Two-component coating composition

By reacting components A and components B in the two-component coating composition to form a coating, the shortcomings of existing easy-to-clean coatings in preventing smear and graffiti pollution are solved, and efficient cleaning and durability are achieved.

CN118974122APending Publication Date: 2024-11-15COVESTRO DEUTSCHLAND AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032433.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2023-03-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing easy-to-clean paints are difficult to effectively prevent malicious smearing and graffiti pollution, and they have poor protection effects on the interior walls, and there are certain difficulties in the cleaning process.

Method used

Two-component coating compositions are used, in which component A is an aqueous polyacrylic acid dispersion containing hydroxyl groups, and in which component B is a polyether modified polyisocyanate, forming a clean and durable one through a specific molar ratio and component ratio. coating.

Benefits of technology

It realizes the formation of an easy-to-clean and durable coating on the surface of the substrate, which can effectively prevent smearing and graffiti contamination, and shows good easy-to-cleaning performance during the cleaning process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070049220000061
    Figure BDA0005070049220000061
  • Figure BDA0005070049220000091
    Figure BDA0005070049220000091
  • Figure BDA0005070049220000261
    Figure BDA0005070049220000261
Patent Text Reader

Abstract

The invention relates to a two-component coating composition, a coating method and application of the two-component coating composition, and a product obtained by coating the two-component coating composition. The bi-component coating composition comprises a component A and a component B, the component A comprises a hydroxyl-containing aqueous polyacrylic acid dispersion, the component B comprises polyether modified polyisocyanate, and the molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.2: 1-2: 1; the hydroxyl content of the hydroxyl-containing water-based polyacrylic acid dispersion is greater than 2% by weight, and the weight-average molecular weight of the hydroxyl-containing water-based polyacrylic acid dispersion is not higher than 450,000 relative to the total weight of solid components of the hydroxyl-containing water-based polyacrylic acid dispersion. The double-component coating composition provided by the invention has a matte effect and is easy to clean.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a two-component coating composition, a coating method and application of the coating composition, and a product obtained by coating the coating composition. Background Art

[0002] Globally, many public facilities, such as urban underground passages, culverts, and building exterior walls, are increasingly being affected by the damage caused by malicious graffiti. It not only seriously affects the city appearance and landscape, but also requires a lot of manpower and material resources to remove malicious graffiti. Easy-to-clean coatings can create a barrier between the surface to be protected and the graffiti, making it difficult to write or easy to remove graffiti. In addition, as people's requirements for interior wall decoration increase, especially for the walls of some functional rooms such as children's rooms, kitchens, and restaurants, an easy-to-clean coating that can prevent graffiti from contaminating the interior walls is needed.

[0003] At present, the commonly used easy-to-clean coatings on the market mainly include fluororesin coatings, water-based cross-linked fluorine-containing compound coatings, polyurethane coatings and silicone-modified coatings.

[0004] CN101585995A discloses a silicone-modified two-component coating based on acrylic resin, comprising component A and component B, wherein component A comprises hydroxy acrylic resin, fluorocarbon resin, modified polydimethylsiloxane resin, polyacrylate-modified silicone resin, smoothing flow agent, leveling agent, defoaming agent, drying agent, dibutyltin dilaurate, butyl acetate and xylene; and component B comprises hexamethyl diisocyanate biuret, butyl acetate and ethylene glycol ethyl ether acetate.

[0005] US7501472B2 discloses an aqueous fluororesin system for one-component or two-component anti-graffiti and antifouling coatings, which can be obtained by the following process: (a) preparing a dispersion of hydroxyl and / or amino functional urethane oligomers and / or polyurethanes and (b) optionally reacting them with a crosslinker component.

[0006] CN 111057456 A discloses a method for preparing a water-based two-component polyurethane anti-cleaning paint, wherein component A is a water-based resin such as a water-based hydroxyl polyacrylic acid dispersion, and component B is a water-based polyurethane curing agent. Summary of the invention

[0007] The purpose of the present invention is to provide a two-component coating composition, a coating method and application of the coating composition, and a product obtained by coating the coating composition.

[0008] The two-component coating composition according to the present invention comprises component A and component B, wherein component A comprises a hydroxyl-containing aqueous polyacrylic acid dispersion, and component B comprises a polyether-modified polyisocyanate, wherein the molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.2:1-2:1; the hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is greater than 2% by weight, and the weight average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is not higher than 450,000, based on the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion; and the polyether-modified polyisocyanate is obtained by reacting a system comprising the following components:

[0009] a) a polyisocyanate having an isocyanate group functionality of 2 to 4.5, comprising at least 30% by weight of hexamethylene diisocyanate trimer, pentamethylene diisocyanate trimer or a combination thereof;

[0010] b) a polyoxyalkylene monoether alcohol; and

[0011] c) optionally a catalyst;

[0012] The number average molecular weight of the polyoxyalkylene monoether alcohol is 250 g / mol-700 g / mol, and the content of oxyethylene groups is 75 wt %-100 wt %, relative to the total weight of the oxyethylene groups of the polyoxyalkylene monoether alcohol; the polyether-modified polyisocyanate has the following characteristics:

[0013] i) an average isocyanate functionality of 1.8 to 4.1;

[0014] ii) an isocyanate group content of 8 wt% to 21 wt% relative to the total weight of the polyisocyanate; and

[0015] iii) a number average molecular weight of 500 g / mol to 1200 g / mol;

[0016] The amount of the polyoxyalkylene monoether structure of the B component is greater than 6.5 wt % and less than 12 wt % relative to the total weight of the B component.

[0017] According to one aspect of the present invention, there is provided use of the two-component coating composition provided according to the present invention for protecting a substrate surface or a coating on a substrate surface.

[0018] According to another aspect of the present invention, a coating method is provided, comprising the following steps: applying the two-component coating composition provided by the present invention to a substrate surface, followed by curing and drying.

[0019] According to another aspect of the present invention, a coating product is provided, which comprises a substrate and a two-component coating composition according to the present invention applied to the substrate, cured, and dried to form a coating. DETAILED DESCRIPTION

[0020] The invention provides a two-component coating composition, comprising component A and component B, wherein the component A comprises a hydroxyl-containing aqueous polyacrylic acid dispersion, the component B comprises a polyether-modified polyisocyanate, the molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.2:1-2:1; the hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is greater than 2% by weight, and the weight-average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is not higher than 450,000 based on the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion; the polyether-modified polyisocyanate is obtained by reacting a system comprising the following components: a) a polyisocyanate having an isocyanate group functionality of 2-4.5, comprising at least 30% by weight of hexamethylene diisocyanate trimer, pentamethylene diisocyanate trimer or a combination thereof; b) a polyoxyalkylene monoether alcohol; and c) an optional catalyst; the number average molecular weight of the polyoxyalkylene monoether alcohol is 250 g / mol-700 g / mol, and the content of oxyethylene groups is 75 wt%-100 wt%, relative to the total weight of the oxyethylene groups of the polyoxyalkylene monoether alcohol; the polyether-modified polyisocyanate has the following characteristics: i) an average isocyanate functionality of 1.8-4.1; ii) an isocyanate group content of 8 wt%-21 wt% relative to the total weight of the polyisocyanate; and iii) a number average molecular weight of 500 g / mol-1200 g / mol; the amount of the polyoxyalkylene monoether structure of the B component is greater than 6.5 wt% and less than 12 wt%, relative to the total weight of the B component. The present invention also provides a coating method and application of the two-component coating composition, and a product obtained by coating the coating composition.

[0021] In a preferred embodiment, the present invention provides a two-component coating composition, comprising component A and component B, wherein component A comprises a hydroxyl-containing aqueous polyacrylic acid dispersion, and component B comprises a polyether-modified polyisocyanate, wherein the molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.2:1-2:1; the hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is greater than 2% by weight, and the weight average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is not higher than 450,000, based on the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion; and the polyether-modified polyisocyanate is obtained by reacting a system comprising the following components:

[0022] a) a polyisocyanate having an isocyanate group functionality of 2 to 4.5, comprising at least 30% by weight of hexamethylene diisocyanate trimer, pentamethylene diisocyanate trimer or a combination thereof;

[0023] b) a polyoxyalkylene monoether alcohol; and

[0024] c) optionally a catalyst;

[0025] The number average molecular weight of the polyoxyalkylene monoether alcohol is 250 g / mol-400 g / mol, and the content of oxyethylene groups is 75 wt %-100 wt %, relative to the total weight of the oxyethylene groups of the polyoxyalkylene monoether alcohol; the polyether-modified polyisocyanate has the following characteristics:

[0026] i) an average isocyanate functionality of 1.8 to 4.1;

[0027] ii) an isocyanate group content of 8 wt% to 21 wt% relative to the total weight of the polyisocyanate; and

[0028] iii) a number average molecular weight of 500 g / mol to 1200 g / mol;

[0029] The amount of the polyoxyalkylene monoether structure of the B component is greater than 8 wt % and less than 11 wt % relative to the total weight of the B component.

[0030] Two-component coating composition

[0031] The two-component coating composition described herein, the term two-component refers to a coating composition comprising at least two components that must be stored in separate containers due to their mutual reactivity. When the two separate components are mixed and applied to a substrate, the mutually reactive compounds in the two components react to crosslink and form a cured coating.

[0032] The terms "curing, drying" as used herein refer to the process of a liquid coating composition changing from a liquid state to a cured state.

[0033] The term "trimer" as used herein refers to the pure trimer, a mixture of the trimer and its higher homologues containing more than one isocyanurate ring.

[0034] The solid content of the dispersion of the present invention refers to the solid component of the dispersion or the effective component of the dispersion.

[0035] The molar ratio of isocyanate groups to hydroxyl groups of the two-component coating composition is preferably 1.3:1-1.7:1.

[0036] The two-component coating composition is preferably water-borne.

[0037] Component A

[0038] The hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is preferably greater than 2 wt% and not greater than 5 wt%, most preferably 2.5 wt% to 5 wt%, relative to the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion.

[0039] The weight average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is preferably not higher than 450,000, more preferably 30,000-450,000, most preferably 30,000-350,000, and the weight average molecular weight is determined according to GB / T21863-2008 by gel permeation chromatography with DMF as the mobile phase and against a polystyrene standard.

[0040] The solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion is preferably 35% to 50% by weight, most preferably 39% to 46% by weight, relative to the total weight of the hydroxyl-containing aqueous polyacrylic acid dispersion.

[0041] Component B

[0042] The amount of the polyoxyalkylene monoether structure of the B component is preferably 7% by weight to 11% by weight, most preferably 8% by weight to 11% by weight, relative to the total weight of the B component.

[0043] The B component preferably further has the following characteristics:

[0044] The average isocyanate functionality is 1.8-4.1;

[0045] The isocyanate group content is 8-21 wt % relative to the total weight of the B component; and the number average molecular weight is 500 g / mol-1200 g / mol.

[0046] The number average molecular weight of the B component is determined at 23° C. using gel permeation chromatography with tetrahydrofuran as the mobile phase and a polystyrene standard according to DIN 55672-1:2016-03.

[0047] The content of isophorone diisocyanate trimer in the B component is preferably not more than 0.5% by weight, relative to the total weight of the B component.

[0048] The average isocyanate functionality of the B component is most preferably from 2.0 to 4.0.

[0049] The isocyanate group content of the B component is preferably 10% to 21% by weight, most preferably 15% to 21% by weight, relative to the total weight of the B component.

[0050] In the present invention, when component B contains components such as catalysts, auxiliary agents, additives, etc., when calculating the isocyanate group content, the amount of isophorone diisocyanate trimer and the amount of polyoxyalkylene monoether structure of the component B, the total weight of the component B is the total weight of the components containing NCO groups in the component B, and the components not containing NCO groups such as catalysts, auxiliary agents, additives, etc. in the component B are not included in the total weight of the component B.

[0051] Polyether modified polyisocyanate

[0052] The polyether-modified polyisocyanate of the present invention may exist in the form of a mixture, which may contain unreacted components in the system.

[0053] The polyether-modified polyisocyanate of the present invention is transparent and almost colorless.

[0054] The average isocyanate functionality of the polyether-modified polyisocyanate is preferably 2.0-4.0, most preferably 2.5-3.5.

[0055] The isocyanate group content of the polyether-modified polyisocyanate is preferably 10% to 21% by weight, most preferably 15% to 21% by weight, relative to the total weight of the polyether-modified polyisocyanate.

[0056] The number average molecular weight of the polyether-modified polyisocyanate is preferably 700 g / mol-1000 g / mol.

[0057] The viscosity of the polyether-modified polyisocyanate is preferably 500 mPa·s to 3500 mPa·s.

[0058] The amount of the polyoxyalkylene monoether structure of the polyether-modified polyisocyanate is preferably greater than 6.5 wt % and less than 12 wt %, further preferably 7 wt %-11 wt %, most preferably 8 wt %-11 wt %, relative to the total weight of the polyether-modified polyisocyanate.

[0059] The isophorone diisocyanate trimer content of the polyether-modified polyisocyanate is preferably not more than 0.5% by weight, relative to the total weight of the polyether-modified polyisocyanate.

[0060] The polyether-modified polyisocyanate most preferably does not contain isophorone diisocyanate trimer.

[0061] The amount of the polyether-modified polyisocyanate is preferably 88% to 93.5% by weight, based on the total weight of the B component.

[0062] The color value of the polyether-modified polyisocyanate is preferably less than 120, most preferably less than 30.

[0063] The polyether-modified polyisocyanate is preferably an aliphatic polyisocyanate composition, an alicyclic polyisocyanate composition or a combination thereof.

[0064] The average isocyanate functionality of the polyether-modified polyisocyanate is calculated according to the following formula:

[0065]

[0066] Where, F: average isocyanate functionality of polyether-modified polyisocyanate

[0067] ∑EquivNCO: The sum of the equivalent weights of isocyanate functional groups of the polyisocyanates with an isocyanate group functionality of 2-4.5 in component a

[0068] ∑Equiv OH: the sum of the hydroxyl equivalents of the polyoxyalkylene monoether alcohol in component b

[0069] f NCO : Component a) of the system: the isocyanate group functionality of a polyisocyanate having an isocyanate group functionality of 2-4.5, calculated from the isocyanate group content of the polyisocyanate and the molecular weight of the polyisocyanate, the molecular weight being determined by gel permeation chromatography (GPC)

[0070] ∑mol OH: the sum of the molar numbers of hydroxyl functional groups of the polyoxyalkylene monoether alcohol of component b.

[0071] The equivalent ratio of isocyanate groups to hydroxyl groups of the system is preferably 5:1 to 110:1.

[0072] Component a) Polyisocyanate with an isocyanate group functionality of 2-4.5

[0073] The isocyanate group functionality of the polyisocyanate having an isocyanate group functionality of 2-4.5 is preferably 2.5-4.4, more preferably 2.5-4, and most preferably 3-4.

[0074] The viscosity of the polyisocyanate having an isocyanate group functionality of 2-4.5 is preferably 500 mPa·s-4000 mPa·s.

[0075] The isocyanate group content of the polyisocyanate having an isocyanate group functionality of 2-4.5 is preferably 15% to 25% by weight, most preferably 16% to 24% by weight, based on 100% by weight of the polyisocyanate having an isocyanate group functionality of 2-4.5 in component a).

[0076] The polyisocyanate with an isocyanate group functionality of 2-4.5 comprises one or more of the following: hexamethylene diisocyanate trimer and pentamethylene diisocyanate trimer. The amount of the hexamethylene diisocyanate trimer, pentamethylene diisocyanate trimer or a combination thereof is at least 30% by weight, preferably 35% by weight to 100% by weight, further preferably 40% by weight to 100% by weight, further preferably 50% by weight to 100% by weight, most preferably 65% ​​by weight to 100% by weight, relative to the total weight of the polyisocyanate with an isocyanate group functionality of 2-4.5.

[0077] Preferably, the component a) polyisocyanate having an isocyanate group functionality of 2 to 4.5 further comprises another isocyanate.

[0078] The amount of the other isocyanates is preferably not more than 70% by weight, further preferably not more than 60% by weight, still more preferably not more than 50% by weight, most preferably not more than 35% by weight, relative to the total weight of the component a) polyisocyanate having an isocyanate group functionality of 2 to 4.5.

[0079] The other isocyanates are preferably one or more of the following: aliphatic polyisocyanates and alicyclic polyisocyanates, more preferably aliphatic polyisocyanates, still preferably one or more of the following: aliphatic isocyanate uretdione and aliphatic isocyanate biuret, still more preferably one or more of the following: hexamethylene diisocyanate uretdione, hexamethylene diisocyanate biuret and pentamethylene diisocyanate uretdione, most preferably one or more of the following: hexamethylene diisocyanate uretdione and hexamethylene diisocyanate biuret.

[0080] The amount of hexamethylene diisocyanate uretdione and / or hexamethylene diisocyanate biuret is preferably not more than 65% by weight, further preferably not more than 60% by weight, still more preferably not more than 50% by weight, most preferably not more than 35% by weight, relative to the total weight of the component a) polyisocyanate having an isocyanate group functionality of 2 to 4.5.

[0081] When the system comprises two or more polyisocyanates, the isocyanate group functionality of the polyisocyanate refers to the average isocyanate group functionality of the two or more polyisocyanates.

[0082] The amount of polyisocyanate having an isocyanate group functionality of 2 to 4.5 is preferably greater than 30% by weight, most preferably greater than 50% by weight, relative to the total weight of the system.

[0083] Component b) Polyoxyalkylene monoether alcohol

[0084] The number average molecular weight of the component b) polyoxyalkylene monoether alcohol is preferably 250 g / mol to 600 g / mol, more preferably 250 g / mol to 500 g / mol, most preferably 250 g / mol to 400 g / mol.

[0085] The component b) polyoxyalkylene monoether alcohol preferably has an oxyethylene group content of 80% to 100% by weight, most preferably 90% to 100% by weight, relative to the total weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0086] The component b) polyoxyalkylene monoether alcohol is preferably polyethylene glycol monomethyl ether containing 5 to 14 ethylene oxide units on average, further preferably polyethylene glycol monomethyl ether containing 5 to 12 ethylene oxide units on average, and most preferably polyethylene glycol monomethyl ether containing 5 to 9 ethylene oxide units on average.

[0087] The polyoxyalkylene monoether alcohol can be obtained by a known method, and the preferred starting components include a monohydric alcohol, a secondary monoamine and an oxyalkylene compound, wherein the monohydric alcohol and the secondary monoamine are present either alone or simultaneously.

[0088] The monohydric alcohol is preferably a monohydric alcohol with a molecular weight of 30 g / mol to 150 g / mol, such as the monohydric alcohol used according to EPA-206059, and most preferably one or more of the following: methanol and butanol.

[0089] The secondary monoamine is preferably one or more of the following: dimethylamine and diethylamine.

[0090] The alkylene oxide compound preferably contains 75% to 100% by weight, further preferably 80% to 100% by weight, most preferably 90% to 100% by weight of ethylene oxide, relative to the total weight of the alkylene oxide compound.

[0091] The oxyalkylene compound may further contain propylene oxide, and the amount of the oxyalkylene compound is preferably not more than 25 wt%, more preferably not more than 20 wt%, and most preferably not more than 10 wt%, relative to the total weight of the oxyalkylene compound.

[0092] The starting components are preferably reacted at 40°C to 150°C, most preferably 60°C to 130°C.

[0093] The NCO / OH equivalent ratio of the starting components is preferably 5: 1 to 110: 1, most preferably 8: 1 to 90: 1. The starting components are preferably reacted further until the theoretically calculated isocyanate content is reached.

[0094] The hydroxyl value of the component b) polyoxyalkylene monoether alcohol is preferably 93 mgKOH / g to 224 mgKOH / g, and the hydroxyl value is measured according to ASTM D4274.

[0095] When the system comprises two or more polyoxyalkylene monoether alcohols, the number average molecular weight of the polyoxyalkylene monoether alcohol refers to the average number average molecular weight of the two or more polyoxyalkylene monoether alcohols; the oxyethylene group content of the polyoxyalkylene monoether alcohol refers to the average oxyethylene group content of the two or more polyoxyalkylene monoether alcohols, that is, the average value of the oxyethylene group content of the two or more polyoxyalkylene monoether alcohols.

[0096] The calculation method for the ethylene oxide group content of the polyoxyalkylene monoether alcohol is as follows:

[0097]

[0098] in:

[0099] ∑(b*EO%wt) is the sum of the weight of ethylene oxide groups of each polyoxyalkylene monoether alcohol

[0100] ∑b is the total weight of polyoxyalkylene monoether alcohol.

[0101] When the system comprises two or more polyoxyalkylene monoether alcohols, the system preferably comprises at least one polyoxyalkylene monoether alcohol meeting the following conditions: its number average molecular weight is preferably 250 g / mol-700 g / mol, further preferably 250 g / mol-600 g / mol, further preferably 250 g / mol-500 g / mol, and most preferably 250 g / mol-400 g / mol; its oxyethylene group content is preferably 75 wt%-100 wt%, further preferably 80 wt%-100 wt%, and most preferably 90 wt%-100 wt%, relative to the total weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0102] The amount of the component b) polyoxyalkylene monoether alcohol is preferably greater than 7% by weight and less than 11% by weight, most preferably 8% by weight to 11% by weight, relative to the total weight of the B component.

[0103] Component c) Catalyst

[0104] The component c) catalyst is preferably one or more of the following: sulfonic acid catalysts, phosphoric acid catalysts, tertiary amine catalysts, tertiary phosphine catalysts, tertiary hydroxyalkylamine catalysts and metal catalysts, and most preferably one or more of the following: metal catalysts and phosphoric acid catalysts.

[0105] The sulfonic acid catalyst is preferably one or more of the following: methanesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, perfluorobutanesulfonic acid, dodecylbenzenesulfonic acid, methyl and ethyl-toluenesulfonate.

[0106] The phosphoric acid catalyst is preferably one or more of the following: silylated acid, monoalkyl phosphate and dialkyl phosphate, further preferably one or more of the following: monobutyl phosphate, monotridecyl phosphate, dibutyl phosphate, dioctyl phosphate, trimethylsilyl methanesulfonate, trimethylsilyl trifluoromethanesulfonate, tris(trimethylsilyl)phosphate and diethyltrimethylsilyl phosphate, most preferably one or more of the following: monobutyl phosphate and dibutyl phosphate.

[0107] The tertiary amine catalyst is preferably one or more of the following: triethylamine, tributylamine, N,N-dimethylaniline, N-ethylpiperidine and N,N'-dimethylpiperazine.

[0108] The tertiary phosphine catalyst is preferably one or more of the following: triethylphosphine, tributylphosphine and dimethylphenylphosphine.

[0109] The tertiary hydroxyalkylamine catalyst is preferably those described in GB2221465 and / or GB2222161, most preferably one or more of the following: triethanolamine, N-methyldiethanolamine, dimethylethanolamine, a mixture of a tertiary bicyclic amine (e.g. DBU) and a low molecular weight simple aliphatic alcohol, N-isopropyldiethanolamine and 1-(2-hydroxyethyl)pyrrolidine.

[0110] The metal catalyst may be those described in DEA 3240613, preferably one or more of the following: manganese octoate, iron octoate, cobalt octoate, nickel octoate, copper octoate, zinc octoate, zirconium octoate, cerium octoate, lead octoate, manganese naphthenate, iron naphthenate, cobalt naphthenate, nickel naphthenate, copper naphthenate, zinc naphthenate, zirconium naphthenate, cerium naphthenate, lead naphthenate and mixtures of the above salts with acetates of lithium, sodium, potassium, calcium or barium. The metal catalyst may also be those described in DEA 3219608, preferably one or more of the following: sodium salts of linear or branched alkane carboxylic acids having up to 10 carbon atoms and potassium salts of linear or branched alkane carboxylic acids having up to 10 carbon atoms, wherein the carboxylic acids are preferably one or more of the following: propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid and undecanoic acid. The metal catalyst can also be a salt of an alkali metal and / or an alkaline earth metal described in EPA0100129, preferably one or more of the following: aliphatic, alicyclic or aromatic monocarboxylic acids and polycarboxylic acids with 2-20 carbon atoms with sodium benzoate or potassium benzoate. The metal catalyst can also be an alkali metal phenolate known in GB1391066A and GB1386399A, preferably one or more of the following: sodium phenolate and potassium phenolate. The metal catalyst can also be those known in GB809809, preferably one or more of the following: alkali metal oxides, alkaline earth metal oxides, alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal alkoxides, alkaline earth metal alkoxides, alkali metal phenolates, alkaline earth metal phenolates, alkali metal salts of olefinizable compounds, metal salts of weak aliphatic carboxylic acids, metal salts of alicyclic carboxylic acids, basic alkali metal compounds complexed with crown ethers, and basic alkali metal compounds complexed with polyether alcohols. The metal catalyst can also be the potassium pyrrolidone salt known in EPA0033581. The metal catalyst can also be the monocyclic or polycyclic complex of titanium, zirconium and / or hafnium known in EPA2883895, preferably one or more of the following: zirconium tetra-n-butyrate, zirconium tetra-2-ethylhexanoate and tetra-2-zirconium hexanoic acid ethyl ester. The metal catalyst can also be a tin compound of the type described in European Polymer Journal, 16, 1979, 147-148, preferably one or more of the following: dibutyltin dichloride, diphenyltin dichloride, triphenyltin alkane, tributyltin acetate, tributyltin oxide, tin octoate, dibutyl (dimethoxy) stannane and imidazole tributyltin.

[0111] The metal salt of the weak aliphatic carboxylic acid and the metal salt of the alicyclic carboxylic acid are each independently preferably one or more of the following: sodium methanol, sodium acetate, potassium acetate, sodium acetoacetate, lead 2-ethylhexanoate and lead naphthenate.

[0112] The basic alkali metal compound complexed with the crown ether and the basic alkali metal compound complexed with the polyether alcohol are each independently preferably one or more of the following: sodium or potassium carboxylate salts of the complexes, which are known from EPA0056158 and EPA0056159.

[0113] When the system comprises a metal catalyst, a terminator needs to be used after the system reaction ends. In addition, the above-mentioned phosphoric acid catalyst, sulfonic acid catalyst and their derivatives can be used as terminators here. In addition to these two acid catalysts, other mineral acids such as hydrochloric acid, phosphorous acid, acyl chlorides such as acetyl chloride, benzoyl chloride or isophthaloyl dichloride can also be used as terminators.

[0114] The amount of the catalyst is preferably 0-0.02% by weight, relative to the total weight of the system.

[0115] Solvents

[0116] The system may further comprise a solvent which is inert towards isocyanate groups.

[0117] The solvent may be those known, preferably one or more of the following: ethyl acetate, butyl acetate, ethylene glycol monomethyl, ethyl ether acetate, 1-acetic acid 2-methoxypropyl-2-acetate, 2-butanone, 4-methyl-2-pentanone, cyclohexanone, toluene, propylene glycol diacetate, diethylene glycol dimethyl ether, diethylene glycol diacetate, butyl ether acetate, N-methylpyrrolidone and N-methylcaprolactam. The amount of the solvent is preferably 0-10% by weight, relative to the total weight of the system.

[0118] Method for preparing polyether-modified polyisocyanate

[0119] Preferably, the component b) polyoxyalkylene monoether alcohol is bonded to the component a) polyisocyanate via urethane groups.

[0120] In the system, a possible excess of component a) a polyisocyanate having an isocyanate group functionality of 2 to 4.5 is present in the polyether-modified polyisocyanate.

[0121] When used, the polyether-modified polyisocyanate may be mixed with an isocyanate different from the polyether-modified polyisocyanate of the present invention, for example, may be mixed with an unmodified isocyanate.

[0122] an isocyanate different from the polyether-modified polyisocyanate

[0123] The B component may further comprise an isocyanate different from the polyether-modified polyisocyanate.

[0124] The isocyanate different from the polyether-modified polyisocyanate is preferably an unmodified isocyanate.

[0125] The isocyanate different from the polyether-modified polyisocyanate is preferably one or more of the following: aliphatic isocyanate trimer, aliphatic isocyanate uretdione, aliphatic allophanate and aliphatic isocyanate biuret.

[0126] The amount of the isocyanate different from the polyether-modified polyisocyanate is preferably 0% to 30% by weight, further preferably 0% to 20% by weight, more preferably 0% to 10% by weight, based on the total weight of the B component.

[0127] When the B component contains an isocyanate different from the polyether-modified polyisocyanate, the average isocyanate functionality of the B component is calculated as follows:

[0128] f=NCO%*4200 / Mn

[0129] f: Average isocyanate functionality of component B

[0130] Mn: number average molecular weight of isocyanate other than the polyether-modified polyisocyanate

[0131] Additives in two-component coating compositions

[0132] The two-component coating composition preferably further comprises an additive and / or auxiliary agent, wherein the additive or auxiliary agent is preferably one or more of the following: a wetting agent, a dispersant, a matting agent, a defoaming agent, a film former, a thickener, an elastic agent, a pigment, a leveling agent, and other additives or auxiliary agents known to those skilled in the art that can be added to the two-component coating composition.

[0133] The film former is preferably one or more of the following: dipropylene glycol methyl ether (DPM), dipropylene glycol n-butyl ether (DPnB), ethylene glycol butyl ether (BG) and propylene glycol butyl ether (PnB).

[0134] The amount of the film former is preferably 0 wt % to 10 wt %, further preferably 0 wt % to 5 wt %, most preferably 0 wt % to 3 wt %, relative to the total weight of the A component.

[0135] The amount of the additive or auxiliary agent can be any amount that is well known to those skilled in the art.

[0136] The additives or auxiliary agents may be optionally contained in the A component and / or the B component, or may be stored separately and added when used to prepare the two-component coating composition.

[0137] use

[0138] Substrate

[0139] The coating is preferably used to protect floors, walls, furniture surfaces or surfaces of metal containers or other surfaces that need protection.

[0140] The substrate may be pre-treated, and the pre-treatment is preferably grinding or coating.

[0141] The substrate may be artificial stone, wood, artificial wood, marble, terrazzo, ceramic, linoleum, metal, mineral material, plastic, rubber, concrete, composite sheet, board, paper, leather or glass.

[0142] Coating method

[0143] The curing and drying temperature is preferably 25±2° C., and the humidity is preferably 60±10%.

[0144] The construction can be a method well known to those skilled in the art, such as scraping, dipping, brushing, rolling, spraying or showering.

[0145] Coating products

[0146] The coated product is preferably a building wall, a furniture surface, a floor or a metal surface.

[0147] The application is preferably carried out using roller coating, which is known to those skilled in the art.

[0148] The coating may be single-layer or multi-layer.

[0149] The two-component coating composition of the present invention has the advantage of being easy to clean and can establish a barrier between the surface of the protected substrate and the contamination, making the contamination easy to remove.

[0150] The two-component coating composition of the invention has a matte effect and can be applied to various occasions.

[0151] Example

[0152] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention belongs. When the definition of a term in this specification conflicts with the meaning commonly understood by those skilled in the art to which the invention belongs, the definition described in this article shall prevail.

[0153] Unless otherwise indicated, all numerical values ​​expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.

[0154] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.

[0155] As used herein, "and / or" means one or all of the mentioned elements.

[0156] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.

[0157] All percentages in the present invention are by weight, unless otherwise specified.

[0158] The analytical measurements of the present invention were all conducted at 23±2°C and 50±5% humidity, unless otherwise stated.

[0159] The isocyanate group (NCO) content is determined in accordance with DIN-EN ISO 11909:2007-05, the data determined include the free and potentially free NCO content.

[0160] The number average molecular weight of isocyanate is determined according to DIN 55672-1:2016-03 by gel permeation chromatography with tetrahydrofuran as mobile phase and compared with polystyrene standards at 23°C.

[0161] The number average molecular weight of the polyoxyalkylene monoether alcohol is determined according to GBT 21863-2008 by gel permeation chromatography with tetrahydrofuran as the mobile phase and against a polyethylene glycol standard at 23°C.

[0162] The solid content of the aqueous polyacrylic acid dispersion is measured according to DIN EN ISO 3251:2008-06 at a drying temperature of 120° C., a drying time of 1 hour, a test plate diameter of 75 mm and a test amount of 1±0.02 g, and the result is expressed in weight %.

[0163] Viscosity according to DIN EN ISO 3219:1994-10 at 23°C, shear rate 10s -1 Under Assay, select the MV-DIN rotor.

[0164] The hydroxyl group content is tested according to DIN EN ISO 4629-2.

[0165] The color value is determined according to DIN-EN1557:1997-03.

[0166] Easy-to-clean test: Use a water-based whiteboard pen (red, blue, black) commonly used for blackboard writing to draw a mark of at least 10 cm in the center of the coating, then wipe the mark back and forth 5 times with a dry napkin, with a wiping pressure of about 0.5 kg, inspect the coating with the naked eye, and score the residual degree of the mark, with a score of 2-5, from poor to good for easy-to-clean performance. A score of 4 or above in the easy-to-clean test is qualified. 5 points means that there is no mark left on the coating surface at all, 4 points means that there is a very slight mark left on the coating surface, 3 points means that there is a clear mark left on the coating surface, and 2 points means that there is a lot of mark left and it is similar to before wiping.

[0167] Film appearance test: The coating appearance is judged and scored by visual observation, with a score of 2-5, from poor to good. The film appearance test score of 4 points and above is qualified. 5 points means that the coating surface is smooth and has no obvious graininess, 4 points means that the coating surface is smooth but has a slight graininess, 3 points means that the coating surface is smooth and has a clear graininess, and 2 points means that the coating surface is rough and has a clear graininess.

[0168] The gloss is measured at 60°C according to GB / T 9754-1988, and a gloss less than 60 is acceptable.

[0169] Pendulum hardness: The coating is prepared on glass using a film scraper (the film thickness is set to 120μm), and the hardness of the coating is measured using a BYK pendulum hardness tester. The pendulum hardness (7d) refers to the pendulum hardness of the coating after seven days of storage. The greater the pendulum hardness, the higher the hardness of the coating formed by the coating. A pendulum hardness greater than 80 is considered acceptable.

[0170] Materials and reagents

[0171] Polyisocyanate 1: A four-necked flask equipped with a stirrer, a thermometer, a reflux cooling tube, a nitrogen blowing tube and a dropping funnel was set to a nitrogen atmosphere, 850 g of Desmodur H was added, and the mixture was heated to 65° C. under stirring, followed by the addition of 5.5 g of benzyltrimethylammonium hydroxide (a solution diluted to 5% by weight with isobutyl alcohol). When the NCO content of the reaction solution reached 45.6% by weight, 1.1 g of di-n-butyl phosphate was added to stop the reaction. Unreacted monomers were removed using a thin film evaporator at 140° C. and 0.05 mbar to obtain a hexamethylene diisocyanate trimer having a nonvolatile component of 100% by weight, an NCO functionality of 3.2, a viscosity of 1200 mPa·s (23° C.), an NCO content of 23.0% by weight, and a hexamethylene diisocyanate (HDI) monomer content of 0.25% by weight.

[0172] Polyisocyanate 2: The method for preparing hexamethylene diisocyanate trimer 1 was used, and dibutyl phosphate was added to terminate the reaction when the NCO content of the reaction solution reached 38 wt%. Unreacted monomers were removed using a thin film evaporator at 140° C. and 0.05 mbar to obtain a hexamethylene diisocyanate trimer having a nonvolatile component of 100 wt%, an NCO functionality of 3.5, a viscosity of 3000 mPa·s (23° C.), an NCO content of 21.7 wt%, and a monomer HDI content of 0.25 wt%.

[0173] Polyisocyanate 3: 2 g of N,N-diethylurea as stabilizer, 10 g of 1,3-butanediol as cocatalyst and 3 g of tri-n-butylphosphine as catalyst were added successively to 1000 g (5.95 mol) of Desmodur H at room temperature under dry nitrogen, and the mixture was then heated to 60° C. After a reaction time of 4 hours, the NCO content of the reaction mixture was 40.4%, corresponding to a degree of oligomerization of 18.0%. The reaction was terminated by adding 2.8 g (0.015 mol) of methyl p-toluenesulfonate and heated to 80° C. for 1 hour. After thin-layer distillation at a temperature of 130° C. and a pressure of 0.15 mbar, hexamethylene diisocyanate uretdione was obtained, which had a nonvolatile content of 100% by weight, an NCO content of 21.4%, an NCO functionality of 2.5, a monomeric HDI content of 0.07% by weight and a viscosity of 185 mPa·s (23° C.).

[0174] Desmodur H: hexamethylene diisocyanate, purchased from Covestro (China) Co., Ltd.

[0175] N,N-Diethylurea: purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0176] 1,3-Butanediol: purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0177] Benzyltrimethylammonium hydroxide: purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0178] Tri-n-butylphosphine: purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0179] Isobutanol: purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0180] MPEG 200: polyoxyalkylene monoether alcohol, oxyethylene groups account for 100% by weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol, number average molecular weight 200 g / mol, OH value 280.5 mgKOH / g.

[0181] MPEG 350: polyoxyalkylene monoether alcohol, oxyethylene groups account for 100% by weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol, number average molecular weight 350 g / mol, OH value 160.3 mgKOH / g.

[0182] MPEG 500: polyoxyalkylene monoether alcohol, oxyethylene groups account for 100% by weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol, number average molecular weight 500 g / mol, OH value 112.2 mgKOH / g.

[0183] MPEG 750: polyoxyalkylene monoether alcohol, oxyethylene groups account for 100% by weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol, number average molecular weight 750 g / mol, OH value 74.8 mgKOH / g.

[0184] T01-A: polyoxyalkylene monoether alcohol, propylene oxide groups account for 100% by weight of the alkylene oxide groups of the polyoxyalkylene monoether alcohol, number average molecular weight 800 g / mol, OH value 70.1 mgKOH / g, starting components are propylene oxide and n-butanol.

[0185] Dibutyl phosphate: can be purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0186] Airex 901W: defoaming agent, available from Evonik Specialty Chemicals (Shanghai) Co., Ltd.

[0187] BYK022: defoaming agent, available from BYK Additives (Shanghai) Co., Ltd.

[0188] BYK348: Wetting agent, available from BYK Additives (Shanghai) Co., Ltd.

[0189] RM-8W: thickener, available from Dow Chemical (Shanghai) Co., Ltd.

[0190] DPM: dipropylene glycol methyl ether, available from Dow Chemical (Shanghai) Co., Ltd.

[0191] DPnB: dipropylene glycol n-butyl ether, available from Dow Chemical (Shanghai) Co., Ltd.

[0192] Bayhydrol A 2546: a hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 41% by weight, an OH content (to solids) of about 4.8% by weight, and a weight-average molecular weight of about 270,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0193] Bayhydrol A 242: a hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 42% by weight, an OH content (to solids) of about 4.0% by weight, and a weight-average molecular weight of about 36,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0194] Bayhydrol A 2457: a hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 40% by weight, an OH content (to solids) of about 2.7% by weight, and a weight-average molecular weight of about 320,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0195] Bayhydrol A 2846: a hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 40% by weight, an OH content (to solids) of about 1.5% by weight, and a weight-average molecular weight of about 140,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0196] XK-101: A hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 40% by weight, an OH content (to solids) of about 2.5% by weight, and a weight-average molecular weight of less than 50,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0197] XK-102: A hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 40% by weight, an OH content (to solids) of about 1.5% by weight, and a weight-average molecular weight of about 70,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0198] XK-103: A hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 45% by weight, an OH content (to solids) of about 3.2% by weight, and a weight-average molecular weight of about 460,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0199] XK-110: A hydroxyl-containing aqueous polyacrylic acid dispersion, with a non-volatile content of about 46.5% by weight, an OH content (to solids) of about 2.5% by weight, and a weight-average molecular weight of about 90,000, which can be purchased from Covestro Shanghai (Investment) Co., Ltd.

[0200] Polyether modified polyisocyanate 1

[0201] 270 g (1.4786 eq) of polyisocyanate 1 and 0.018 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 25.0 g (0.0714 eq) of MPEG 350 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 20.09%, and the heating was stopped to obtain a polyether-modified polyisocyanate 1, which was a colorless transparent solution and met the following characteristic data:

[0202] Solid content: 100% by weight

[0203] NCO content, relative to the total weight of polyether-modified polyisocyanate 1: 20.09 wt %

[0204] Viscosity (23°C): 1328 mPa·s

[0205] Hazen: 13

[0206] Isocyanate functionality: 3.05

[0207] Number average molecular weight (g / mol): 827 g / mol

[0208] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 8.5 wt % relative to the total weight of the polyether-modified polyisocyanate 1. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0209] The content of isophorone diisocyanate trimer was 0% by weight based on the total weight of the polyether-modified polyisocyanate 1.

[0210] Polyether modified polyisocyanate 2

[0211] 270 g (1.4786 eq) of polyisocyanate 1 and 0.021 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30.0 g (0.0857 eq) of MPEG 350 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 19.7%, and the heating was stopped to obtain a polyether-modified polyisocyanate 2, which was a colorless transparent solution and met the following property data:

[0212] Solid content: 100% by weight

[0213] NCO content relative to the total weight of polyether-modified polyisocyanate 2: 19.72 wt%

[0214] Viscosity (23°C): 1287 mPa·s

[0215] Hazen: 12

[0216] Isocyanate functionality: 3.01

[0217] Number average molecular weight (g / mol): 829 g / mol

[0218] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 2. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0219] The content of the isophorone diisocyanate trimer relative to the total weight of the polyether-modified polyisocyanate 2 is 0% by weight.

[0220] Polyether modified polyisocyanate 3

[0221] 270 g (1.4786 eq) of polyisocyanate 1 and 0.039 g (0.0002 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30.0 g (0.0600 eq) of MPEG 500 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 19.96%, and the heating was stopped to obtain a polyether-modified polyisocyanate 3, which was a colorless transparent solution and met the following characteristic data:

[0222] Solid content: 100% by weight

[0223] NCO content relative to the total weight of polyether-modified polyisocyanate 3: 19.96 wt%

[0224] Viscosity (23°C): 1548 mPa·s

[0225] Hazen: 9

[0226] Isocyanate functionality: 3.07

[0227] Number average molecular weight (g / mol): 847 g / mol

[0228] The number average molecular weight of the polyoxyalkylene monoether alcohol is 500 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 3. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0229] The content of the isophorone diisocyanate trimer is 0% by weight relative to the total weight of the polyether-modified polyisocyanate 3.

[0230] Polyether modified polyisocyanate 4

[0231] 189 g (1.0499 eq) of polyisocyanate 1, 81 g (0.4175 eq) of polyisocyanate 3 and 0.024 g (0.0001 mol) of dibutyl phosphate were added into a 500 ml flask with a dropping funnel and a nitrogen inlet, and stirred to obtain a solution. The solution was heated to 100° C., and 30.0 g (0.0857 eq) of MPEG 350 was added dropwise into the flask over 45 minutes to react until the isocyanate group (NCO) content reached 19.40%. The heating was stopped to obtain a polyether-modified polyisocyanate 4, which was a colorless transparent solution and met the following characteristic data:

[0232] Solid content: 100% by weight

[0233] NCO content relative to the total weight of polyether-modified polyisocyanate 4: 19.40 wt%

[0234] Viscosity (23°C): 709 mPa·s

[0235] Hazen: 21

[0236] Isocyanate functionality: 2.79

[0237] Number average molecular weight (g / mol): 771 g / mol

[0238] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 4. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0239] The content of the isophorone diisocyanate trimer was 0% by weight relative to the total weight of the polyether-modified polyisocyanate 4.

[0240] Polyether modified polyisocyanate 5

[0241] 135 g (0.7496 eq) of polyisocyanate 1, 135 g (0.6959 eq) of polyisocyanate 3 and 0.024 g (0.0001 mol) of dibutyl phosphate were added into a 500 ml flask with a dropping funnel and a nitrogen inlet, and stirred to obtain a solution. The solution was heated to 100° C. 30.0 g (0.0857 eq) of MPEG 350 was added dropwise into the flask over 45 minutes to react until the isocyanate group (NCO) content reached 18.95%. Heating was stopped to obtain a polyether-modified polyisocyanate 5, which was a colorless transparent solution and met the following property data:

[0242] Solid content: 100% by weight

[0243] NCO content relative to the total weight of polyether-modified polyisocyanate 5: 18.95 wt%

[0244] Viscosity (23°C): 519 mPa·s

[0245] Hazen: 17

[0246] Isocyanate functionality: 2.65

[0247] Number average molecular weight (g / mol): 758 g / mol

[0248] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 5. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0249] The content of the isophorone diisocyanate trimer was 0% by weight based on the total weight of the polyether-modified polyisocyanate 5.

[0250] Polyether modified polyisocyanate 6

[0251] 270 g (1.4014 eq) of polyisocyanate 2 and 0.021 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30.0 g (0.0857 eq) of MPEG 350 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 18.39%, and the heating was stopped to obtain a comparative polyether-modified polyisocyanate 6, which was a colorless transparent solution and met the following characteristic data:

[0252] Solid content: 100% by weight

[0253] NCO content relative to the total weight of polyether-modified polyisocyanate 6: 18.39 wt%

[0254] Viscosity (23°C): 3136 mPa·s

[0255] Hazen: 12

[0256] Isocyanate functionality: 3.29

[0257] Number average molecular weight (g / mol): 958 g / mol

[0258] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 6. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0259] The content of the isophorone diisocyanate trimer is 0% by weight based on the total weight of the polyether-modified polyisocyanate 6.

[0260] Polyether modified polyisocyanate 7

[0261] 270 g (1.4786 eq) of polyisocyanate 1 and 0.021 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 27.2 g (0.0777 eq) of MPEG 350 and 2.83 g (0.0035 eq) of T01A were added dropwise to the flask in sequence over 45 minutes to react until the isocyanate group (NCO) content reached 19.66%, and the heating was stopped to obtain a polyether-modified polyisocyanate 7, which was a colorless transparent solution and met the following characteristic data:

[0262] Solid content: 100% by weight

[0263] NCO content relative to the total weight of polyether-modified polyisocyanate 7: 19.96 wt%

[0264] Viscosity (23°C): 1325 mPa·s

[0265] Hazen: 6

[0266] Isocyanate functionality: 3.02

[0267] Number average molecular weight (g / mol): 815 g / mol

[0268] The number average molecular weight of the polyoxyalkylene monoether alcohol is 370 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the polyether-modified polyisocyanate 7. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 90.5 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0269] The content of the isophorone diisocyanate trimer was 0% by weight based on the total weight of the polyether-modified polyisocyanate 7.

[0270] Comparison of polyether-modified polyisocyanate 1

[0271] 270 g (1.4786 eq) of polyisocyanate 1 and 0.013 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 18.8 g (0.0537 eq) of MPEG 350 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 20.99%, and the heating was stopped to obtain a comparative polyether-modified polyisocyanate 1, which was a colorless transparent solution and met the following characteristic data:

[0272] Solid content: 100% by weight

[0273] NCO content, relative to the total weight of comparative polyether-modified polyisocyanate 1: 20.99 wt.%

[0274] Viscosity (23°C): 1236 mPa·s

[0275] Hazen: 4

[0276] Isocyanate functionality: 3.08

[0277] Number average molecular weight (g / mol): 804 g / mol

[0278] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 6.5 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 1. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0279] The content of isophorone diisocyanate trimer was 0% by weight, relative to the total weight of comparative polyether-modified polyisocyanate 1.

[0280] Comparison of polyether-modified polyisocyanate 2

[0281] 220 g (1.2079 eq) of polyisocyanate 1 and 0.021 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30 g (0.0857 eq) of MEPG 350 was added dropwise to the flask within 45 minutes to react until the isocyanate group (NCO) content reached 18.80%, and the heating was stopped to obtain a comparative polyether-modified polyisocyanate 2, which was a colorless transparent solution and met the following characteristic data:

[0282] Solid content: 100% by weight

[0283] Relative to the total weight of comparative polyether-modified polyisocyanate 2, NCO content: 18.80 wt% Viscosity (23° C.): 1280 mPa·s

[0284] Hazen: 10

[0285] Isocyanate functionality: 2.43

[0286] Number average molecular weight (g / mol): 857 g / mol

[0287] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 12 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 2. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0288] The content of isophorone diisocyanate trimer was 0% by weight relative to the total weight of the comparative polyether-modified polyisocyanate 2.

[0289] Comparison of polyether-modified polyisocyanate 3

[0290] 220 g (1.3054 eq) of polyisocyanate 1 and 0.1 g (0.0005 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 26 g (0.1308 eq) of MPEG 200 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 18.95%, and the heating was stopped to obtain a comparative polyether-modified polyisocyanate 3, which was a colorless transparent solution and met the following characteristic data:

[0291] Solid content: 100% by weight

[0292] Relative to the total weight of comparative polyether-modified polyisocyanate 3, NCO content: 18.95 wt % Viscosity (23° C.): 1613 mPa·s

[0293] Hazen: 9

[0294] Isocyanate functionality: 2.88

[0295] Number average molecular weight (g / mol): 812 g / mol

[0296] The number average molecular weight of the polyoxyalkylene monoether alcohol is 200 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 3. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0297] The content of isophorone diisocyanate trimer was 0% by weight relative to the total weight of comparative polyether-modified polyisocyanate 3.

[0298] Comparison of polyether-modified polyisocyanate 4

[0299] 270 g (1.4786 eq) of polyisocyanate 1 and 0.051 g (0.0002 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30 g (0.04 eq) of MPEG 750 was added dropwise to the flask over 45 minutes to react until the isocyanate group (NCO) content reached 20.30%, and heating was stopped to obtain a comparative polyether-modified polyisocyanate 4, which was a colorless transparent solution and met the following characteristic data:

[0300] Solid content: 100% by weight

[0301] Relative to the total weight of comparative polyether-modified polyisocyanate 4, NCO content: 20.30 wt% Viscosity (23° C.): 1134 mPa·s

[0302] Hazen: 3

[0303] Isocyanate functionality: 3.11

[0304] Number average molecular weight (g / mol): 805 g / mol

[0305] The number average molecular weight of the polyoxyalkylene monoether alcohol is 750 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 4. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0306] The content of isophorone diisocyanate trimer was 0% by weight relative to the total weight of comparative polyether-modified polyisocyanate 4.

[0307] Comparison of polyether-modified polyisocyanate 5

[0308] 81 g (0.4497 eq) of polyisocyanate 1, 189 g (0.9743 eq) of polyisocyanate 3 and 0.024 g (0.0001 mol) of dibutyl phosphate were added into a 500 ml flask with a dropping funnel and a nitrogen inlet, stirred to obtain a solution, the solution was heated to 100° C., 30.0 g (0.0857 eq) of MPEG 350 was added dropwise into the flask over 45 minutes to react until the isocyanate group (NCO) content reached 18.72%, and heating was stopped to obtain a comparative polyether-modified polyisocyanate 5, which was a colorless transparent solution and met the following characteristic data: Solid content: 100 wt %

[0309] Relative to the total weight of comparative polyether-modified polyisocyanate 5, NCO content: 18.72 wt % Viscosity (23° C.): 396 mPa·s

[0310] Hazen: 28

[0311] Isocyanate functionality: 2.53

[0312] Number average molecular weight (g / mol): 723 g / mol

[0313] The number average molecular weight of the polyoxyalkylene monoether alcohol is 350 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 5. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 100 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0314] The content of isophorone diisocyanate trimer was 0% by weight relative to the total weight of the comparative polyether-modified polyisocyanate 5.

[0315] Comparison of polyether-modified polyisocyanate 6

[0316] 270 g (1.4786 eq) of polyisocyanate 1 and 0.021 g (0.0001 mol) of dibutyl phosphate were added to a 500 ml flask with a dropping funnel and a nitrogen inlet, and stirred to obtain a solution. The solution was heated to 100° C. 22.8 g (0.0652 eq) of MPEG 350 and 7.82 g (0.0098 eq) of T01A were added dropwise to the flask in sequence over 45 minutes to react until the isocyanate group (NCO) content reached 19.84%, and heating was stopped to obtain a comparative polyether-modified polyisocyanate 6, which was a colorless transparent solution and met the following characteristic data:

[0317] Solid content: 100% by weight

[0318] Relative to the total weight of comparative polyether-modified polyisocyanate 6, NCO content: 19.84 wt % Viscosity (23° C.): 1343 mPa·s

[0319] Hazen: 7

[0320] Isocyanate functionality: 3.04

[0321] Number average molecular weight (g / mol): 758 g / mol

[0322] The number average molecular weight of the polyoxyalkylene monoether alcohol is 409 g / mol. The amount of the polyoxyalkylene monoether structure is 10 wt % relative to the total weight of the comparative polyether-modified polyisocyanate 6. The oxyethylene groups of the polyoxyalkylene monoether alcohol account for 74.5 wt % of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

[0323] The content of isophorone diisocyanate trimer was 0% by weight relative to the total weight of comparative polyether-modified polyisocyanate 6.

[0324] Method for preparing two-component coating composition

[0325] The components of component A and component B and the content of each component are shown in Table 1 and Table 2. The substances of component A are mixed at room temperature to obtain component A. Component A and component B are mixed at room temperature to obtain a two-component coating composition.

[0326] Coating preparation method

[0327] The coating composition was applied to the surface of the substrate using a 120 μm scraper, and cured and dried at 23° C. and 50% RH to obtain a coating.

[0328] Among them, transparent glass was selected as the substrate, and the coating was used to measure the pendulum hardness and easy-to-clean performance after curing; black PC / ABS plastic plate was selected as the substrate, and the coating was used to measure the film appearance and gloss after curing.

[0329] Examples 1-26 and Comparative Examples 1-13

[0330] Table 1 shows the components of the compositions of Examples 1-7 and Comparative Examples 1-6, and the performance test results of the compositions and their coatings. Table 2 shows the components of the compositions of Examples 8-11 and Comparative Examples 7-9, and the performance test results of the compositions and their coatings.

[0331] Table 1 Components and test results of the compositions of Examples 1-7 and Comparative Examples 1-6

[0332]

[0333]

[0334]

[0335] Note: * indicates that the composition cannot be dispersed and performance testing cannot be performed

[0336] **The surface is rough and uneven, so accurate data cannot be obtained

[0337] The two-component coating compositions of Examples 1-7 have good easy-to-clean properties, good film appearance and pendulum hardness, and matte gloss.

[0338] The B component of the two-component coating composition of Comparative Example 1 comprises comparative polyether-modified polyisocyanate 1, and the coating formed therefrom is not easy to clean.

[0339] The B component of the two-component coating composition of Comparative Example 2 contains comparative polyether-modified polyisocyanate 2, and the coating formed therefrom has high gloss but is not matte.

[0340] The B component of the two-component coating composition of Comparative Example 3 comprises comparative polyether-modified polyisocyanate 3, and the coating formed therefrom is unqualified in terms of easy cleaning, film appearance, pendulum hardness and matte properties.

[0341] The B component of the two-component coating composition of Comparative Example 4 contained comparative polyether-modified polyisocyanate 4. The composition could not be dispersed and the performance test could not be performed.

[0342] The B component of the two-component coating composition of Comparative Example 5 contains comparative polyether-modified polyisocyanate 5, and the coating formed therefrom is not easy to clean.

[0343] The B component of the two-component coating composition of Comparative Example 6 comprises comparative polyether-modified polyisocyanate 6, and the coating formed therefrom is not easy to clean.

[0344] Table 2 Components and test results of the compositions of Examples 8-11 and Comparative Examples 7-9

[0345]

[0346] The two-component coating compositions of Examples 8-11 have good easy-to-clean properties, good film appearance and pendulum hardness, and matte gloss.

[0347] The A component of the two-component coating composition of Comparative Example 7 comprises XK-102, the coating formed is difficult to clean and the film appearance is poor.

[0348] The A component of the two-component coating composition of Comparative Example 8 contained Bayhydrol A 2846, and the coating formed therefrom was not easy to clean.

[0349] The A component of the two-component coating composition of Comparative Example 9 comprises XK-103, the coating formed is difficult to clean and the film appearance is poor.

[0350] It is easy for a person skilled in the art to know that the present invention is not limited to the above-mentioned specific details, and the present invention can be implemented in other specific forms without departing from the spirit or main characteristics of the present invention. Therefore, the embodiments described should be regarded as illustrative rather than restrictive from any point of view, so that the scope of the present invention is indicated by the claims rather than the above description; and therefore any changes, as long as they fall within the meaning and scope of the equivalents of the claims, should be regarded as belonging to the present invention.

Claims

1. A two-component coating composition, comprising component A and component B, wherein component A comprises a hydroxyl-containing aqueous polyacrylic acid dispersion, and component B comprises a polyether-modified polyisocyanate, wherein the molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.2:1-2:1; the hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is greater than 2% by weight, and the weight average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is not higher than 450,000, based on the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion; and the polyether-modified polyisocyanate is obtained by reacting a system comprising the following components: a) a polyisocyanate having an isocyanate group functionality of 2 to 4.5, comprising at least 30% by weight of hexamethylene diisocyanate trimer, pentamethylene diisocyanate trimer or a combination thereof; b) a polyoxyalkylene monoether alcohol; and c) optionally a catalyst; The number average molecular weight of the polyoxyalkylene monoether alcohol is 250 g / mol-700 g / mol, and the content of oxyethylene groups is 75 wt %-100 wt %, relative to the total weight of the oxyethylene groups of the polyoxyalkylene monoether alcohol; the polyether-modified polyisocyanate has the following characteristics: i) an average isocyanate functionality of 1.8 to 4.1; ii) an isocyanate group content of 8 wt% to 21 wt% relative to the total weight of the polyisocyanate; and iii) a number average molecular weight of 500 g / mol to 1200 g / mol; The amount of the polyoxyalkylene monoether structure of the B component is greater than 6.5 wt % and less than 12 wt % relative to the total weight of the B component.

2. The two-component coating composition according to claim 1, characterized in that The molar ratio of isocyanate groups to hydroxyl groups of the composition is 1.3:1-1.7:

1.

3. The two-component coating composition according to claim 1 or 2, characterized in that: The hydroxyl content of the hydroxyl-containing aqueous polyacrylic acid dispersion is greater than 2 wt % and not greater than 5 wt %, most preferably 2.5 wt % to 5 wt %, relative to the total weight of the solid content of the hydroxyl-containing aqueous polyacrylic acid dispersion.

4. The two-component coating composition according to any one of claims 1 to 3, characterized in that: The weight average molecular weight of the hydroxyl-containing aqueous polyacrylic acid dispersion is 30,000-450,000, and most preferably 30,000-350,000. The weight average molecular weight is determined by gel permeation chromatography using DMF as the mobile phase and comparing with a polystyrene standard sample according to GB / T 21863-2008.

5. The two-component coating composition according to any one of claims 1 to 4, characterized in that: The amount of the polyoxyalkylene monoether structure of the B component is 7 wt% to 11 wt%, most preferably 8 wt% to 11 wt%, relative to the total weight of the B component.

6. The two-component coating composition according to any one of claims 1 to 5, characterized in that: The polyether-modified polyisocyanate further has one of the following characteristics: iv) the amount of the polyoxyalkylene monoether structure is greater than 6.5 wt% and less than 12 wt%, preferably 7 wt% to 11 wt%, most preferably 8 wt% to 11 wt%, relative to the total weight of the polyisocyanate; and v) the content of isophorone diisocyanate trimer is not more than 0.5% by weight, based on the total weight of the polyisocyanate.

7. The two-component coating composition according to any one of claims 1 to 6, characterized in that: The B component further comprises an isocyanate different from the polyether-modified polyisocyanate, and most preferably comprises an unmodified isocyanate.

8. The two-component coating composition according to any one of claims 1 to 7, characterized in that: The component a) polyisocyanate having an isocyanate group functionality of 2-4.5 further comprises another isocyanate, and the other isocyanate is one or more of the following: aliphatic isocyanate uretdione and aliphatic isocyanate biuret.

9. The two-component coating composition according to claim 8, characterized in that: The other isocyanate is one or more of the following: hexamethylene diisocyanate uretdione, hexamethylene diisocyanate biuret and pentamethylene diisocyanate uretdione.

10. The two-component coating composition according to any one of claims 1 to 9, characterized in that: The polyoxyalkylene monoether alcohol of component b) has an oxyethylene group content of 80% to 100% by weight, most preferably 90% to 100% by weight, relative to the total weight of the oxyalkylene groups of the polyoxyalkylene monoether alcohol.

11. The two-component coating composition according to any one of claims 1 to 10, characterized in that: The amount of the component b) polyoxyalkylene monoether alcohol is greater than 7% by weight and less than 11% by weight, most preferably 8% by weight to 11% by weight, relative to the total weight of the B component.

12. The two-component coating composition according to any one of claims 1 to 11, characterized in that: The number average molecular weight of the component b) polyoxyalkylene monoether alcohol is 250 g / mol to 600 g / mol, preferably 250 g / mol to 500 g / mol, most preferably 250 g / mol to 400 g / mol.

13. Use of the two-component coating composition according to any one of claims 1 to 12 for protecting a substrate surface or a substrate surface coating.

14. A coating method, comprising the following steps: applying the two-component coating composition according to any one of claims 1 to 12 to a substrate surface, followed by curing and drying.

15. A coated product comprising a substrate and a coating formed by applying the two-component coating composition according to any one of claims 1 to 12 to the substrate, curing and drying, wherein the coated product is preferably selected from building walls, furniture surfaces, floors or metal surfaces.