loads, tensile creep resistance at 230°C, and durability against tensile forces applied at 230°C.
[0012] Means for solving problems
[0013] According to the present invention, a copolymer is provided, which contains tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of the perfluoro(propyl vinyl ether) units is 4.3 to 6.0% by mass relative to all monomer units, the melt flow rate at 372° C. is 0.7 to 1.4 g / 10 minutes, and the number of functional groups is 10 6 The number of carbon atoms in the main chain is 20 or less.
[0014] Effects of the Invention
[0015] According to the present invention, there is provided a copolymer capable of obtaining a molded product having excellent abrasion resistance at 135°C, low permeability to chemical solutions, rigidity at a high temperature of 85°C, durability against repeated loads, tensile creep resistance at 230°C, and durability against tensile forces applied at 230°C. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention are described in detail below, but the present invention is not limited to the following embodiments.
[0017] The copolymer of the present invention comprises tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.
[0018] A copolymer (PFA) containing TFE units and PPVE units is used as a material for forming a delivery tube for delivering a drug solution. In particular, in a large-diameter tube, since a large amount of fluid flows, there is a problem that the inner surface of the tube is easily worn by the fluid. In addition, there is a problem that it is easy to deform due to the pressure caused by a large amount of fluid. Therefore, in order to suppress the wear and deformation of the tube when a large amount of fluid flows, a fluorine-containing copolymer is needed that can obtain a molded body with excellent wear resistance, low permeability to the drug solution, rigidity at high temperature, durability to repeated loads, tensile creep resistance, and durability to tensile forces applied at 230°C.
[0019] It was found that by appropriately adjusting the PPVE unit content, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units, a copolymer can be obtained that can obtain a molded body that has excellent abrasion resistance at 135°C, low permeability to drug liquids, rigidity at a high temperature of 85°C, durability to repeated loads, tensile creep resistance at 230°C, and durability to tensile forces applied at 230°C.
[0020] The copolymer of the present invention is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using existing processing equipment such as an extruder and an injection molding machine.
[0021] The content of the PPVE unit in the copolymer is 4.3 to 6.0% by mass relative to the total monomer units. The content of the PPVE unit in the copolymer is preferably 4.4% by mass or more, more preferably 4.5% by mass or more, further preferably 4.6% by mass or more, preferably 5.9% by mass or less, more preferably 5.8% by mass or less, further preferably 5.7% by mass or less, and particularly preferably 5.6% by mass or less. If the content of the PPVE unit in the copolymer is too much, the rigidity at a high temperature of 85°C, the durability to repeated loads, and the tensile creep resistance at 230°C will be poor. If the content of the PPVE unit in the copolymer is too little, the wear resistance at 135°C and the durability to the tensile force applied at 230°C will be poor.
[0022] The content of the TFE unit of the copolymer is preferably 94.0% by mass or more, more preferably 94.1% by mass or more, further preferably 94.2% by mass or more, further preferably 94.3% by mass or more, particularly preferably 94.4% by mass or more, preferably 95.7% by mass or less, more preferably 95.6% by mass or less, further preferably 95.5% by mass or less, further preferably 95.4% by mass or less. If the content of the TFE unit of the copolymer is too small, the rigidity at a high temperature of 85°C, the durability to repeated loads, and the tensile creep resistance at 230°C will be poor. If the content of the TFE unit of the copolymer is too large, the wear resistance at 135°C and the durability to the tensile force applied at 230°C may be poor.
[0023] In the present invention, the content of each monomer unit in the copolymer is determined by 19 Determined by F-NMR method.
[0024] The copolymer may also contain monomer units derived from monomers copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 1.7% by mass, more preferably 0.05 to 1.4% by mass, further preferably 0.1 to 0.5% by mass, and particularly preferably 0.1 to 0.3% by mass relative to all monomer units of the copolymer. The content of the monomer units copolymerizable with TFE and PPVE may be 0.1% by mass or less relative to all monomer units of the copolymer.
[0025] Examples of monomers copolymerizable with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF 2 ) n Z 4 (Where Z 1 , Z 2 and Z 3 Same or different, means H or F, Z 4 represents H, F or Cl, and n represents an integer of 2 to 10. ) represents a vinyl monomer, CF 2 =CF-ORf 1 (Where Rf 1 Perfluoro(alkyl vinyl ether) [PAVE] (excluding PPVE) represented by a perfluoroalkyl group having 1 to 8 carbon atoms, and CF 2 =CF-OCH 2 -Rf 1 (Where Rf 1 represents a perfluoroalkyl group having 1 to 5 carbon atoms. ) and the like. Among them, HFP is preferred.
[0026] The copolymer is preferably at least one selected from the group consisting of a copolymer consisting only of a TFE unit and a PPVE unit and a TFE / HFP / PPVE copolymer, and more preferably a copolymer consisting only of a TFE unit and a PPVE unit.
[0027] The melt flow rate (MFR) of the copolymer is 0.7 to 1.4 g / 10 minutes. The MFR of the copolymer is preferably 0.9 g / 10 minutes or more, more preferably 1.0 g / 10 minutes or more, preferably 1.3 g / 10 minutes or less, more preferably 1.1 g / 10 minutes or less, and further preferably 1.0 g / 10 minutes or less. If the MFR of the copolymer is too high, the wear resistance at 135°C, the tensile creep resistance at 230°C, and the durability to the tensile force applied at 230°C will be poor. If the MFR of the copolymer is too low, the low permeability of the drug solution, the rigidity at a high temperature of 85°C, and the durability to repeated loads will be poor.
[0028] In the present invention, MFR is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer in accordance with ASTM D1238.
[0029] The MFR can be adjusted by adjusting the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, etc., used when polymerizing the monomers.
[0030] Each 10 6 The number of functional groups per main chain carbon atom is 20 or less. 6 The number of functional groups per main chain carbon atom is preferably 15 or less, more preferably 10 or less, and further preferably less than 6. If the number of functional groups is too large, a molded article having low chemical liquid permeability and excellent 230° C. tensile creep resistance cannot be obtained.
[0031] The identification of the types of the functional groups and the measurement of the number of the functional groups can be performed using infrared spectroscopy.
[0032] The number of functional groups is specifically determined by the following method. First, the copolymer is formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer and a differential spectrum from a background spectrum of complete fluorination without the presence of functional groups. The number of functional groups per 1×10 6 The number of functional groups N per carbon atom.
[0033] N=I×K / t(A)
[0034] I: Absorbance
[0035] K: Correction coefficient
[0036] t: film thickness (mm)
[0037] For reference, absorption frequencies, molar absorption coefficients, and correction coefficients for some functional groups are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low-molecular model compounds.
[0038] [Table 1]
[0039] Table 1
[0040]
[0041] -CH 2 CF 2 H, -CH 2 COF, -CH 2 COOH, -CH 2 COOCH 3 、-CH 2 CONH 2 The absorption frequency ratios are shown in Table -CF 2 H, -COF, free -COOH and bonded -COOH, -COOCH 3 、-CONH 2 The absorption frequency is several tens of cm lower. -1 ).
[0042] For example, the functional group number of -COF refers to the number of functional groups derived from -CF 2 The absorption frequency of COF is 1883 cm -1 The number of functional groups obtained from the absorption peak at -CH 2 The absorption frequency of COF is 1840 cm -1 The total number of functional groups found from the absorption peak at .
[0043] The functional groups are the functional groups present at the ends of the main chain or the side chains of the copolymer and the functional groups present in the main chain or the side chains. The number of functional groups can be -CF=CF 2 , -CF 2 H, -COF, -COOH, -COOCH 3 、-CONH 2 and -CH 2 The total number of OH.
[0044] The functional groups are introduced into the copolymer by, for example, a chain transfer agent or a polymerization initiator used when producing the copolymer. For example, alcohol is used as a chain transfer agent, or a -CH 2 When the peroxide with OH structure is used as the polymerization initiator, -CH 2 OH is introduced into the main chain terminal of the copolymer. In addition, by polymerizing a monomer having a functional group, the above functional group is introduced into the side chain terminal of the copolymer.
[0045] By fluorinating the copolymer having such a functional group, a copolymer having the number of functional groups within the above range can be obtained. That is, the copolymer of the present invention is preferably fluorinated. The copolymer of the present invention also preferably has -CF 3 Terminal group.
[0046] The melting point of the copolymer is preferably 295 to 315° C., more preferably 298° C. or higher, further preferably 300° C. or higher, particularly preferably 301° C. or higher, and more preferably 308° C. or lower. When the melting point is within the above range, a copolymer can be obtained that can provide a molded body that is more excellent in abrasion resistance at 135° C., low permeability to chemical liquids, rigidity at a high temperature of 85° C., durability against repeated loads, tensile creep resistance at 230° C., and durability against tensile forces applied at 230° C.
[0047] In the present invention, the melting point can be measured using a differential scanning calorimeter [DSC].
[0048] The methyl ethyl ketone (MEK) permeability of the copolymer is preferably 89.0 mg·cm / m 2 ·day or less, more preferably 85.0 mg·cm / m 2 · days or less. The copolymer of the present invention has excellent low permeability to chemical liquids because the content of PPVE units, melt flow rate (MFR) and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. That is, by using the copolymer of the present invention, a molded body that is not easily permeable to chemical liquids such as MEK can be obtained.
[0049] In the present invention, the MEK permeability can be measured under the conditions of a temperature of 60° C. and a period of 70 days. The MEK permeability can be specifically measured by the method described in the Examples.
[0050] The copolymer of the present invention can be produced by polymerization methods such as suspension polymerization, solution polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization method, emulsion polymerization or suspension polymerization is preferred. In these polymerizations, various conditions such as temperature and pressure, polymerization initiator, and other additives can be appropriately set according to the composition and amount of the copolymer.
[0051] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.
[0052] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:
[0053] Dialkyl peroxydicarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate and di-2-ethoxyethyl peroxydicarbonate;
[0054] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;
[0055] Dialkyl peroxides such as di-tert-butyl peroxide;
[0056] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.
[0057] Examples of di[fluoro(or chlorofluoro)acyl]peroxides include [(RfCOO)-] 2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).
[0058] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetrafluorooctanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoropentanoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, di(perfluorohexanoyl ... (ω-chloro-decafluorohexanoyl) peroxide, bis(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, bis(dichloropentafluorobutyryl) peroxide, bis(trichlorooctafluorohexanoyl) peroxide, bis(tetrachloroundecanoyl) peroxide, bis(pentachlorotetrafluorodecanoyl) peroxide, bis(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.
[0059] The water-soluble free radical polymerization initiator may be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide and diglutaric acid peroxide, tert-butyl permaleate, tert-butyl hydroperoxide, etc. A reducing agent such as sulfite may be used in combination with the peroxide, and the amount used may be 0.1 to 20 times that of the peroxide.
[0060] A surfactant, a chain transfer agent, and a solvent may be used in the polymerization, and conventionally known surfactants may be used.
[0061] As the surfactant, known surfactants can be used, such as nonionic surfactants, anionic surfactants, cationic surfactants, etc. Among them, fluorinated anionic surfactants are preferred, and more preferred are fluorinated anionic surfactants that may contain ether-bonded oxygen (i.e., oxygen atoms may be inserted between carbon atoms) and have a linear or branched carbon number of 4 to 20. The amount of surfactant added (relative to polymerization water) is preferably 50 to 5000 ppm.
[0062] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane, etc. The amount of chain transfer agent added can vary depending on the chain transfer constant of the compound used, and is usually used in the range of 0.01 to 20% by mass relative to the polymerization solvent.
[0063] Examples of the solvent include water and a mixed solvent of water and alcohol.
[0064] In suspension polymerization, a fluorinated solvent may be used in addition to water. Examples of the fluorinated solvent include CH 3 CClF 2 , CH 3 CCl 2 F. CF 3 CF 2 CCl 2 H.CF 2 CCF 2 CFHCl and other hydrochlorofluoroalkanes; CF 2 ClCFClCF 2 CF 3 CF 3 CFClCFClCF 3 Chlorofluoroalkanes; CF 3 CFHCFHCF 2 CF 2 CF3 CF 2 HCF 2 CF 2 CF 2 CF 2 H.CF 3 CF 2 CF 2 CF 2 CF 2 CF 2 CF 2 H and other hydrofluoroalkanes; CH 3 OC 2 F 5 , CH 3 OC 3 F 5 CF 3 CF 2 CH 2 OCHF 2 CF 3 CHF 2 OCH 3 , CHF 2 CF 2 OCH 2 F, (CF 3 ) 2 CHCF 2 OCH 3 CF 3 CF 2 CH 2 OCH 2 CHF 2 CF 3 CHF 2 OCH 2 CF 3 Hydrofluoroethers, such as perfluorocyclobutane, CF 3 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 2 CF 3 The amount of the fluorinated solvent used is preferably 10 to 100% by mass relative to the aqueous medium from the viewpoint of suspending properties and economic efficiency.
[0065] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure is appropriately determined depending on the type and amount of the solvent used and other polymerization conditions such as vapor pressure and polymerization temperature, and may generally be 0 to 9.8 MPaG.
[0066] In the case of obtaining an aqueous dispersion comprising a copolymer by polyreaction, the copolymer can be recovered by precipitating, cleaning, and drying the copolymer contained in the aqueous dispersion. In addition, in the case of obtaining a copolymer in the form of a slurry by polyreaction, the copolymer can be recovered by taking out the slurry from a reaction vessel and cleaning and drying. By drying, the copolymer can be recovered in the form of a powder.
[0067] The copolymer obtained by polymerization can be formed into pellets. There is no particular limitation on the molding method for forming the pellets, and a conventionally known method can be used. For example, there can be cited a method in which the copolymer is melt-extruded using a single-screw extruder, a twin-screw extruder, or a tandem extruder, and the copolymer is cut into a predetermined length to form pellets. The extrusion temperature during melt extrusion needs to be changed according to the melt viscosity and the manufacturing method of the copolymer, and is preferably the melting point of the copolymer + 20°C to the melting point of the copolymer + 140°C. There is no particular limitation on the method for cutting the copolymer, and conventionally known methods such as a wire cutting method, a heat cutting method, an underwater cutting method, and a sheet cutting method can be used. The volatile components in the pellets can also be removed by heating the obtained pellets (degassing treatment). The obtained pellets can also be treated by contacting with warm water at 30°C to 200°C, steam at 100°C to 200°C, or hot air at 40°C to 200°C.
[0068] The copolymer obtained by polymerization may also be subjected to fluorination treatment. Fluorination treatment may be carried out by contacting the copolymer that has not been subjected to fluorination treatment with a fluorine-containing compound. Fluorination treatment can reduce the -COOH and -COOCH 3 、-CH 2 OH, -COF, -CF=CF 2 、-CONH 2 Thermally unstable functional groups and thermally stable -CF 2 H and other functional groups are converted into extremely thermally stable -CF 3 As a result, the COOH and -COOCH 3 、-CH 2 OH, -COF, -CF=CF 2 、-CONH 2 and -CF 2 The total number of H (the number of functional groups) is adjusted to fall within the above range.
[0069] The fluorine-containing compound is not particularly limited, and examples thereof include a fluorine radical source that generates fluorine radicals under fluorination treatment conditions. Examples of the fluorine radical source include F 2 Gas, CoF 3 , AgF 2 、UF 6 、OF 2 、N 2 F 2 CF 3 OF, fluorinated halogens (such as IF 5 , ClF 3 )wait.
[0070] F 2 The fluorine radical source such as gas can be 100% concentration, but from the aspect of safety, it is preferably mixed with an inert gas and diluted to 5% to 50% by mass for use, and more preferably diluted to 15% to 30% by mass for use. As the above-mentioned inert gas, nitrogen, helium, argon, etc. can be cited, and nitrogen is preferred from the aspect of economy.
[0071] The conditions for the fluorination treatment are not particularly limited, and the molten copolymer may be brought into contact with the fluorine-containing compound. However, the fluorination treatment may be carried out at a temperature below the melting point of the copolymer, preferably at 20°C to 240°C, and more preferably at 100°C to 220°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably for 5 to 25 hours. The fluorination treatment is preferably carried out by bringing the unfluorinated copolymer into contact with fluorine gas (F 2 Gas) contact treatment.
[0072] The copolymer of the present invention may also be mixed with other components as required to obtain a composition. Other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, dehydrofluorination agents, etc.
[0073] As fillers, for example, silicon dioxide, kaolin, clay, organic clay, talc, mica, aluminum oxide, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, glass fibers, etc. can be cited. As conductive agents, carbon black, etc. can be cited. As plasticizers, dioctyl phthalate, pentaerythritol, etc. can be cited. As processing aids, carnauba wax, sulfone compounds, low molecular weight polyethylene, fluorine-based additives, etc. can be cited. As dehydrofluorination agents, organic onium, amidines, etc. can be cited.
[0074] As the other components, other polymers other than the above copolymers may be used. Examples of the other polymers include fluororesins, fluororubbers, and non-fluorinated polymers other than the above copolymers.
[0075] Examples of the method for producing the composition include a method of dry-mixing the copolymer and other components; a method of preliminarily mixing the copolymer and other components with a mixer and then melt-kneading them with a kneader, melt extruder or the like; and the like.
[0076] The copolymer of the present invention or the above-mentioned composition can be used as a processing aid, a molding material, etc., and is preferably used as a molding material. The aqueous dispersion, solution, suspension, and copolymer / solvent system of the copolymer of the present invention can also be utilized, and they can be applied as a coating, or used for encapsulation, impregnation, or film casting. However, the copolymer of the present invention is preferably used as the above-mentioned molding material because it has the above-mentioned characteristics.
[0077] The copolymer of the present invention or the above-mentioned composition may be molded to obtain a molded product.
[0078] The method for molding the above-mentioned copolymer or the above-mentioned composition is not particularly limited, and injection molding, extrusion molding, compression molding, blow molding, transfer molding, rotational molding, roto-lining molding, etc. can be cited. As a molding method, among them, extrusion molding, compression molding or transfer molding are preferred, and extrusion molding or transfer molding are more preferred because molded bodies can be produced with high productivity, and extrusion molding is further preferred. That is, as a molded body, extrusion molded body, compression molded body, injection molded body or transfer molded body are preferably used, and extrusion molded body or transfer molded body are more preferred because they can be produced with high productivity, and extrusion molded body is further preferred. The copolymer of the present invention is molded by extrusion molding or transfer molding, so that a beautiful molded body can be obtained.
[0079] Examples of the molded article containing the copolymer of the present invention include nuts, bolts, joints, films, bottles, washers, wire coatings, tubes, hoses, pipes, valves, sheets, seals, gaskets, tanks, rollers, containers, cocks, connectors, filter housings, filter covers, flow meters, pumps, wafer carriers, wafer boxes, and the like.
[0080] The copolymer of the present invention, the composition or the molded article can be used, for example, in the following applications.
[0081] Films for food packaging, lining materials for fluid delivery pipelines used in food manufacturing processes, gaskets, sealing materials, sheets and other fluid delivery components for food manufacturing equipment;
[0082] Chemical plugs, packaging films, lining materials, gaskets, sealing materials, sheets and other liquid delivery components for fluid delivery pipelines used in chemical manufacturing processes;
[0083] Lining components for the inner surface of liquid tanks and piping in chemical equipment and semiconductor factories;
[0084] O (square) rings / tubes / gaskets, valve core materials, hoses, sealing materials, etc. used in automobile fuel systems and peripheral devices; fuel delivery components such as hoses and sealing materials used in automobile AT devices;
[0085] Flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in car engines and peripheral devices of automobiles; other automobile components such as automobile brake hoses, air conditioning hoses, radiator hoses, wire covering materials, etc.;
[0086] Semiconductor manufacturing equipment O (square) rings, tubes, gaskets, valve core materials, hoses, sealing materials, rollers, gaskets, diaphragms, joints and other semiconductor device liquid delivery components;
[0087] Coating rollers, hoses, tubes, ink containers and other coating and ink components for coating equipment;
[0088] Food and beverage conveying components such as tubes or hoses for food and beverages, tubes, hoses, belts, gaskets, joints, etc., food packaging materials, and glass cooking equipment;
[0089] Waste liquid transmission components such as pipes and hoses used for waste liquid transmission;
[0090] Components for high-temperature liquid transmission such as pipes and hoses used for high-temperature liquid transmission;
[0091] Steam piping components such as pipes and hoses used for steam piping;
[0092] Pipe corrosion protection tapes such as tapes wrapped around pipes on ship decks, etc.
[0093] Various covering materials such as wire covering materials, optical fiber covering materials, transparent surface covering materials and back-side agents provided on the light incident side surface of photovoltaic elements of solar cells;
[0094] Diaphragms of diaphragm pumps and sliding components such as various sealing gaskets;
[0095] Weather-resistant covers for agricultural films, various roofing materials, sidewalls, etc.;
[0096] Interior materials used in the construction field, non-combustible fireproof safety glass and other glass covering materials;
[0097] Lining materials for laminated steel sheets used in the home appliance field, etc.
[0098] Further examples of the fuel delivery member used in the fuel system of the above-mentioned automobile include fuel hoses, filler hoses, evaporator hoses, etc. The above-mentioned fuel delivery member can also be used as a fuel delivery member for sour gasoline, alcohol fuel, and fuel added with gasoline additives such as methyl tert-butyl ether resistance and amine resistance.
[0099] The chemical plug and packaging film have excellent chemical resistance to acids, etc. In addition, as the chemical liquid conveying member, there can also be mentioned a corrosion-resistant tape wound around the piping of chemical equipment.
[0100] The molded product containing the copolymer of the present invention has excellent 135°C abrasion resistance, low drug liquid permeability, 85°C high temperature rigidity, durability against repeated loads, 230°C tensile creep resistance, and durability against tensile force applied at 230°C, and is therefore particularly suitable for use in sheets, tubes, etc.
[0101] Examples of the molded article include automobile radiator water chambers, chemical tanks, bellows, partitions, rollers, gasoline tanks, waste liquid transport containers, high temperature liquid transport containers, fisheries and fish farming tanks, and the like.
[0102] Examples of the molded bodies include automobile bumpers, door trims, instrument panels, food processing equipment, cooking machines, waterproof and oil-proof glass, lighting-related instruments, indicator panels and housings of OA instruments, electrically illuminated signboards, display screens, liquid crystal display screens, mobile phones, printer chassis, electrical and electronic components, groceries, trash cans, bathtubs, integrated bathrooms, ventilation fans, lighting frames, and the like.
[0103] The molded article containing the copolymer of the present invention can be suitably used as a compressed member such as a gasket or a seal. The compressed member of the present invention may be a gasket or a seal.
[0104] The size and shape of the compressed member of the present invention can be appropriately set according to the purpose, and there is no particular limitation. The shape of the compressed member of the present invention can be, for example, annular. In addition, the compressed member of the present invention can have a circular, elliptical, quadrilateral with rounded corners, etc. shape when viewed from above, and has a through hole in its central portion.
[0105] The compressed member of the present invention is preferably used as a member for constituting a non-aqueous electrolyte battery. The compressed member of the present invention is particularly suitable as a member used in a state of contact with a non-aqueous electrolyte in a non-aqueous electrolyte battery. That is, the compressed member of the present invention may have a liquid contact surface with the non-aqueous electrolyte in the non-aqueous electrolyte battery.
[0106] The nonaqueous electrolyte battery is not particularly limited as long as it is a battery having a nonaqueous electrolyte, and examples thereof include lithium ion secondary batteries, lithium ion capacitors, etc. In addition, members constituting the nonaqueous electrolyte battery include sealing members, insulating members, and the like.
[0107] The non-aqueous electrolyte is not particularly limited, and one or more of known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate can be used. The non-aqueous electrolyte battery can further include an electrolyte. The electrolyte is not particularly limited, and LiClO 4 、LiAsF 6 、LiPF 6 , LiBF 4 、LiCl、LiBr、CH 3 SO 3 Li, CF 3 SO 3 Li, cesium carbonate, etc.
[0108] The compressed member of the present invention can be preferably used as a sealing member such as a sealing gasket or a sealing pad, or an insulating member such as an insulating gasket or an insulating pad. A sealing member is a member used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating member is a member used for electrical insulation. The compressed member of the present invention can also be a member used for both sealing and insulation purposes.
[0109] The copolymer of the present invention can be suitably used as a material for forming an electric wire coating.
[0110] The covered electric wire comprises a core wire and a covering layer disposed around the core wire and containing the copolymer of the present invention. For example, an extrusion molded body formed by melt extrusion molding the copolymer of the present invention on the core wire can be used as the covering layer. The covered electric wire is suitable for high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is suitable for high-frequency transmission cables.
[0111] As the material of the core wire, a metal conductor material such as copper or aluminum can be used. The core wire preferably has a diameter of 0.02 mm to 3 mm. The core wire diameter is more preferably 0.04 mm or more, further preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire diameter is more preferably 2 mm or less.
[0112] As specific examples of the core wire, AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 μm), AWG-26 (solid copper wire with a diameter of 404 μm), AWG-24 (solid copper wire with a diameter of 510 μm), AWG-22 (solid copper wire with a diameter of 635 μm), etc. can be used.
[0113] The thickness of the coating layer is preferably 0.1 mm to 3.0 mm, and the thickness of the coating layer is also preferably 2.0 mm or less.
[0114] As a high-frequency transmission cable, a coaxial cable can be cited. A coaxial cable generally has a structure in which an inner conductor, an insulating coating, an outer conductor layer and a protective coating are sequentially stacked from the core to the periphery. A molded body containing the copolymer of the present invention can be suitably used as an insulating coating containing a copolymer. The thickness of each layer in the above structure is not particularly limited. Generally, the diameter of the inner conductor is about 0.1 mm to 3 mm, the thickness of the insulating coating is about 0.3 mm to 3 mm, the thickness of the outer conductor layer is about 0.5 mm to 10 mm, and the thickness of the protective coating is about 0.5 mm to 2 mm.
[0115] The coating layer may contain air bubbles, and the air bubbles are preferably uniformly distributed in the coating layer.
[0116] The average bubble diameter of the bubbles is not limited, and is, for example, preferably 60 μm or less, more preferably 45 μm or less, further preferably 35 μm or less, further preferably 30 μm or less, particularly preferably 25 μm or less, and particularly preferably 23 μm or less. In addition, the average bubble diameter is preferably 0.1 μm or more, more preferably 1 μm or more. The average bubble diameter can be obtained by obtaining an electron microscope image of a cross section of the wire, calculating the diameter of each bubble by image processing, and averaging them.
[0117] The foaming rate of the coating layer may be 20% or more. More preferably, it is 30% or more, further preferably, it is 33% or more, and further preferably, it is 35% or more. The upper limit is not particularly limited, for example, it is 80%. The upper limit of the foaming rate may be 60%. The foaming rate is a value calculated as ((specific gravity of the wire coating material - specific gravity of the coating layer) / specific gravity of the wire coating material) × 100. The foaming rate can be appropriately adjusted according to the application by, for example, adjusting the amount of gas inserted in the extruder described later, or by selecting the type of dissolved gas.
[0118] The covered electric wire may also have other layers between the core wire and the covering layer, and may further have other layers (outer layers) around the covering layer. When the covering layer contains bubbles, the electric wire of the present invention may also be a two-layer structure (skin-foam) in which a non-foam layer is inserted between the core wire and the covering layer; a two-layer structure (foam-skin) in which a non-foam layer is covered on the outer layer; and a three-layer structure (skin-foam-skin) in which a non-foam layer is covered on the outer layer of the skin-foam. The non-foam layer is not particularly limited, and may be a resin layer composed of TFE / HFP copolymers, TFE / PAVE copolymers, TFE / ethylene copolymers, vinylidene fluoride polymers, polyolefin resins such as polyethylene [PE], and polyvinyl chloride [PVC].
[0119] The covered electric wire can be produced, for example, by heating a copolymer using an extruder and extruding the copolymer onto a core wire in a molten state to form a covering layer.
[0120] When forming the coating, it is also possible to heat the copolymer and, under the state where the copolymer is molten, introduce gas into the copolymer to form the above-mentioned coating containing bubbles. As the gas, for example, a mixture of gases such as chlorodifluoromethane, nitrogen, carbon dioxide or the like or the above-mentioned gases can be used. The gas can be introduced into the heated copolymer in the form of pressurized gas, or it can be produced by mixing a chemical foaming agent in the copolymer. The gas dissolves in the copolymer in a molten state.
[0121] Furthermore, the copolymer of the present invention can be suitably used as a material for products for high-frequency signal transmission.
[0122] The high-frequency signal transmission product is not particularly limited as long as it is a product used for the transmission of high-frequency signals, and examples thereof include (1) insulating plates of high-frequency circuits, insulating materials of connecting components, molded plates such as printed wiring boards, (2) molded bodies such as bases and antenna covers of high-frequency vacuum tubes, and (3) coated wires such as coaxial cables and LAN cables. The high-frequency signal transmission product can be suitably used in equipment that utilizes microwaves, particularly 3 GHz to 30 GHz microwaves, such as satellite communication equipment and mobile phone base stations.
[0123] In the above-mentioned products for high-frequency signal transmission, the copolymer of the present invention can be suitably used as an insulator because of its low dielectric loss tangent.
[0124] As the above-mentioned (1) molded plate, a printed wiring board is preferred from the aspect of obtaining good electrical characteristics. The above-mentioned printed wiring board is not particularly limited, and examples thereof include printed wiring boards of electronic circuits such as mobile phones, various computers, and communication equipment. As the above-mentioned (2) molded body, a radome is preferred from the aspect of low dielectric loss.
[0125] The molded product containing the copolymer of the present invention can be suitably used as a film or a sheet.
[0126] The film of the present invention is useful as a release film. The release film can be produced by molding the copolymer of the present invention by melt extrusion molding, calendaring molding, press molding, cast molding, etc. From the perspective of obtaining a uniform film, the release film can be produced by melt extrusion molding.
[0127] The film of the present invention can be applied to the surface of a roller used in OA equipment. In addition, the copolymer of the present invention can be formed into a necessary shape by extrusion molding, compression molding, press molding, etc., and formed into a sheet, film, or tube, and used as a surface material for OA equipment rollers or OA equipment belts, etc. In particular, thin-walled tubes and films can be produced by melt extrusion molding.
[0128] The molded article containing the copolymer of the present invention can be suitably used as bottles, tubes, joints, valves, piping members, etc. These can be used for storage and distribution of chemical solutions.
[0129] Although the embodiments have been described above, it should be understood that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0130] <1> According to a first aspect of the present invention, there is provided a polymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units,
[0131] The content of the perfluoro(propyl vinyl ether) unit is 4.3% to 6.0% by mass relative to the total monomer units, and the melt flow rate at 372° C. is 0.7 g / 10 min to 1.4 g / 10 min.
[0132] The number of functional groups per 10 6 The number of carbon atoms in the main chain is 20 or less.
[0133] <2> According to a second aspect of the present invention, there is provided the copolymer according to the first aspect, wherein the content of the perfluoro(propyl vinyl ether) unit is 4.6% by mass to 5.6% by mass based on all monomer units.
[0134] <3> According to a third aspect of the present invention, there is provided the copolymer according to the first or second aspect, wherein the melt flow rate at 372° C. is 0.7 g / 10 min to 1.3 g / 10 min.
[0135] <4> According to a fourth aspect of the present invention, there is provided an extrusion-molded product comprising the copolymer according to any one of the first to third aspects.
[0136] <5> According to a fifth aspect of the present invention, there is provided a transfer molded article comprising the copolymer according to any one of the first to third aspects.
[0137] <6> According to a sixth aspect of the present invention, there is provided a molded article comprising the copolymer according to any one of the first to third aspects, wherein the molded article is a sheet or a tube.
[0138] Example
[0139] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.
[0140] Each numerical value in the examples was measured by the following method.
[0141] (Content of monomer units)
[0142] The content of each monomer unit is measured using an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker BioSpin).
[0143] (Melt Flow Rate (MFR))
[0144] The mass (g / 10 min) of the polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes was determined using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D1238.
[0145] (Number of functional groups)
[0146] The pellets of the copolymer were formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film was scanned 40 times by a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] and analyzed to obtain an infrared absorption spectrum, which was a difference spectrum from the background spectrum of complete fluorination without the presence of functional groups. From the absorption peak of the specific functional group appearing in the differential spectrum, the following formula (A) was used to calculate the absorption peak of each 1×10 6 The number of functional groups N per carbon atom.
[0147] N=I×K / t(A)
[0148] I: Absorbance
[0149] K: Correction coefficient
[0150] t: film thickness (mm)
[0151] For reference, regarding the functional groups in the present invention, the absorption frequency, molar absorption coefficient and correction coefficient are shown in Table 2. The molar absorption coefficient is determined from the FT-IR measurement data of a low molecular weight model compound.
[0152] [Table 2]
[0153] Table 2
[0154]
[0155] (Melting Point)
[0156] Using a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd.), the temperature was increased from 200°C to 350°C for the first time at a heating rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and the temperature was increased from 200°C to 350°C for the second time at a heating rate of 10°C / min. The melting point was determined from the peak of the melting curve generated in the second heating process.
[0157] Comparative Example 1
[0158] 1.752L of pure water was put into a 5.88L autoclave with a stirrer. After fully replacing with nitrogen, 1.383kg of perfluorocyclobutane, 60g of perfluoro(propyl vinyl ether) (PPVE) and 137g of methanol were added, and the temperature in the system was maintained at 35°C. Next, tetrafluoroethylene (TFE) was pressed into 0.64MPa, and 0.5g of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to initiate polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously supplied to keep the pressure constant. For every 15g of TFE supplied, 0.6g of PPVE was added. The polymerization was terminated when the additional amount of TFE reached 484g. The unreacted TFE was released, and after returning the autoclave to atmospheric pressure, the obtained reaction product was washed with water and dried to obtain 504g of powder.
[0159] The obtained powder was melt-extruded at 360°C using a 14φ screw extruder (manufactured by Imoto Seisakusho) to obtain pellets of the copolymer. The PPVE content of the obtained pellets was measured by the above-mentioned method.
[0160] The obtained pellets were placed in a portable reactor (TVS1 model, manufactured by Taiping Glass Industry Co., Ltd.), and the temperature was raised to 210°C. After evacuation, N 2 The gas was diluted to 20% by volume of F 2 Gas to atmospheric pressure. From F 2 0.5 hours after the gas was introduced, temporarily evacuate the air and introduce F again. 2 After 0.5 hours, the vacuum was evacuated again and F 2 Gas. Then, the above F 2The gas introduction and vacuuming were continued once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the reactor was fully replaced with N 2 The fluorinated pellets were used to measure various physical properties by the above methods.
[0161] Comparative Example 2
[0162] 51.8L of pure water was put into a 174L autoclave with a stirrer. After fully replacing with nitrogen, 40.9kg of perfluorocyclobutane, 2.75kg of perfluoro(propyl vinyl ether) (PPVE) and 3.73kg of methanol were added, and the temperature in the system was maintained at 35°C. Next, tetrafluoroethylene (TFE) was pressed into 0.64MPa, and 0.013kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to initiate polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously supplied to keep the pressure constant. For every 1kg of TFE supplied, 0.058kg of PPVE was added. The polymerization was terminated when the additional amount of TFE reached 40.9kg. The unreacted TFE was released, and after returning the pressure in the autoclave to atmospheric pressure, the obtained reaction product was washed with water and dried to obtain 43.3kg of powder.
[0163] The obtained powder was melt-extruded at 360° C. using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The PPVE content was measured using the obtained pellets by the above-mentioned method.
[0164] The obtained pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 210°C. After evacuation, N 2 The gas was diluted to 20% by volume of F 2 Gas to atmospheric pressure. From F 2 0.5 hours after the gas was introduced, temporarily evacuate the air and introduce F again. 2 After 0.5 hours, the vacuum was evacuated again and F 2 Gas. Then, the above F 2 The gas introduction and vacuuming were continued once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the reactor was fully replaced with N 2 The fluorinated pellets were used to measure various physical properties by the above methods.
[0165] Comparative Example 3
[0166] A dry powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 86 g, methanol was not added, and 0.8 g of PPVE was added per 15 g of TFE to obtain 510 g of dry powder. The obtained powder was used to measure the PPVE content by the above method.
[0167] The obtained powder was placed in a portable reactor (TVS1 model, manufactured by Taiping Glass Industry Co., Ltd.), and the temperature was raised to 210°C. After evacuation, N 2 The gas was diluted to 20% by volume of F 2 Gas to atmospheric pressure. From F 2 0.5 hours after the gas was introduced, temporarily evacuate the air and introduce F again. 2 After 0.5 hours, the vacuum was evacuated again and F 2 Gas. Then, the above F 2 The gas introduction and vacuuming were continued once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the reactor was fully replaced with N 2 gas, ending the fluorination reaction and obtaining powder.
[0168] Comparative Example 4
[0169] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 113 g, methanol was changed to 20 g, and 1.0 g of PPVE was additionally added per 15 g of TFE supplied to obtain 517 g of dry powder.
[0170] Comparative Example 5
[0171] Unfluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 95 g, methanol to 70 g, and 0.9 g of PPVE was additionally added per 15 g of TFE supplied to obtain 512 g of dry powder.
[0172] Example 1
[0173] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 73 g, methanol was changed to 50 g, and 0.7 g of PPVE was additionally added per 15 g of TFE supplied to obtain 507 g of dry powder.
[0174] Example 2
[0175] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 84 g, methanol to 65 g, and 0.8 g of PPVE was additionally added per 15 g of TFE supplied to obtain 510 g of dry powder.
[0176] Example 3
[0177] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 95 g, methanol to 70 g, and 0.9 g of PPVE was additionally added per 15 g of TFE supplied to obtain 512 g of dry powder.
[0178] The various physical properties of the pellets or powders obtained in Examples and Comparative Examples were measured by the above-mentioned methods.
[0179] [Table 3]
[0180] Table 3
[0181]
[0182] The expression “<6” in Table 3 means that the number of functional groups is less than 6.
[0183] Next, the following properties were evaluated using the obtained pellets or powders. The results are shown in Table 4.
[0184] (Abrasion test)
[0185] Use pellets or powder and a hot press molding machine to make a sheet test piece with a thickness of about 0.2mm, and cut out a 10cm×10cm test piece from it. Fix the produced test piece on the test bench of a Taber wear tester (No.101 special Taber wear tester, manufactured by Yasuda Seiki Manufacturing Co., Ltd.), and use the Taber wear tester to perform a wear test under the conditions of a test piece surface temperature of 135°C, a load of 500g, a wear wheel CS-10 (grinded with abrasive paper #240 for 20 turns), and a rotation speed of 60rpm. Measure the weight of the test piece after 1000 turns, and use the same test piece to further measure the weight of the test piece after 4500 turns. The amount of wear is calculated by the following formula.
[0186] Wear amount (mg) = M1 - M2
[0187] M1: Weight of test piece after 1000 revolutions (mg)
[0188] M2: Test piece weight after 4500 revolutions (mg)
[0189] (Methyl ethyl ketone (MEK) permeability)
[0190] Use pellets or powder and a hot press molding machine to make a sheet test piece with a thickness of about 0.1 mm. 2 ) was placed in a container, covered with a sheet test piece, and sealed with a PTFE gasket. The sheet test piece was kept at 60°C for 70 days, then taken out and left at room temperature for 1 hour to measure the mass loss. The MEK permeability (mg·cm / m2 ·sky).
[0191] MEK permeability (mg·cm / m 2 ·day) = [mass loss (mg) × thickness of sheet test piece (cm)] / [permeation area (m 2 )·Days (days)]
[0192] (85℃ load deflection)
[0193] Use pellets or powder and a hot press molding machine to make a sheet test piece with a thickness of about 2.3 mm, cut out a 80×10 mm test piece from it, and heat it at 100°C for 20 hours in an electric furnace. In addition to using the obtained test piece, according to the method described in JIS K-K7191-1, use a heat deformation tester (manufactured by Yasuda Seiki Manufacturing Co., Ltd.) to test at a test temperature of 30°C to 150°C, a heating rate of 120°C / hour, a bending stress of 1.8MPa, and a flat method. The load deflection rate is calculated by the following formula. The heat rigidity of the sheet with a small load deflection rate at 85°C is excellent.
[0194] Load deflection (%) = a2 / a1×100
[0195] a1: Thickness of the test piece before the test (mm)
[0196] a2: Deflection at 85°C (mm)
[0197] (Tensile strength after 60,000 cycles)
[0198] The tensile strength after 60,000 cycles was measured using a fatigue testing machine MMT-250NV-10 manufactured by Shimadzu Corporation. A sheet with a thickness of about 2.4 mm was made using pellets or powder and a hot pressing machine, and a dumbbell-shaped sample (thickness 2.4 mm, width 5.0 mm, measuring portion length 22 mm) was made using an ASTM D1708 micro dumbbell. The sample was mounted on a measuring fixture, and the measuring fixture was placed in a constant temperature bath at 150°C with the sample mounted. Stretching in a uniaxial direction was repeated with a stroke of 0.2 mm and a frequency of 100 Hz, and the tensile strength of each stretch (tensile strength when the stroke is +0.2 mm) was measured. The tensile strength after 60,000 cycles was calculated from the measured value according to the following formula. In this embodiment, the cross-sectional area of the sample is 12.0 mm 2 .
[0199] Tensile strength after 60,000 cycles (mN / mm 2 ) = tensile strength (60,000 times) (mN) / cross-sectional area of sample (mm 2 )
[0200] The tensile strength after 60,000 cycles is the ratio of the tensile strength to the cross-sectional area of the sample when the load is applied 60,000 times. A sheet with a high tensile strength after 60,000 cycles maintains a high tensile strength even after the load is applied 60,000 times, and has excellent durability against repeated loads.
[0201] (Tensile creep test)
[0202] The tensile creep strain was measured using a Hitachi High-Technologies Corporation TMA-7100. A sheet of about 0.1 mm thickness was made using pellets or powder and a hot press molding machine, and a sample of 2 mm width and 22 mm length was made from the sheet. The sample was mounted on a measuring fixture with a distance of 10 mm between the fixtures. For the sample, a cross-sectional load of 2.63 N / mm 2 The sample was loaded in a manner of 230°C, and the sample length displacement (mm) was measured from 90 minutes after the start of the test to 555 minutes after the start of the test, and the ratio of the length displacement (mm) to the initial sample length (10 mm) was calculated (tensile creep strain (%)). The sheet with a small tensile creep strain (%) measured at 230°C and 555 minutes is not easy to elongate even when a tensile load is applied in a very high temperature environment, and has excellent high temperature tensile creep resistance.
[0203] (230℃ tensile strength)
[0204] The pellets and a hot press molding machine were used to obtain a 2.0 mm thick test piece (compression molding). A dumbbell-shaped test piece was punched out from the test piece using an ASTM V-type dumbbell, and the obtained dumbbell-shaped test piece was used to measure the tensile strength at 230° C. under the conditions of 50 mm / min using Autograph (AG-I 300 kN manufactured by Shimadzu Corporation) according to ASTM D638.
[0205] A molded body having a high tensile strength at 230°C is not easily broken even when a tensile force is applied at a high temperature.
[0206] [Table 4]
[0207] Table 4
[0208]
Claims
1. A copolymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of the perfluoro(propyl vinyl ether) unit is 4.3% to 6.0% by mass based on the total monomer units. The melt flow rate at 372°C is 0.7 g / 10 min to 1.4 g / 10 min. The number of functional groups per 10 6 The number of carbon atoms in the main chain is 20 or less.
2. The copolymer according to claim 1, wherein The content of the perfluoro(propyl vinyl ether) unit is 4.6% by mass to 5.6% by mass based on the total monomer units.
3. The copolymer according to claim 1 or 2, wherein The melt flow rate at 372° C. is 0.7 g / 10 min to 1.3 g / 10 min. 4 . An extrusion molded product comprising the copolymer according to claim 1 . 5 . A transfer molded article comprising the copolymer according to claim 1 .
6. A molded product comprising the copolymer according to any one of claims 1 to 3, wherein The shaped body is a sheet or a tube.