Low-magnetic-conductance amorphous nanocrystalline master alloy material and preparation method thereof
By optimizing the composition and preparation process of Fe-Si-B-Cu-Nb iron-based nanocrystalline materials, the problem of high energy loss in alternating magnetic fields of existing low magnetic permeability alloy materials has been solved, and amorphous nanocrystalline master alloys with low magnetic permeability and high magnetic induction intensity have been prepared to meet market demand.
Patent Information
- Application Number
- CN202411123213.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
Existing low-permeability alloy materials suffer from high energy loss and large iron loss in alternating magnetic fields, making it difficult to meet market demands for low permeability and high magnetic induction intensity.
By optimizing the composition of Fe-Si-B-Cu-Nb iron-based nanocrystalline materials and strictly controlling the contents of copper, silicon, boron, niobium and cobalt, combined with the use of inert gas purging, slag remover and slag-forming agent, the materials are purified during the smelting process to form an amorphous nanocrystalline master alloy with low magnetic permeability and excellent soft magnetic properties.
It achieves a balance between low magnetic permeability and high magnetic induction intensity. The material exhibits low energy loss and low iron loss in alternating magnetic fields, meeting market demands.
Smart Images

Figure CN118996290A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of magnetic materials, and more specifically, to a low magnetic permeability amorphous nanocrystalline master alloy material and a preparation method thereof. Background Art
[0002] Low magnetic permeability alloy materials are often used in electromagnetic interference (EMI) shielding, magnetic isolation, magnetic field sensors, and other scenarios where magnetic field interference needs to be reduced. For example, in electronic devices, they can be used to shield the magnetic field around circuit boards or electronic components to reduce interference between devices; in medical devices, they can be used to manufacture magnets in magnetic resonance imaging (MRI) equipment to ensure the uniformity and stability of the magnetic field. Common low magnetic permeability alloys include nickel-iron alloys, cobalt-iron alloys, copper-nickel alloys, etc. These materials usually have good soft magnetic properties, that is, they are easy to magnetize and demagnetize under an external magnetic field, and have low residual magnetic induction intensity, but in an alternating magnetic field, the magnetic material produces high energy loss and high iron loss. Summary of the invention
[0003] The present application provides a low magnetic permeability master alloy material and a preparation method thereof. The prepared master alloy material has lower magnetic permeability and good soft magnetic properties. In an alternating magnetic field, the magnetic material generates low energy loss and low iron loss.
[0004] In the first aspect, the present application provides a low magnetic permeability amorphous nanocrystalline master alloy material adopts the following technical solution: a low magnetic permeability amorphous nanocrystalline master alloy material, comprising the following raw materials in mass percentage: 1.25-1.35% copper, 8.5-8.9% silicon, 1.2-1.7% boron, 5.4-5.65% niobium, 0.1-0.3% cobalt, and the balance is iron.
[0005] In a second aspect, the present application provides a method for preparing a low magnetic permeability amorphous nanocrystalline master alloy material, using the following technical solution: A method for preparing a low magnetic permeability amorphous nanocrystalline master alloy material comprises the following steps: Step 1, drying metallic silicon, pure iron, ferroniobium and ferroboron to obtain dry raw materials; Step 2, mixing the dried pure iron with 1 / 3-1 / 2 weight of ferroniobium and metallic silicon, heating until the materials are melted and keeping the temperature, introducing an inert gas, which is argon or a mixture of argon and oxygen, so that the liquid surface rolls 1-5 bubbles per second, and then adding the remaining ferroniobium in batches and using a slag remover to cover and remove slag and keep the temperature, to ensure that all the materials are fully melted; the amount of the slag remover added is 0.1-0.2% of the total weight of the molten iron after the pure iron is melted; Step 3, respectively adding ferroboron, electrolytic copper and remaining metallic silicon to the material in step 2 and keeping the temperature to obtain a melt; Step 4, adding a slag-forming agent to the melt and stirring, and then sprinkling a layer of slag-forming agent on the surface of the melt after slag removal and slagging, and pouring at a temperature of 100 °C, and cooling in a water-cooled ingot mold to form a master alloy material; the amount of the slag-forming agent added is 0.2-0.5% of the total weight of the melt; The slag-forming agent comprises white glass and high-calcium white lime particles.
[0006] By adopting the above technical scheme, the present invention optimizes the component design of the traditional Fe-Si-B-Cu-Nb iron-based nanocrystalline material, takes iron as the main element, strictly controls the contents of copper, silicon, boron, niobium and cobalt, and adjusts the magnetic permeability of the alloy material by means of the synergistic effect between the alloy elements, so that it has lower magnetic permeability and good soft magnetic properties, and in the alternating magnetic field, the magnetic material produces low energy loss and low iron loss, so that the iron-based nanocrystalline soft magnetic alloy has both good magnetic properties and mechanical properties; by adjusting the specific element ratio, the preparation meets the current market demand for amorphous nanocrystalline master alloy materials with high magnetic induction intensity and wide-band low magnetic permeability.
[0007] Iron is a magnetic element in nanocrystals and the main source of magnetism of iron-based amorphous and nanocrystalline alloy strips. The higher the Fe content, the higher the saturation magnetic induction intensity of the amorphous and nanocrystalline alloy strips. The mass percentage of the Fe element is preferably above 80%, but too high an Fe content will increase the core loss and deteriorate the amorphous forming ability of the alloy, reducing the yield of the strip. On the other hand, for the alloy system, a higher Fe content will increase the difficulty of preparing the amorphous alloy strip. Although the amorphous alloy strip can be prepared during the preparation process, the amorphous alloy strip in the prepared state is partially crystallized. The partially crystallized strip will have coarse grains after subsequent heat treatment, and the performance will deteriorate. The mass percentage upper limit of the Fe content of the present invention is 83%, and the Fe mass percentage range needs to be controlled within 81.5-82.5%.
[0008] Boron is a metalloid element. The B element has the effect of improving the amorphous formation of soft magnetic alloys, preventing the coarsening of crystal structures, and inhibiting the generation of compound phases in the heat treatment process, thereby enhancing thermal stability. The addition of the B element can not only keep the saturation magnetic induction intensity of the alloy at room temperature unchanged, but also improve the Curie temperature and crystallization temperature of the alloy, so that the alloy can be annealed and heat treated at a higher temperature annealing temperature, so that the alloy strip can fully eliminate internal stress and promote the formation of the alloy magnetic ordered state, thereby improving the magnetic properties of the alloy strip. When the B element content is less, it is difficult to make the alloy amorphous, resulting in a decrease in soft magnetic properties and an increase in core loss. When the B content is more, the mass percentage of Fe and Si in the alloy will be reduced, resulting in a decrease in magnetic flux density. The mass percentage upper limit of the Fe element content of the present invention is 1.7%, and the mass percentage range of the B element needs to be controlled at 1.2-1.7%.
[0009] Silicon is a metalloid element that can greatly improve the amorphous forming ability of the alloy and enhance thermal stability. The Si element exists in the alloy purification precipitation phase in the form of a solid solution, which can reduce the melting point of the amorphous alloy, increase the fluidity of the melt, thereby improving the amorphous forming ability, facilitating the preparation of amorphous alloy strips, and can also increase the resistivity of the amorphous alloy and reduce losses. Too high Si element content leads to core loss of amorphous alloy strips. The mass percentage upper limit of the Si element content of the present invention is 8.9%, and the mass percentage range of the Si element needs to be controlled within 8.5-8.9%.
[0010] The Cu element can be used as a heterogeneous nucleation point for the precipitation of α-Fe nanocrystals. The role of the Cu element is to promote the rapid nucleation of nanocrystalline iron particles and form nanocrystalline particles around the Cu element. Properly increasing the content of the Cu element is not only conducive to pre-storing more α-Fe nuclei in the process of forming amorphous, but also can promote the precipitation of more α-Fe nuclei during heat treatment. The newly formed nuclei and the pre-storage nuclei compete with each other to grow to avoid grain growth, forming a nanocrystalline structure with a smaller grain size and uniform distribution, which is conducive to improving the Bs of the alloy and achieving excellent comprehensive soft magnetic properties. Increasing the Cu content is also likely to form high Nd nucleation points in the alloy. However, if the Cu content is too high, the amorphous forming ability of the alloy will be reduced, and an amorphous alloy strip cannot be formed. The mass percentage upper limit of the Cu element content of the present invention is 1.35%, and the mass percentage range of the Cu element needs to be controlled at 1.25-1.35%.
[0011] Niobium is a transition metal element and an important element in iron-based nanocrystalline alloys. Nb plays an important role in the toughness of Fe-based amorphous and nanocrystalline strips and in controlling the size of nanocrystalline grains. Nb atoms can inhibit the growth of nanocrystalline grains, thereby refining the grains and improving the magnetic properties of the material. However, excessive addition of Nb will reduce the saturation magnetization intensity of nanocrystalline. The mass percentage of the Nb element content in the present invention is upper limited to 5.65%, and the mass percentage range of the Nb element needs to be controlled within 5.4-5.65%.
[0012] Cobalt is a pre-transition element, and Co is mainly used to improve the alloy system with iron. The Co element is also a strong magnetic element, and the addition of the Co element can increase the complexity of the alloy system, improve the fluidity of the alloy, improve the toughness of the spray strip, and then obtain a strip with better surface quality. On the other hand, the Co element can be preferentially combined with non-metallic elements such as B, Si elements, etc., and then retain more amorphous phases during the treatment process, inhibit the growth of nano-crystals with high iron content, refine the α-Fe grains in the crystallized alloy, and improve the Bs value and soft magnetic properties of the alloy system. However, from the perspective of the market application of amorphous nanocrystalline master alloy materials, the price of Co metal is high, and the mass percentage upper limit of the Co element content of the present invention is 0.3%, and the Co element mass percentage range needs to be controlled at 0.1-0.3%.
[0013] Furthermore, in step 2, pure iron is first placed in the smelting furnace, and after two circles, a layer of pure iron is laid at the bottom of the central hole area, and then the rest of the material is added to the central hole area. Through the above-mentioned material distribution method, the material can be melted evenly and is not easy to stick to the wall.
[0014] Furthermore, in step 4, the pouring temperature of the heat-insulating pouring is 1250° C.-1310° C., and then the master alloy material is formed after cooling in a water-cooled ingot mold.
[0015] By adopting the above technical scheme, the raw material components are first dried to remove moisture from each component, and the slag remover, inert gas purge and slag forming agent cooperate with each other, which can not only bond the slag and impurities in the molten material, play the role of slag gathering and slag removal, and purify the material, but also isolate the air and maintain the stability of the temperature, prevent the liquid surface from contacting with the air during the tumbling process to oxidize and form oxide scale or oxidized inclusions, and avoid adverse effects on subsequent process steps and material properties. During the smelting process, the rust on the surface of the material, the adhered dust, the oxides formed by the burning of the metal elements, and the corrosion of the furnace lining will interact with each other to form slag. The slag formed during the melting process has a high viscosity, which is not conducive to the smooth progress of the metallurgical reaction during the melting process. The slag forming agent is used to dilute the slag so that the slag in the melt can float up and be removed smoothly, and the high-temperature reaction and the slag in the melt in the furnace react to achieve the role of purifying the melt.
[0016] Preferably, the weight ratio of the white glass to the high-calcium white lime particles is (1.5-3):1.
[0017] Furthermore, the calcium content in the high-calcium white lime particles is greater than 96%, and the silicon dioxide content in the white glass is greater than 90%.
[0018] By adopting the above technical solution, high-calcium white lime particles can react with impurities in the melt to form slag or molten slag. At the same time, they can also react with sulfur S elements in the melt to form calcium sulfur compounds that are easy to remove, thereby reducing the sulfur content in the melt and effectively preventing the equipment from being blocked, thereby extending the service life of the equipment. Adding white glass can increase the adhesion of materials such as slag or molten slag in the melt in the furnace, so that inclusions in the slag are more easily wrapped by the melt, effectively reducing the inclusion content. In addition, white glass can also neutralize sulfur and oxygen elements in the melt, reducing the harmful effects of heavy impurities in the melt.
[0019] Preferably, the deslagging agent comprises the following raw materials in percentage by mass: 71-76% silicon dioxide, 11-16% aluminum oxide, 1-1.5% iron oxide, 1-2% calcium oxide, 3-4% potassium oxide, 3-4% sodium oxide, and inevitable impurities.
[0020] By adopting the above technical solution, the components of the slag remover are optimized, which is beneficial to bonding the slag and impurities in the molten metal during the smelting process, thereby playing the role of slag aggregation and slag removal.
[0021] Preferably, the drying process is carried out at a temperature of 200-260°C and for a time of 20-24 hours.
[0022] By adopting the above technical solution and selecting a suitable temperature for drying, it is helpful to remove moisture in the raw materials and reduce the adverse effects on the materials.
[0023] Preferably, in steps 2 to 4, the insulation temperature is 1450-1550°C.
[0024] By adopting the above technical solution, the temperature in the furnace is maintained within a suitable range to ensure that all raw materials can be fully melted.
[0025] Preferably, the silicon content in the metallic silicon is ≥99.6%, the iron content is ≤0.23%, the calcium content is <0.02%, and the aluminum content is <0.04%.
[0026] Preferably, the iron content of the ferroniobium is greater than 30%, the niobium content is 65.4-66.5%, and the particle size of the ferroniobium is 5-30 mm.
[0027] Preferably, the boron content in the ferroboron is ≥17%, manganese is <0.25%, carbon is <0.3%, silicon is <0.3%, phosphorus is <0.03%, sulfur is <0.03%, aluminum is <0.03%, titanium is <0.02%, and the balance is iron.
[0028] By adopting the above technical solution, the selection of metallic silicon, ferroniobium and ferroboron raw materials is optimized, which is beneficial to improving the comprehensive performance of the alloy material.
[0029] In summary, this application has the following beneficial effects: The present invention optimizes the components of the traditional Fe-Si-B-Cu-Nb iron-based nanocrystalline material, takes iron as the main element, strictly controls the contents of copper, silicon, boron, niobium and cobalt, and adjusts the magnetic permeability of the alloy material by means of the synergistic effect between the alloy elements, so that the alloy material has lower magnetic permeability and better soft magnetic properties. In addition, in the alternating magnetic field, the magnetic material generates low energy loss and low iron loss, so that the iron-based nanocrystalline soft magnetic alloy has both good magnetic properties and mechanical properties. By adjusting the specific element ratio, the preparation meets the current market demand for amorphous nanocrystalline master alloy materials with both high magnetic induction intensity and wide-band low magnetic permeability. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a SEM image of the strip obtained after spraying the low magnetic permeability amorphous nanocrystalline master alloy material of Example 1 of the present application. DETAILED DESCRIPTION
[0031] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. Example
[0032] Example 1 A low magnetic permeability amorphous nanocrystalline master alloy material is composed of the following raw materials in percentage by mass: 1.3% copper, 8.71% silicon, 1.5% boron, 5.52% niobium, 0.23% cobalt, and the balance is iron.
[0033] The method for preparing a low magnetic permeability amorphous nanocrystalline master alloy material comprises the following steps: Step 1, putting metallic silicon, pure iron, ferroniobium and ferroboron into a large hopper and entering a heat treatment furnace for drying at a temperature of 250±10°C for 24 hours to obtain a dry raw material; The silicon content of metallic silicon is ≥99.6%, iron ≤0.23%, calcium <0.02%, and aluminum <0.04%; The iron content in ferroniobium is more than 30%, niobium is 65.4-66.5%, silicon is less than 2%, tantalum is less than 0.05%, manganese is less than 0.5%, carbon is less than 0.15%, phosphorus is less than 0.15%, aluminum is less than 0.3%, titanium is less than 0.1%, lead is less than 0.15%, zinc is less than 0.05%, tin is less than 0.04%, sulfur is less than 0.02%, and the particle size of ferroniobium is 5-15mm; The boron content in ferroboron is ≥17%, manganese <0.25%, carbon <0.3%, silicon <0.3%, phosphorus <0.03%, sulfur <0.03%, aluminum <0.03%, titanium <0.02%, and the balance is iron; Step 2, put the dried pure iron into the smelting furnace, arrange it in two circles, and then lay another layer of pure iron at the bottom of the central hole area, and then add 1 / 3 of the total weight of ferroniobium and metallic silicon mixture to the central hole of the smelting furnace, heat until the materials are melted and keep warm, control the melt temperature in the furnace at 1550℃±10℃ and keep warm for 25 minutes, after all the pure iron is melted, turn on the argon blowing device, and pass argon gas so that the liquid surface rolls 1-2 bubbles per second; About 5 minutes after all the pure iron in the furnace is melted and falls into the liquid surface, add 1 / 3 of the total weight of ferroniobium. When adding ferroniobium, add it in small amounts at intervals of 4 minutes. When the ferroniobium alloy is added to the furnace melt, the temperature should be controlled at 1530℃±10℃. Then use a slag remover to cover and remove the slag. After the pure iron slag is removed, add the remaining 1 / 3 of the weight of ferroniobium. When adding ferroniobium, add it in small amounts at intervals of 4 minutes. After the materials are added, keep them warm for 10 minutes to ensure that all the materials are fully melted. The amount of slag remover added is 0.15% of the total weight of the molten iron after the pure iron is melted. The deslagging agent comprises the following raw materials in percentage by mass: 75% silicon dioxide, 14% aluminum oxide, 1.2% iron oxide, 1.8% calcium oxide, 3.5% potassium oxide, 4% sodium oxide, and the balance of inevitable impurities; Step 3, adding ferroboron to the material in step 2, controlling the melt temperature in the furnace to 1500±10°C, adding in small amounts at intervals for 3 minutes, keeping warm for 8 minutes after all the materials are added, and ensuring that the ferroboron alloy is fully melted, and then adding electrolytic copper with a copper content of 99.9% and the remaining metallic silicon, the melt temperature is controlled at 1480±10°C, adding in small amounts at intervals for 3 minutes, keeping warm for 8 minutes after all the materials are added, ensuring that the materials are fully melted to obtain a melt; Step 4: Add slag-forming agent to the melt and stir the melt to quickly slag for 3 minutes. Use a steel rod to turn over the melt. After slagging, sprinkle a layer of slag-removing agent on the surface of the melt to cover the melt by 1mm. The melt is cooled by low-power power supply. The power supply of ABP electric furnace is 100Kw to ensure that the melt surface rolls slightly and keeps warm. This process ensures that the melt temperature decreases slowly and measures the temperature at all times. The cooling process takes 10-15 minutes and the furnace temperature drops to 1 At 350±10℃, the liquid surface is skimmed and slag removed to ensure that the melt surface is pure and free of floating residues. When the melt is discharged from the furnace, the electric furnace is powered off and the argon gas is turned off. The discharge temperature is 1280±10℃. The melt is slowly poured into the water-cooled ingot mold. The pouring temperature is 1250±10℃. The circulating cooling water pressure of the water-cooled ingot mold is 1.4Mpa. After cooling in the water-cooled ingot mold, the master alloy material is formed. The amount of slag-forming agent added is 0.3% of the total weight of the melt. The slag-making agent comprises white glass and high-calcium white lime particles in a mass ratio of 2:1, wherein the silicon dioxide content in the white glass is 95%, the calcium content in the high-calcium white lime particles is 98%, and the particle size is 2-3 mm.
[0034] Example 2 A low magnetic permeability amorphous nanocrystalline master alloy material is composed of the following raw materials in percentage by mass: 1.35% copper, 8.5% silicon, 1.2% boron, 5.65% niobium, 0.2% cobalt, and the balance is iron.
[0035] The method for preparing a low magnetic permeability amorphous nanocrystalline master alloy material comprises the following steps: Step 1, putting metallic silicon, pure iron, ferroniobium and ferroboron into a large hopper and entering a heat treatment furnace for drying at a temperature of 210±10°C for 24 hours to obtain a dry raw material; The silicon content of metallic silicon is ≥99.6%, iron ≤0.23%, calcium <0.02%, and aluminum <0.04%; The iron content of ferroniobium is more than 30%, niobium is 65.4-66.5%, silicon is less than 2%, tantalum is less than 0.05%, manganese is less than 0.5%, carbon is less than 0.15%, phosphorus is less than 0.15%, aluminum is less than 0.3%, titanium is less than 0.1%, lead is less than 0.15%, zinc is less than 0.05%, tin is less than 0.04%, sulfur is less than 0.02%, and the particle size of ferroniobium is 15-30mm; The boron content in ferroboron is ≥17%, manganese <0.25%, carbon <0.3%, silicon <0.3%, phosphorus <0.03%, sulfur <0.03%, aluminum <0.03%, titanium <0.02%, and the balance is iron; Step 2, put the dried pure iron into the smelting furnace, arrange it in two circles, and then lay another layer of pure iron at the bottom of the central hole area, and then add 1 / 2 of the total weight of ferroniobium and metallic silicon to the central hole of the smelting furnace, heat until the materials are melted and keep warm, control the melt temperature in the furnace at 1480℃±10℃ for 20 minutes, and after all the pure iron is melted, introduce a mixed gas of argon and oxygen in a volume ratio of 10:1, so that 3-5 bubbles roll on the liquid surface per second; 5 minutes after all the pure iron in the furnace is melted and falls into the liquid surface, add 1 / 2 of the total weight of ferroniobium. When adding ferroniobium, add it in small amounts at intervals of 3-5 minutes. When the ferroniobium alloy is added to the furnace melt, the temperature should be controlled at 1500℃±10℃. After the materials are added, keep them warm for 10 minutes to ensure that all the materials are fully melted. Then, use a slag remover to cover and remove the slag. The amount of the slag remover added is 0.2% of the total weight of the molten iron after the pure iron is melted; The deslagging agent comprises the following raw materials in percentage by mass: 71% silicon dioxide, 16% aluminum oxide, 1% iron oxide, 1% calcium oxide, 4% potassium oxide, 3% sodium oxide, and the balance of inevitable impurities; Step 3, adding ferroboron to the material in step 2, controlling the melt temperature in the furnace to 1500±10°C, adding in small amounts at intervals for 3 minutes, keeping warm for 5 minutes after all the materials are added, and ensuring that the ferroboron alloy is fully melted, and then adding electrolytic copper with a copper content of 99.9% and the remaining metallic silicon, the melt temperature is controlled at 1480±10°C, adding in small amounts at intervals for 5 minutes, and keeping warm for 10 minutes after all the materials are added, ensuring that the materials are fully melted to obtain a melt; Step 4: Add slag-forming agent to the melt and stir the melt to quickly slag for 5 minutes. Use a steel rod to turn over the melt. After slagging, sprinkle a layer of slag-removing agent on the melt surface to cover the melt by 1mm. The melt is cooled by low-power power supply. The power supply of ABP electric furnace is 100Kw to ensure that the melt surface rolls slightly and keeps warm. This process ensures that the melt temperature decreases slowly and measures the temperature at all times. The cooling process takes 10-15 minutes and the furnace temperature drops to 1 At 350±10℃, the liquid surface is slag-removed to ensure that the melt surface is pure and free of floating residues. When the melt is discharged from the furnace, the electric furnace is powered off and the argon gas is turned off. The discharge temperature is 1280±10℃. The melt is slowly poured into the water-cooled ingot mold. The circulating cooling water pressure of the water-cooled ingot mold is 1.2Mpa, and the pouring temperature is 1250±10℃. After cooling in the water-cooled ingot mold, the master alloy material is formed. The amount of slag-forming agent added is 0.5% of the total weight of the melt. The slag-making agent comprises white glass and high-calcium white lime particles in a mass ratio of 1.5:1, wherein the silicon dioxide content in the white glass is 91%, the calcium content in the high-calcium white lime particles is 97%, and the particle size is 2-3 mm.
[0036] Example 3 The difference from Example 1 is that in step 2, the slag remover includes the following raw materials in percentage by mass: 76% silicon dioxide, 11% aluminum oxide, 1.5% iron oxide, 2% calcium oxide, 3.2% potassium oxide, 3.8% sodium oxide, and inevitable impurity residues; the rest are the same as in Example 1.
[0037] Example 4 The difference from Example 1 is that the silicon content in the metallic silicon is 95%, the iron content in the ferroniobium is 28%, the niobium content is 66%, and the boron content in the ferroboron is 15%; the rest is the same as Example 1.
[0038] Example 5 The difference from Example 1 is that the weight ratio of white glass to high-calcium white lime particles is 3:1, and the rest is the same as Example 1.
[0039] Example 6 The difference from Example 1 is that the weight ratio of white glass to high-calcium white lime particles is 1:1, the calcium content in the high-calcium white lime particles is 90%, and the silicon dioxide content in the white glass is 90%. The rest is the same as Example 1.
[0040] Example 7 The difference from Example 1 is that the amount of slag remover added is 0.1% of the total weight of molten iron after pure iron is melted, and the amount of slag forming agent added is 0.2% of the total weight of the melt. The rest is the same as Example 1.
[0041] Comparative Example Comparative Example 1 The difference from Example 1 is that the low magnetic permeability amorphous nanocrystalline master alloy material is composed of the following raw materials in percentage by mass: 0.8% copper, 10% silicon, 1.0% boron, 5.9% niobium, 0.5% cobalt, and the balance is iron.
[0042] Comparative Example 2 The difference from Example 1 is that the low magnetic permeability amorphous nanocrystalline master alloy material is composed of the following raw materials in percentage by mass: 1.26% copper, 7.2% silicon, 1.7% boron, 3.7% niobium, 2.3% manganese, and the balance is iron.
[0043] Comparative Example 3 The difference from Example 1 is that steps 2 to 4 are omitted, and the dried metallic silicon, pure iron, ferroniobium and ferroboron are directly melted, argon gas is introduced, and a slag remover is added to remove the slag and scrape the slag, and then a slag forming agent is added to remove the slag and scrape the slag, and the electric furnace is powered off and the argon gas is turned off when the melt is discharged from the furnace. The discharge temperature is 1280±10°C, and the melt is slowly poured into a water-cooled ingot mold at a pouring temperature of 1250±10°C. After cooling in the water-cooled ingot mold, a master alloy material is formed.
[0044] Comparative Example 4 The difference from Example 1 is that the added amount of the slag remover is 0.5% of the total weight of the molten iron after the pure iron is melted, the slag remover is 60wt% of calcium oxide and 40wt% of calcium silicate, and the rest is the same as Example 1.
[0045] Comparative Example 5 The difference from Example 1 is that the slag-forming agent is white glass with a particle size of 3-5 mm, and the amount of the slag-forming agent added is 0.1% of the total weight of the melt. The rest is the same as Example 1.
[0046] Performance testing The master alloy materials obtained in Examples 1-7 and Comparative Examples 1-5 were sprayed to obtain strips. According to the standards: GB / T19345.1-2017 "Amorphous Nanocrystalline Alloys Part 1 Iron-based Amorphous Soft Magnetic Alloy Strip", GB / T 19345.2-2017 "Amorphous Nanocrystalline Alloys Part 2 Iron-based Nanocrystalline Soft Magnetic Alloy Strip", GB / T 19346.1-2017 "Test Methods for Amorphous Nanocrystalline Alloys Part 1: AC Magnetic Properties of Ring-shaped Specimens", the saturation magnetic induction intensity, magnetic permeability 1 (1kHz / transverse magnetic field 560°C annealing for 2 hours), magnetic permeability 2 (10kHz / transverse magnetic field 560°C annealing for 2 hours), and iron loss (0.3T / 100k) were tested, and the results are shown in Table 1.
[0047] Table 1 In combination with Examples 1-7 and Table 1, it can be seen that the material element components of the present application are used with the help of the synergistic effect between the alloy elements and in combination with a specific preparation method to adjust the magnetic permeability of the alloy material so that it has lower magnetic permeability and good soft magnetic properties, and in the alternating magnetic field, the magnetic material produces low energy loss and low iron loss, so that the iron-based nanocrystalline soft magnetic alloy has both good magnetic properties and mechanical properties, meeting the current market demand for amorphous nanocrystalline master alloy materials with both high magnetic induction intensity and wide-band low magnetic permeability.
[0048] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low magnetic permeability amorphous nanocrystalline master alloy material, characterized in that: The invention comprises the following raw materials in percentage by mass: 1.25-1.35% copper, 8.5-8.9% silicon, 1.2-1.7% boron, 5.4-5.65% niobium, 0.1-0.3% cobalt, and the balance is iron.
2. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 1, characterized in that: The following steps are involved: Step 1, drying metallic silicon, pure iron, ferroniobium and ferroboron to obtain dry raw materials; Step 2, mixing the dried pure iron with 1 / 3-1 / 2 weight of ferroniobium and metallic silicon, heating until the materials are melted and keeping the temperature, introducing an inert gas, wherein the inert gas is one or two of argon or a mixture of argon and oxygen, so that the liquid surface rolls 1-5 bubbles per second, and then adding the remaining ferroniobium in batches and using a slag remover to cover and remove slag and keep the temperature, to ensure that all the materials are fully melted; the amount of the slag remover added is 0.1-0.2% of the total weight of the molten iron after the pure iron is melted; Step 3, respectively adding ferroboron, electrolytic copper and remaining metallic silicon to the material in step 2 and keeping the temperature to obtain a melt; Step 4, adding a slag-forming agent to the melt and stirring, removing slag and slagging, and then sprinkling a layer of slag-forming agent on the surface of the melt, pouring under heat preservation, and forming a master alloy material after cooling; the amount of the slag-forming agent added is 0.2-0.5% of the total weight of the melt; The slag-forming agent comprises white glass and high-calcium white lime particles.
3. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 2, characterized in that: The weight ratio of the white glass to the high-calcium white lime particles is (1.5-3):
1.
4. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 3, characterized in that: The deslagging agent comprises the following raw materials in percentage by mass: 71-76% silicon dioxide, 11-16% aluminum oxide, 1-1.5% iron oxide, 1-2% calcium oxide, 3-4% potassium oxide, 3-4% sodium oxide, and inevitable impurities.
5. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 2, characterized in that: The drying process is carried out at a temperature of 200-260° C. and for a time of 20-24 hours.
6. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 2, characterized in that: In the steps 2 to 4, the insulation temperature is 1450-1550°C.
7. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 2, characterized in that: The metal silicon has a silicon content of ≥99.6%, an iron content of ≤0.23%, a calcium content of <0.02%, and an aluminum content of <0.04%.
8. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 7, characterized in that: The iron content of the ferroniobium is greater than 30%, the niobium content is 65.4-66.5%, and the particle size of the ferroniobium is 5-30 mm.
9. The method for preparing the low magnetic permeability amorphous nanocrystalline master alloy material according to claim 8, characterized in that: The boron content of the ferroboron is ≥17%, manganese is <0.25%, carbon is <0.3%, silicon is <0.3%, phosphorus is <0.03%, sulfur is <0.03%, aluminum is <0.03%, titanium is <0.02%, and the balance is iron.
Citation Information
Patent Citations
Mother alloy for iron-based nanocrystalline alloy, smelting technology for mother alloy and cast steel groove used in smelting technology
CN107385325A
Ultralow-Al iron-based nanocrystalline master alloy and preparation method thereof
CN116855845A
Manufacture of fe-base magnetic alloy
JP1989031922A