Degradable polymers for coatings, films and adhesives
By introducing copolymers of organic sulfur monomers with cyclic disulfide groups into the polymer, acid-functional monomers or vinyl monomers, it is solved that polymers in the prior art are difficult to achieve high molecular weight and tunable degradability. Problem, achieving high molecular weight and tunable degradability of polymers while maintaining or changing the performance properties of commercial materials, promoting sustainability.
Patent Information
- Application Number
- CN202380028077.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2023-01-25
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to prepare polymers with high molecular weight and tunable degradability, and their performance properties are difficult to match with commercial materials, especially in the fields of packaging materials, coatings, adhesives and films.
Using copolymers of organic sulfur monomers containing cyclic disulfide groups, acid functional monomers, polar monomers or vinyl monomers, the polymers are easily decomposed through chemical or biodegradable mechanisms to form high molecular weight and Degradable polymers that adjust degradability.
The high molecular weight and tunable degradability of polymers while maintaining or changing the performance properties of commercial materials, providing solutions to reduce waste plastics and improve sustainability.
Smart Images

Figure CN118974143A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to degradable polymers for use in coatings, films, adhesives, etc. In particular, the present disclosure relates to a new class of degradable polymers that share the performance attributes of current commercial materials with the added benefits of being configurable with high molecular weight and tunable degradation. Background Art
[0002] There are many polymer-based products for which degradability is desirable. For example, films and laminates used in packaging materials, coatings, adhesives, and as seed coverings are intended to remain intact only for short-term use. Other polymer-based products for which degradability is desired are molded articles.
[0003] Several approaches to improve the environmental degradability of polymers have been proposed and attempted. However, there remains a need to prepare degradable polymers with high molecular weight that share the performance attributes of current commercial materials. Summary of the invention
[0004] The present disclosure provides a degradable polymer, which is a copolymer of up to 50 mol% of an organosulfur monomer containing a cyclic disulfide group and at least 50 mol% of at least one organic monomer selected from the group consisting of an acid functional monomer, a base functional monomer, a polar monomer, a vinyl monomer, or a combination thereof. The use of the organosulfur monomer as a comonomer introduces a cleavable disulfide bond into the main backbone of the polymer, which makes the polymer susceptible to degradation by chemical or biological mechanisms. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] The drawings described below are for illustration purposes only. The drawings are not intended to limit the scope of the present disclosure.
[0006] Figure 1 is a schematic diagram of an exemplary polymerization reaction.
[0007] Figure 2 The reactions of exemplary monomers in the polymerization reaction are shown.
[0008] Figure 3 Exemplary degradation reaction conditions are shown.
[0009] Figure 4A Shown is the concentration effect for an exemplary polymerization reaction of lipoic acid ester and n-butyl acrylate and the subsequent degradation of the polymer.
[0010] Figure 4B Show Figure 4A Molecular weight analysis of the polymers prepared in and their degradation products.
[0011] Figure 4C Show Figure 4A Degradation linker analysis of the degradation products of the polymers prepared in.
[0012] Figure 5A The temperature effect is shown for an exemplary polymerization reaction of lipoic acid ester and n-butyl acrylate and the subsequent degradation of the polymers.
[0013] Figure 5B Show Figure 5A Molecular weight analysis of the polymers prepared in and their degradation products.
[0014] Figure 5C Show Figure 5A Degradation linker analysis of the degradation products of the polymers prepared in.
[0015] Figure 6 Analysis of the glass transition temperature of polymers of lipoic acid ester and n-butyl acrylate is shown.
[0016] Fig. 7A An exemplary polymerization reaction of lipoic acid, n-butyl acrylate, and acrylic acid is shown.
[0017] Figure 7B Show Fig. 7A Molecular weight analysis of the polymers prepared in and their degradation products.
[0018] Fig. 8A An exemplary polymerization reaction of lipoic acid, n-butyl acrylate, and acrylic acid is shown.
[0019] Figure 8B Show Fig. 8A Analysis of the storage modulus (●) and loss modulus (○) of the polymer prepared in comparison with conventional pressure-sensitive adhesives.
[0020] Figure 8C Show Fig. 8A Molecular weight analysis of the polymers prepared in comparison with conventional pressure sensitive adhesives.
[0021] Fig.9A An exemplary polymerization reaction of lipoic acid ester, n-butyl acrylate, and acrylic acid is shown.
[0022] Fig. 9B Show Fig.9A Molecular weight analysis of the polymers prepared in and their degradation products.
[0023] Fig. 10A Exemplary polymerization reactions of lipoic acid ester, n-butyl acrylate, and t-butyl acrylate are shown.
[0024] Fig. 10B Show Fig. 10A Molecular weight analysis of the polymers prepared in and their degradation products.
[0025] Fig.11AAn exemplary polymerization reaction of lipoic acid ester, n-butyl acrylate, and 1,4-butanediol diacrylate is shown.
[0026] Fig. 11B Shown before and after degradation Fig.11A A polymer having Lp prepared in .
[0027] Fig. 11C Shown by Fig.11A A polymer without Lp, prepared according to the procedure in , but without the lipoic acid ester component, did not degrade under the same conditions.
[0028] Fig.11D Show Fig.11A Molecular weight analysis of the degradation products of the WLp polymer prepared in.
[0029] Fig.12 Shown are the UV absorbance of exemplary polymers after degradation with and without dye functionalization.
[0030] Fig.13A Exemplary lipoic acid ester and styrene monomer units are shown.
[0031] Fig. 13B Show Fig.13A The conversion rate of monomer in the polymerization reaction.
[0032] Fig. 13C Show Fig.13A Molecular weight analysis of the undegraded polymers and degradation products of the monomers.
[0033] Fig.13D Shown by Fig.13A Analysis of the glass transition temperatures of polymers prepared from monomers.
[0034] Fig.14A Exemplary lipoic acid ester and methacrylate monomer units are shown.
[0035] Fig. 14B Show Fig.14A The conversion rate of monomer in the polymerization reaction.
[0036] FIG. 15 shows a master curve generated for PELp.
[0037] Fig.16 The entangled molecular weights of PELp (left) and PnBA (right) are shown.
[0038] Fig.17 The heating rate is 10℃min -1 DSC trace of the homopolymer taken during the second heating cycle of , and the exotherm is located above.
[0039] Fig.18Representative 1H-NMR analysis of degraded ELp-nBA copolymer is shown, highlighting the characteristic resonances.
[0040] Fig.19 Graph showing the effect of polymerization conditions on the degradability of lipoic acid-acrylate copolymers.
[0041] Fig. 20A Shown are size exclusion chromatograms evaluating the effect of polymerized monomer concentration ([M]) on degradability.
[0042] Fig. 20B Shown is a size exclusion chromatography graph evaluating the effect of polymerization temperature (T) on degradability.
[0043] Fig.21A Shown using 0.5 mm min –1 The uniaxial tensile rate of the degradable αLA-ELp-nBA was lap sheared compared with that of the conventional nBA-AA copolymer.
[0044] Fig. 21B Compared with conventional nBA-AA copolymers, the degradable αLA-ELp-nBA -1 Results of 180° peel test under uniaxial extension rate.
[0045] Fig.22A Shown are the preparation of an αLA-ELp-nBA PSA (left) and a traditional acrylic PSA (right) as adhesives for water bottle labels.
[0046] Fig. 22B Shown is the temperature at t = 0 when immersed in THF: water Fig.22A bottle.
[0047] Fig. 22C Shown is the case of a sample immersed in THF:water at t=4. Fig.22A bottle.
[0048] Fig.23 Schematically showing that the functional chain ends generated after degradation undergo repeated oxidative repolymerization and reductive degradation for closed-loop recycling of αLA-ELp-nBA PSA.
[0049] Fig.24 Size exclusion chromatography analysis showing repeated oxidative repolymerization and reductive degradation of the degradable αLA-ELp-nBA PSA. DETAILED DESCRIPTION
[0050] In the following description, numerous specific details are set forth, such as specific structures, components, materials, dimensions, processing steps and techniques, in order to provide a thorough understanding of the present embodiments. However, one of ordinary skill in the art will appreciate that the embodiments may be practiced without these specific details. In other cases, well-known structures or processing steps are not described in detail to avoid obscuring the embodiments.
[0051] The present disclosure relates to compositions of degradable polymers that are easily synthesized from simple chemical building blocks and methods for preparing the same. Advantageously, the compositions can exhibit high molecular weight and adjustable degradation. The disclosed polymer compositions can also advantageously be configured to maintain or even desirably change the performance attributes of current commercial materials, with the additional benefit that the disclosed polymers are degradable. Imparting degradable properties to materials made from conventional polymers provides a mechanism for reducing waste plastics and improving sustainability. Examples of application spaces include: coatings or films in the packaging industry, adhesives, paper coatings, printing inks, foils, personal care / cosmetics (e.g., for hair, skin, washing, clothing), agriculture (e.g., seed protection), resins, films, solutions, and emulsions / dispersions.
[0052] We have developed a new class of degradable polymers that are easily synthesized from simple chemical building blocks. The key features of these materials are (i) high molecular weight, which is critical for commercial applications, and (ii) tunable degradation, including chemical or biological degradation through the introduction of an organosulfur monomer containing a cyclic disulfide group. The degradable polymers disclosed herein are copolymers of an organosulfur monomer containing a cyclic disulfide group and at least one organic monomer such as styrene, acrylate, or vinyl acetate. Figure 1 As shown, copolymerization using an organic sulfur monomer results in the incorporation of sulfur atoms (including disulfide bonds) into the main backbone of the polymer. The resulting polymer can be degraded by chemical degradation (such as by chemical reduction or biodegradation) via cleavage (where the organic sulfur monomer is incorporated into the main backbone).
[0053] like Figure 2 As shown, in free radical polymerization, both the organosulfur monomer and the organic monomer can react with free radicals to generate new free radicals. The free radical of the organosulfur monomer can form a bond with another organosulfur monomer or an organic monomer. Similarly, the free radical of the organic monomer can form a bond with an organosulfur monomer or another organic monomer. A disulfide bond (SS bond) can be formed in the main backbone of the polymer, wherein two organosulfur monomers are bonded to each other during polymerization. The disulfide bond is highly degradable. In addition, the CS and SC bonds formed by the bonding of the organosulfur monomer and the organic monomer can provide alternative sites for initiating degradation.
[0054] When disulfide bonds or thioether bonds degrade, the polymer breaks down into oligomers of fractional size relative to the undegraded polymer. Incorporation of a higher number of disulfide bonds in the main backbone of the polymer is associated with degradation into oligomers with smaller molecular weights compared to polymers with a lower number of disulfide bonds in their main backbone.
[0055] Thus, without wishing to be bound by theory, the degradation of the degradable polymers of the present disclosure can be "tunable" by controlling the amount of organic sulfur monomers forming the repeating units of the polymer backbone and the number of disulfide bonds obtained within the main backbone. In some examples, at least 1% of the bonds between the repeating units of the main backbone of the degradable polymer are disulfide bonds. More preferably, at least 5%, at least 10%, at least 15%, at least 20%, or at least 25% of the bonds between the repeating units of the main backbone of the degradable polymer are disulfide bonds. The upper limit of the disulfide bonds between the repeating units of the main backbone of the degradable polymer is generally limited by the performance characteristics of the resulting polymer. Suitably, the proportion of disulfide bonds in the bonds between the repeating units of the main backbone of the degradable polymer can be 50% or less, 45% or less, 40% or less, 35% or less, or 30% or less.
[0056] Suitable organosulfur monomers typically contain cyclic disulfide groups that can be used for free radical ring-opening polymerization. In addition to two sulfur atoms, the cyclic disulfide group also includes two covalently bonded sulfur atoms in its ring, and preferably between 1 and 6 carbon atoms. Suitable cyclic disulfides are commercially available. Reduced forms of cyclic disulfides can also be used. In some aspects, the hydrocarbon moiety is attached to the cyclic disulfide of the organosulfur monomer. The hydrocarbon moiety can be a hydrocarbon, substituted hydrocarbon, heteroalkyl or substituted heteroalkyl, optionally with a functional group selected from the group consisting of amino, ammonium, imino, amido, imido, nitrile, azo, azido, cyano, cyanooxy, isocyanato, isothiocyanato, hydrazide, nitro, nitroso, nitrosooxy, pyridyl, hydroxyl, alkoxy, carboxyl, ester, acyl, halogen, haloformyl, phosphino, phosphoric acid, phospho, sulfide, disulfide, sulfenyl, mercaptan, sulfonyl, sulfo, sulfinyl, alkenyl, alkynyl, allenyl and silyl. Preferred examples include lipoic acid and lipoic acid derivatives, such as, but not limited to, amides and esters, such as alkyl lipoamides and alkyl lipoic acid esters, including ethyl lipoamide, ethylhexyl lipoamide, ethyl lipoic acid ester, n-butyl lipoic acid ester and ethylhexyl lipoic acid ester.
[0057] In some examples, the organosulfur monomer has the structure of formula (1):
[0058]
[0059] wherein R1, R2 and R3 are each independently selected from the group consisting of: a hydrocarbon group, a substituted hydrocarbon group, a heterohydrocarbon group or a substituted heterohydrocarbon group, optionally having a functional group selected from the group consisting of: an amino group, an ammonium group, an imino group, an acylamino group, an imido group, a nitrile group, an azo group, an azido group, a cyano group, a cyano group, an isocyanato group, an isothiocyanato group, a hydrazide group, a nitro group, a nitroso group, a nitrosooxy group, a pyridyl group, a hydroxyl group, an alkoxy group, a carboxyl group, an ester group, an acyl group, a halogen group, a haloformyl group, a phosphino group, a phosphate group, a phospho group, a sulfide group, a disulfide group, a thiol group, a sulfonyl group, a sulfonyl group, a sulfinyl group, an alkenyl group, an alkynyl group, a propadienyl group and a silyl group. In addition, although formula (1) is shown as having three carbon atoms, it should be understood that the ring may alternatively include a different number of carbon atoms, such as preferably 1 to 6 carbon atoms. It should also be understood that the R1 group can be attached to any carbon in the ring, or there can be multiple R1 groups attached to any combination of carbon atoms in the ring, or the R1 group can be attached to functional groups such as amino, alkoxy, carboxyl, ester, acyl, thio and silyl.
[0060] Suitable organic monomers are not particularly limited. The organic monomers may be polymerized with the organic sulfur monomer alone or in combination with one or more other organic monomers. Exemplary organic monomers include acid-functional monomers, wherein the acid functional group may be an acid itself, such as a carboxylic acid, or a portion thereof may be a salt thereof, such as an alkali metal carboxylate. Useful acid-functional monomers include, but are not limited to, those selected from ethylenically unsaturated carboxylic acids, ethylenically unsaturated sulfonic acids, ethylenically unsaturated phosphonic acids, and mixtures thereof. Examples of such compounds include those selected from acrylic acid, itaconic acid, fumaric acid, crotonic acid, citraconic acid, maleic acid, oleic acid, (meth) β-carboxyethyl acrylate, 2-sulfoethyl methacrylate, styrene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, vinylphosphonic acid, and mixtures thereof. Exemplary polar monomers include, but are not limited to, N-vinyl pyrrolidone; N-vinyl caprolactam; acrylamide; mono- or di-N-alkyl substituted acrylamide; tert-butyl acrylamide; dimethylaminoethyl acrylamide; N-octylacrylamide; alkyl vinyl ethers, including vinyl methyl ether; and mixtures thereof. Exemplary nonpolar monomers include ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate (i.e., isopentyl (meth)acrylate), 3-pentyl (meth)acrylate, 2-methyl-1-butyl (meth)acrylate, 3-methyl-1-butyl (meth)acrylate, stearyl (meth)acrylate, phenyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-methyl-1-pentyl (meth)acrylate, 3-methyl-1-pentyl (meth)acrylate, 4-methyl-2-pentyl (meth)acrylate, 2-ethyl-1-butyl (meth)acrylate, 2-methyl-1-hexyl(meth)acrylate, 3,5,5-trimethyl-1-hexyl(meth)acrylate, cyclohexyl(meth)acrylate, 3-heptyl(meth)acrylate, benzyl(meth)acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, 2-octyl(meth)acrylate, 2-ethyl-1-hexyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, isobornyl(meth)acrylate, 2-propylheptyl(meth)acrylate, isononyl(meth)acrylate, isophoryl(meth)acrylate, n-dodecyl(meth)acrylate (i.e., lauryl(meth)acrylate), n-tridecyl(meth)acrylate, isotridecyl(meth)acrylate, 3,7-dimethyloctyl(meth)acrylate, and any combination or mixture thereof.Exemplary base functional monomers include N,N-dimethyl (meth) acrylamide (NNDMA); N,N-diethyl (meth) acrylamide; N,N-dimethylaminopropyl methacrylamide (DMAPMAm); N,N-diethylaminopropyl methacrylamide (DEAPMAm); N,N-dimethylaminoethyl acrylamide (DMAEAm); N,N-dimethylaminoethyl methacrylamide (DMAEMAm); N,N-diethylaminoethyl acrylamide (DEAEMAm); N,N-diethylaminoethyl methacrylamide (DEAEMAm); N-vinyl formamide, (meth) acrylamide; N-methyl acrylamide , N-ethylacrylamide; n-butyl acrylate; tert-butyl acrylate; 1,4-butanediol diacrylate; N,N-dimethylaminoethyl acrylate (DMAEA); N,N-diethylaminoethyl acrylate (DEAEA); N,N-dimethylaminopropyl acrylate (DMAEA); N,N-diethylaminopropyl acrylate (DEAPA); N,N-dimethylaminoethyl methacrylate (DMAEMA); N,N-diethylaminoethyl methacrylate (DEAEMA); N,N-dimethylaminoethyl vinyl ether (DMAEVE); N,N-diethylaminoethyl vinyl ether (DEAEVE); and mixtures thereof. Other useful basic monomers include vinyl pyridine, vinyl imidazole, tertiary amino functionalized styrene (e.g., 4-(N,N-dimethylamino)-styrene (DMAS), 4-(N,N-diethylamino)-styrene (DEAS)), N-vinyl pyrrolidone, N-vinyl caprolactam, acrylonitrile, and mixtures thereof. Exemplary vinyl monomers include acrylates, substituted acrylates, vinyl esters (e.g., vinyl acetate and vinyl propionate), styrene, substituted styrenes (e.g., α-methylstyrene), vinyl halides, and mixtures thereof. Exemplary monomers also include aliphatic or aromatic comonomer units. In some aspects, the organic monomer is difunctional or trifunctional. Styrene, acrylate, and vinyl acetate monomers are preferred.
[0061] In some aspects, the degradable polymer comprises an organosulfur monomer structural unit in a ratio of up to 50 mol % relative to all structural units. Suitably, the degradable polymer comprises an organosulfur monomer in a mass ratio of up to 45 mol %, up to 40 mol %, up to 35 mol %, up to 35 mol %, up to 25 mol %, up to 20 mol %, up to 15 mol % or up to 10 mol %.
[0062] In some aspects, the degradable polymer comprises an organic monomer or a combination of organic monomers in a molar ratio totaling at least 50 mole %. Suitably, the degradable polymer comprises an organic monomer or a combination of organic monomers in a mass ratio totaling at least 50 mole %, at least 55 mole %, at least 60 mole %, at least 65 mole %, at least 70 mole %, at least 75 mole %, at least 80 mole %, at least 85 mole % or at least 90 mole %.
[0063] In some aspects, the degradable polymer comprises a combination of styrene organic monomers and organic monomers other than styrene in a molar ratio of at least 1 mole %. Suitably, the degradable polymer comprises a combination of styrene organic monomers and organic monomers other than styrene in a mass ratio of at least 2 mole %, at least 3 mole %, at least 4 mole %, at least 5 mole %, at least 10 mole %, at least 15 mole %, at least 20 mole % or at least 25 mole %.
[0064] Polymerization initiators, chain transfer agents, emulsifiers, etc. can be used for polymerization. The polymerization initiator is not particularly limited and can be appropriately selected and used, provided that the initiator does not destroy the organic sulfur monomer. Preferably, the polymerization is carried out in the presence of an azo or non-oxidizing polymerization initiator such as V-65 (2,2'-azobis(2.4-dimethylvaleronitrile) with a CAS number of 4419-11-8 purchased from Wako Specialty Chemicals) or V-70 (2,2'-azobis(4-methoxy-2.4-dimethylvaleronitrile) with a CAS number of 15545-97-8 purchased from Wako Specialty Chemicals). The polymerization initiator can be used alone or in combination of two or more, but the total content is generally 0.005 to 2.5 parts by weight relative to 100 parts by weight of the monomer, and more preferably about 0.02 to 1.5 parts by weight.
[0065] The degradable polymer may be soluble in water or an organic solvent, or may be water-insoluble.
[0066] Degradable polymers can be prepared using crosslinking agents. Examples of crosslinking agents include diacrylate crosslinking agents, distilbene crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, silicone crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, silane crosslinking agents, alkyl etherified melamine crosslinking agents, metal chelate crosslinking agents, including crosslinking agents such as oxides. Crosslinking agents can be used alone or in combination of two or more. As the crosslinking agent, isocyanate crosslinking agents and epoxy crosslinking agents are preferably used. Degradable polymers can also be prepared by crosslinking of ketone groups with dihydrazines (e.g., DAAM and ADDH) and copolymerizable UV photoinitiators.
[0067] The crosslinking agent may be used alone or in combination of two or more, but the total content is based on 100 parts by weight of the degradable polymer. Preferably, 0.01 to 5 parts by weight of the crosslinking agent is contained. The content of the crosslinking agent is preferably 0.01 to 4 parts by weight, more preferably 0.02 to 3 parts by weight.
[0068] The degradable polymer can be synthesized by free radical polymerization techniques. Typically, the method comprises copolymerizing at least two monomers by a copolymerization process, wherein at least one of the comonomers is an organic sulfur monomer capable of incorporating a degradable functional group into the polymer by polymerization.
[0069] Examples of the method also include polymerizing monomers in a chain extension polymerization to form a degradable polymer. The copolymer can be polymerized by conventional techniques including, but not limited to, solvent polymerization, emulsion polymerization, dispersion polymerization, and solvent-free bulk polymerization. The polymerization can be batch or semi-batch.
[0070] Polymerization via emulsion technology may require the presence of an emulsifier (which may also be referred to as an emulsifying agent or surfactant). Emulsifiers useful for the present invention include those selected from the group consisting of anionic surfactants, cationic surfactants, nonionic surfactants and mixtures thereof. Preferably, emulsion polymerization is carried out in the presence of anionic surfactants. Based on the total weight of all monomers of the degradable polymer, the useful range of surfactant concentration is from about 0.5 wt % to about 8 wt %, preferably from about 1 wt % to about 5 wt %.
[0071] Emulsion polymerization processes using organic sulfur monomers typically require a styrene monomer component during the process, otherwise the emulsion may not be stable enough when lipoic acid is added to the system. However, it is possible to prepare emulsions with a monomer mass ratio of up to 50% lipoic acid and 50% comonomer. Dispersions with mass ratios of 12.5% (about 1:12 molar ratio), 25% (about 1:6 molar ratio), and 50% (about 1:3 molar ratio) lipoic acid were polymerized.
[0072] A typical solution polymerization process can be carried out by adding monomers, a suitable solvent and an optional chain transfer agent to a reaction vessel, adding a free radical initiator, purging with nitrogen, and maintaining the reaction vessel at an elevated temperature, typically in the range of about 25°C to 100°C, until the reaction is complete, typically within about 1 to 20 hours, depending on the batch size and temperature. Suitable temperatures include 25°C to 80°C, preferably about 30°C to about 70°C, or more preferably about 40°C to about 60°C. Examples of suitable solvents include methanol, tetrahydrofuran (THF), ethanol, isopropanol, acetone, methyl ethyl ketone, methyl acetate, ethyl acetate, toluene, xylene, dichloromethane (DMC) and ethylene glycol alkyl ethers. These solvents can be used alone or as a mixture. As a specific example of solution polymerization, the reaction is carried out under an inert gas flow such as nitrogen, and a polymerization initiator is added, and the reaction is typically carried out at about 50 to 70°C under reaction conditions of about 5 to 30 hours.
[0073] Degradation of degradable polymers can be accomplished by various methods, including chemical degradation and biological degradation. Figure 3 As shown, chemical degradation can be carried out in various ways, including treatment with amidine compounds such as 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,8-octanedithiol, acid, base, organic fluorine compounds such as trifluoroacetic acid (TFA), reducing agents such as tris(2-carboxyethyl)phosphine (TCEP) or redox agents such as dithiothreitol (DTT). Degradation can be carried out in the presence of solvents such as toluene, tetrahydrofuran (THF) or dichloromethane (DMC), possibly at elevated temperatures. Suitable temperatures include 25°C to 80°C, preferably about 30°C to about 70°C, or more preferably about 35°C to about 60°C.
[0074] Degradable polymers can advantageously have high molecular weights, such as weight average molecular weights greater than 100,000Da. Degradable polymers can have number average molecular weights greater than 125,000Da, greater than 150,000Da or greater than 200,000Da. The upper limit of weight average molecular weight is generally limited by the performance characteristics of the resulting polymer. Suitable upper limits can be 2,000,000Da or less, 1,000,000Da or less, 500,000Da or less, 450,000Da or less, 400,000Da or less or 300,000Da or less. The number average molecular weight can be determined by size exclusion chromatography (SEC), or when the initiator has a group that can be easily distinguished from the monomer by NMR spectroscopy, it can be determined.
[0075] The degradation of the degradable polymer breaks down the polymer into oligomers having fractional sizes relative to the undegraded polymer. Upon degradation, the ratio of the number average molecular weight of the degradation products of the degradable polymer relative to the number average molecular weight of the undegraded form of the degradable polymer is between 0.001 and 0.1, preferably between 0.005 and 0.08, and more preferably between 0.01 and 0.05.
[0076] Degradable polymers also cover novel block, multi-block, star, gradient, random, grafted, comb, hyperbranched and dendritic degradable copolymers, as well as degradable polymer networks and other degradable polymer materials.
[0077] Degradable polymers advantageously retain the performance attributes of current commercial materials with the added benefit that they are degradable, providing a mechanism to reduce waste plastics and improve sustainability. For example, degradable polymers can be used to control the glass transition temperature of a polymer relative to a comparable polymer prepared in the absence of an organosulfur monomer. Additionally, when such degradable polymers are used as adhesives, the glued parts or laminates can be easily separated from each other. This on-demand peeling supports recycling. In such examples, organosulfur monomers can be selectively combined with organic monomers to obtain polymers with increased or decreased glass transition temperatures relative to polymers with only organic monomers. For applications as adhesives, a T of -20°C or less is preferred. g For architectural coating applications, a T of -10°C to 20°C g For paper coating and fiber bonding, a T of 40°C to 80°C g is preferred.
[0078] The degradable polymers of the present disclosure are advantageously suitable for recycling, particularly closed-loop recycling. Suitable methods include subjecting the degradable polymers of the present disclosure to conditions that reduce the disulfide bonds of the degradable polymer to obtain degraded fragments of the degradable polymer. The degraded fragments of the degradable polymer can be repolymerized by any suitable technique to obtain a recycled degradable polymer. Advantageously, the recycling process can be further repeated once, twice, three times or more. For example, the disulfide bonds of the recycled degradable polymer can be subjected to conditions that reduce the disulfide bonds to obtain degraded fragments of the recycled degradable polymer, and the degraded fragments of the recycled degradable polymer can be repolymerized to obtain a twice recycled degradable polymer.
[0079] Example :
[0080] To synthesize ethyl lipoate, ethanol (16.8 g), lipoic acid (25.0 g), 4-dimethylaminopyridine (16.3 g) and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (25.6 g) were added to 300 mL of dichloromethane and stirred at room temperature for 24 hours.
[0081] Lipoic acid was obtained from commercially available sources.
[0082] Copolymerization is usually carried out by mixing monomers (e.g., 10.9 g n-butyl acrylate, 0.4 g acrylic acid, and 3.7 g lipoic acid ester) in a desired ratio in a reactor, and then adding an initiator (e.g., WAKO V65 or WAKO V70 initiator) to the cooled monomer mixture in an ice bath. The monomer solution is fully purged with argon (e.g., 20 minutes), and polymerization is initiated by placing the reactor in an oil bath at 40° C. The polymerization is quenched by cooling with liquid nitrogen, and the synthesized polymer is isolated by precipitation in methanol and drying under high vacuum.
[0083] CDCl3 and acetone-d6 were used as deuterated solvents, and the conversion during polymerization was monitored by nuclear magnetic resonance (NMR, Varian Unity Inova 500 MHz). The molecular weight of the synthesized polymer was measured by differential refractive index (RI) detector, gel permeation chromatography (GPC, Waters Alliance HPLC system) equipped with a photodiode array (PDA) detector, using PLgel, 5μm MiniMIX-D, 250×4.6mm column, and dimethylformamide (DMF) as eluent. The thermal properties of the polymers were observed by differential scanning calorimetry (DSC), and the data were collected on a TA Instruments Discovery DSC 2500 equipped with a liquid nitrogen cooler at a heating rate of 10°C / min. Rheological properties were collected using an advanced rheological expansion system (ARES-G2, TA Instruments).
[0084] Example 1: Pressure-sensitive adhesive (concentration effect)
[0085] according to Figure 4A The monomer units of lipoic acid ester with a total monomer concentration of 1M, 2M or 4M were polymerized with n-butyl acrylate under the reaction conditions listed in to obtain a degradable polymer. The samples of the degradable polymer were prepared according to Figure 4A The molecular weights of the undegraded polymer and the degradation products obtained from the reactions with a total lipoic acid ester monomer concentration of 1 M, 2 M or 4 M were measured and the results are shown in Figure 4BThe undegraded polymer had a number average molecular weight of 141 kDa relative to a polystyrene standard. The molecular weight of the degradation product varied depending on the lipoic acid ester monomer concentration, where the total monomer concentration was 1 M, 2 M, or 4 M, resulting in a number average molecular weight of the degraded polymer of 16 kDa, 4.4 kDa, and 2.0 kDa relative to a polystyrene standard. By comparing the molecular weights before and after degradation with Figure 4C The results shown are compared to measure the % degradation of linker / total.
[0086] Example 2: Pressure Sensitive Adhesive (Temperature Effect)
[0087] according to Figure 5A The reaction conditions listed in the above were used to polymerize monomer units of lipoic acid ester and n-butyl acrylate at a total monomer concentration of 2 M to obtain a degradable polymer. The samples of the degradable polymer were prepared according to Figure 5A The molecular weights of the undegraded polymer and the degradation products obtained from the reactions at 25°C, 40°C or 70°C were measured and the results are shown in Figure 5B The undegraded polymer had a number average molecular weight of 141 kDa relative to a polystyrene standard. The molecular weight of the degradation product varied depending on the polymerization reaction temperature, where the reaction temperature was 25°C, 40°C or 70°C, resulting in a number average molecular weight of the degraded polymer of 3.3 kDa, 4.4 kDa and 13 kDa relative to a polystyrene standard. The degradation linker / total % was measured and the results are shown in Figure 5C middle.
[0088] Example 3: Effect on glass transition temperature
[0089] The effect of incorporating lipoic acid ester comonomer on the glass transition temperature of poly(n-butyl acrylate) (PnBA) was evaluated. Copolymers were prepared with lipoic acid ester monomer and nBA monomer in molar ratios of 0, 10 / 90, 30 / 70, 50 / 50 and 100. The glass transition temperatures of the polymers were measured and the results are shown in Figure 6 As shown in the figure, the corresponding glass transition temperatures of lipoic acid ester and poly(n-butyl acrylate) (PnBA) are similar, and therefore, the lipoic acid ester copolymer exhibits a glass transition temperature in the range between the glass transition temperatures of lipoic acid ester and poly(n-butyl acrylate) (PnBA) homopolymers.
[0090] Example 4: Potential Synthesis Route of PSA (LpOH-nBA-AA)
[0091] according to Fig. 7AThe monomer units of lipoic acid (10 mol%), n-butyl acrylate (85.5 mol%) and acrylic acid (4.5 mol%) were polymerized under the reaction conditions listed in to obtain a degradable polymer. A sample of the degradable polymer was chemically degraded, and the molecular weights of the undegraded polymer and the degradation products obtained from the reaction are shown in Figure 7B The undegraded polymer had a number average molecular weight of 123 kDa relative to a polystyrene standard. The number average molecular weight of the degradation product was 15 kDa relative to a polystyrene standard.
[0092] Example 5: Comparison with Reference Pressure Sensitive Adhesive
[0093] The degradable polymer prepared in Example 4 was compared with a conventional pressure-sensitive adhesive lacking an organosulfur monomer. The conventional pressure-sensitive adhesive contained 95% n-butyl acrylate and 5% acrylic acid on the basis of the main monomers. The 100% resin had a zero shear viscosity of about 40 Pa s at 130°C. The reaction conditions of the degradable polymer were Fig. 8A The storage modulus (●) and loss modulus (○) were compared with those of a conventional pressure-sensitive adhesive (PSA), and the results are shown in Figure 8B The molecular weight distribution of the synthesized degradable polymer (dPSA) prepared in Example 4 was compared with that of a conventional pressure-sensitive adhesive (PSA), and the results are shown in Figure 8C middle.
[0094] Example 6: Potential Synthesis Route of PSA (LpOEt-nBA-AA)
[0095] according to Fig.9A The monomer units of ethyl lipoate (20 mol%), n-butyl acrylate (75 mol%) and acrylic acid (5 mol%) were polymerized under the reaction conditions listed in to obtain a degradable polymer. A sample of the degradable polymer was chemically degraded, and the molecular weights of the undegraded polymer and the degradation products obtained from the reaction are shown in Fig. 9B The undegraded polymer has a number average molecular weight of 120 kDa relative to a polystyrene standard. The number average molecular weight of the degradation product is 1 kDa relative to a polystyrene standard.
[0096] Example 7: Potential Synthesis Route of PSA (LpOEt-nBA-tBA)
[0097] according to Fig. 10A The monomer units of ethyl lipoate (20 mol%), n-butyl acrylate (75 mol%) and tert-butyl acrylate (5 mol%) were polymerized under the reaction conditions listed in to obtain a degradable polymer. A sample of the degradable polymer was chemically degraded with trifluoroacetic acid, and the molecular weights of the undegraded polymer and the degradation products obtained from the reaction are shown in Fig. 10BThe undegraded polymer had a number average molecular weight of 360 kDa relative to a polystyrene standard. The number average molecular weights of the degradation products were 1 kDa and 240 Da relative to a polystyrene standard.
[0098] Example 8: Potential Synthesis Route of Elastomer (LpOEt-nBA-DiAc)
[0099] like Fig.11A As shown, the degradable elastomeric polymer was prepared by bulk polymerization of ethyl lipoate, n-butyl acrylate and 1,4-butanediol diacrylate at 40° C. for 2 hours. The elastomeric polymer was prepared at the molar ratio listed in Table 1.
[0100] Table 1 :
[0101]
[0102] Elastomers prepared with ethyl lipoate (with Lp) were observed and Fig. 11B Treatment with diazabicyclo[5.4.0]undec-7-ene (DBU) and 1,8-octanedithiolic acid was performed under the conditions shown using tetrahydrofuran (THF) as solvent. Elastomers prepared in the absence of ethyl lipoate (without Lp) and in Fig. 11C Treatment with diazabicyclo[5.4.0]undec-7-ene (DBU) and 1,8-octanedithiol acid was performed under the indicated conditions using tetrahydrofuran (THF) as solvent. Fig. 11B and Fig. 11C The comparison of the results confirmed that the elastomer prepared with ethyl lipoate was easily degradable, whereas the elastomer prepared without ethyl lipoate was not degradable even after two days. The molecular weights of the degradation products obtained from the elastomer prepared with ethyl lipoate were measured and are shown in Fig.11D middle.
[0103] Example 9: Post-functionalization of degraded polymers
[0104] like Fig.12 As shown, after degradation, polymers with and without functionalization were prepared by Michael addition with Disperse Red-maleimide. The UV absorbance of the degradation products was measured and is shown in Fig.12 It can be seen that the polymer is bound to the dye and the low molecular weight polymer material is a degradation product of the polymer.
[0105] Example 10: Versatility of Styrene
[0106] The monomer units of ethyl lipoate (15 mol%) and styrene (85 mol%) are as follows Fig.13A The conversion of the monomers was evaluated over a 40 hour period and the results are shown in Fig. 13BThe molecular weights of the undegraded polymer and the degradation products were measured and the results are shown in Fig. 13C Preparation with Fig.13D Monomer units of ethyl lipoate and styrene were added to the polymer in the listed molar ratios and the glass transition temperatures were measured.
[0107] Comparative Example 1: Methacrylate Comonomer
[0108] The monomer units of ethyl lipoate (15 mol%) and methacrylate (85 mol%) were subjected to Fig.14A The polymerization reaction listed in . The conversion of the monomers was evaluated over a 20 hour period and the results are shown in Fig. 14B In. Fig. 14B As shown, ethyl lipoate and methacrylate did not form a copolymer.
[0109] Example 11: Preparation of monomers with a mass ratio of 69% n-butyl acrylate, 25% thioctic acid, 5% styrene and 1% propylene Emulsion of acrylic acid (w / w)
[0110] 37.5g demineralized water, 1.56g Disponil FES 77, 0.22g Dowfax 2A1, 1g ammonia (25%, in water) and 0.5g acrylic acid are added in a 100mL conical flask. Add a triangular magnetic stirring bar, and stir the mixture on a magnetic stirring plate with 1000rpm until a dense foam layer is formed. Add a mixture of 2.5g styrene and 34.5g n-butyl acrylate in small portions to form a stable emulsion. The emulsion was stirred for 5 minutes again. The magnetic stirring plate is set to 500rpm, and the DL-α-lipoic acid of 12.5g is added to the emulsion in small portions, while controlling the stability of the emulsion. If any separation is visible, the stirring plate is set to 1000rpm again until the emulsion becomes stable. After adding the lipoic acid of the entire amount, the emulsion was stirred at least 10 minutes at 1000rpm.
[0111] To introduce the ethyl ester of lipoic acid: the ester is directly miscible with the monomers and the emulsion is prepared by adding the monomers (including the lipoic acid ester) in small portions to the aqueous phase.
[0112] Examples 12-14: Emulsion Polymerization
[0113] 0.3g polystyrene seed (solid content 33%, diameter 30nm) is mixed with 50g water, and added to a 250mL 4-neck round bottom flask and flushed with nitrogen. The mixture is heated up to 70°C-75°C with an oil bath, and 5g initiator WAKO V50 (1%, in water) (2,2'-azobis[2-methylpropionamidine] dihydrochloride) is added. After 5 minutes, the emulsion is fed at a flow rate of 0.62g / min for 180 minutes. The polymerization is continuously initiated for 180 minutes with 20g WAKO V50 at a flow rate of 0.11g / min. Table 2 shows the preparation of the emulsion. Table 3 shows the amount of reactants in the polymerization reaction.
[0114] Table: 2
[0115]
[0116]
[0117] Example 15: Entanglement Molecular Weight
[0118] In order to determine the entanglement molecular weight (M e ) were quantified, and high molecular weight samples were measured in oscillatory shear (Table 4). The master curve was generated via an isothermal frequency sweep at a frequency of 0.1≤ω≤100 rad / s at a fixed strain amplitude. A horizontal shift factor was applied to each frequency series. According to the convention reported in the following literature, the plateau modulus ( N 0 ) to calculate M e : Fetters, LJ et al., Connection between Polymer Molecular Weight, Density, Chain Dimensions, and Melt Viscoelastic Properties. Macromolecules 1994, 27(17), 4639–4647, where R, T and ρ are gas constant, absolute temperature and mass density, respectively. The entanglement molecular weight was calculated using Equation 1.
[0119]
[0120] Table 4: Characterization of PELp homopolymer
[0121]
[0122] a Number average molar mass and D determined using SEC with THF as eluent.
[0123] b Glass transition temperature determined from DSC at a heating rate of 10 °C / min.
[0124] cHomopolymer density was measured at 25°C using a pycnometer.
[0125] dAt reference temperature T ref = Plateau modulus determined by the minimum value of tan δ at 25°C.
[0126] The results show that the key viscoelastic and thermal properties of poly(ethyl lipoate) (PELp) are very similar to those of poly(n-butyl acrylate) (PnBA) (Figure 15), including the entanglement molecular weight, M, determined by rheology. e,PELp =31 kg mol –1 With M e,PnBA =28 kg mol –1 ( Fig.16 ), 41 and T g,PELp =T g,PnBA =–50°C( Fig.17 ). Therefore, partial replacement of n-butyl acrylate with ELp and partial replacement of acrylic acid with αLA should maintain the excellent properties of conventional poly(acrylate) PSAs but impart substantially better degradability.
[0127] Example 16: Degradation of ELp-nBA with TCEP
[0128] In a 4 mL dram vial, ELp-nBA (150 mg, 0.09 mmol) was dissolved in a minimum amount of THF. A solution of TCEP (5 equivalents of thiol) in THF / water (4:1) was added, and the reaction was carried out at 60°C for 16 hours. DCM was added to the reaction mixture, and the degraded polymer was washed with NaHCO3 (10 mL x 1) and purified by precipitation in cold methanol (15 mL x 2). SEC: M n =3.9 kg mol –1 The degradation reaction is shown below.
[0129]
[0130] pass 1 H-NMR analysis of degraded ELp-nBA, such as Fig.18 Importantly, the resulting material has a higher molecular mass than previously reported (and is actually suitable for the range of PSA (M>>M e )) significantly higher number average molecular weight (M n =140 g mol –1 As shown in Table 5, a significant decrease in molecular weight (e.g., 140 kg mol ) was demonstrated upon exposure to tris(2-carboxyethyl)phosphine (Table 5). –1→3.9 kg mol –1 , tris(2-carboxyethyl)phosphine is a chemical reducing agent that reduces disulfide bonds in the ELp–ELp dyad.
[0131] Table 5: Summary of copolymers synthesized at 40 °C and corresponding degradation results
[0132]
[0133] Example 17: Effect of polymerization conditions on degradation
[0134] Applicants have also surprisingly discovered that, as an example, the reaction conditions during the polymerization of nBA ELp copolymers can affect degradability. Fig.19 . Maximum absolute monomer concentration (total [M], Fig. 20A ) and lower reaction temperature (T, Fig. 20B ) results in higher synthetic molecular weight but produces smaller oligomers upon degradation.
[0135] Although unexpected based on the common copolymerization behavior of acrylates, these results can be understood through analysis of the reaction kinetics. In the “terminal model” (in which the monomer addition rate depends only on the chemical identity of the propagating chain end), the “copolymer equation” is often used to relate feed and polymer composition in any case in time. Within this framework, the absolute concentrations of monomers 1 and 2 [M1] and [M2] (e.g., in mol cm -3 denoted by [M2] / [M1] has no effect on the polymer composition, since [M2] / [M1] always appears as a ratio. Any temperature dependence is also minimal, since the various propagation rate constants generally exhibit small differences in activation energies and are subsumed into the so-called reactivity ratios r1 and r2. However, the copolymer equations assume that each propagation step is irreversible. The literature suggests that this may not be true for nBA–ELp copolymers, since ELp homopolymers exhibit an upper temperature limit (T c =139°C), which is characteristic of an equilibrium caused by reversible monomer addition.
[0136] In 1971, Wittmer derived an analogue of the copolymer equation that could handle reversible monomer addition of either one (as shown below) or two components:
[0137]
[0138] Where d[M1] / d[M2] is the instantaneous composition of the polymer formed, K1 is an equilibrium constant characterizing the rate of degrowth versus growth, and x1(r1,K1[M1],[M2]) are functions of the same variables and are abbreviated in Equation 2. In Example 17, we define component 1 as ELp and component 2 as nBA. As is apparent from Equation 2, the instantaneous composition of the polymer includes a term that is scaled as K1 / [M2], which depends on both the absolute concentration [M2] and the temperature through the equilibrium constant K1.
[0139] Copolymerization of ELp or αLA with nBA exhibits reversibility in the growth of 1,2-dithiolane monomers, explaining the significant dependence of degradability on the concentration and temperature used during polymerization. [M2] and T control the average sequence of monomers along the polymer chain, where higher [M2] and lower T favor the formation of ELp–ELp units containing degradable disulfide bonds.
[0140] In addition, the application of Equation 2 at low monomer conversion provides an estimate of the reactivity ratio for nBA–ELp copolymerization: ELp =18.5 and r nBA = 0.36. These values highlight two features of acrylate-1,2-dithiolane polymerization that are essential for efficient formation of degradable poly(acrylate): (i) facile incorporation of lipoate into growing polymer chains (rELp>>1, rnBA<1), and (ii) preferential addition of lipoate radicals to lipoate monomers (rELp>>1), both of which generate degradable disulfide bonds.
[0141] Example 18: Adhesive Properties
[0142] Poly(lipoic acid-co-ethyl lipoate-co-n-butyl acrylate) (αLA-ELp-nBA) copolymers containing 3:58:39 mol % αLA:ELp:nBA were prepared. αLA:ELp:nBA was formulated with Al(acac) at relatively low loadings to improve cohesive strength by mild crosslinking. 0.4 wt % Al(acac) was selected for detailed comparison of physical properties. A control adhesive (poly(n-butyl acrylate-co-acrylic acid) (nBA-AA) with a composition of 97:3 mol %) was also synthesized to simulate traditional commercial adhesives without additional plasticizers or tackifiers.
[0143] Comparison of degradable (αLA-ELp-nBA) and control (nBA-AA) PSA. -1 The lap shear test and uniaxial tensile test rate were 100 mm min -1 The cohesive strength measured by the 180° peel test ( Fig.21A) and bonding strength ( Fig. 21B ) demonstrated similar performance of degradable and non-degradable control analogs.
[0144] Example 19: Recyclability of Removable Labels
[0145] Acrylic PSA and αLA-ELp-nBA were used as adhesives to adhere labels to plastic water bottles. Unlike acrylic PSA, when used as an adhesive for bottle labels, αLA-ELp-nBA degraded cleanly from between the label and the bottle when immersed in 4:1 by volume THF:water containing 1 equivalent of tri(2-carboxyethyl)phosphine (TCEP). The label adhered using αLA-ELp-nBA detached from the bottle after immersion for 4 hours, while the label adhered by acrylic PSA remained attached to the bottle. Fig.22A Showing the label prepared on the bottle, Fig. 22B The bottle is shown immersed in THF:water at t=0 hours, and Fig. 22C The bottle is shown after t = 4 hours in THF:water.
[0146] Example 20: Closed Loop Recirculation
[0147] In principle, reduction of disulfide bonds along the synthesized polymer chain generates telechelic fragments with thiols at each chain end. Coupling experiments of the degraded fragments with maleimide-disperse red 1 in the presence of 1,8-diazabicyclo(5.4.0)undec-7-ene (DBU) showed that thiols are indeed present at both chain ends as monitored by SEC with a UV absorption detector. These thiols can be used to cycle between polymerized and degraded binders, such as Fig.23 Shown schematically.
[0148] For example, initially degraded to M n =13 kg mol –1 The fragments of the synthesized ELp-nBA copolymer (M n , original = 175 kg mol –1 ) can be oxidatively repolymerized using I2 and pyridine to reform the disulfide bonds and restore 81% of the original molecular weight (M n,1× =142 kg mol –1 ). See Fig.24 Subjecting this sample to the same TCEP degradation conditions again reduced the Mn to 11 kgmol –1 And another iteration with M n,2× =119 kg mol –1 polymer. Fig.24 Despite a modest decrease in molecular weight after repeated cycling, these values are still sufficient for adhesive applications.
[0149] Although features and elements are described above in specific combinations, it will be understood by those skilled in the art that each feature or element can be used alone or in any combination with other features and elements. In addition, the compositions and methods described herein can be implemented as coatings or films in the packaging industry, adhesives (including pressure sensitive adhesives), paper coatings, printing inks, foils, personal care / cosmetics (e.g., for hair, skin, washing, clothing), agriculture (e.g., seed protection), resins, films, solutions, and emulsions / dispersions.
Claims
1. A degradable polymer, which is a copolymer of: a) up to 50 mole % of an organosulfur monomer containing a cyclic disulfide group, and b) at least 50 mole % of at least one organic monomer selected from the group consisting of an acid functional monomer, a base functional monomer, a polar monomer, a vinyl monomer, or a combination thereof; The main backbone of the degradable polymer comprises disulfide bonds. 2 . The degradable polymer according to claim 1 , comprising 25 mol % or less of the organic sulfur monomer.
3. The degradable polymer according to claim 1, wherein the organic monomer is selected from the group consisting of styrene, acrylate and vinyl acetate.
4. The degradable polymer according to claim 1, wherein the organic monomer is selected from the group consisting of n-butyl acrylate, ethylhexyl acrylate, tert-butyl acrylate, 1,4-butanediol diacrylate and acrylic acid. The degradable polymer according to claim 1 , wherein the cyclic disulfide group comprises 1 to 8 carbon atoms. The degradable polymer according to claim 1 , wherein the organic sulfur monomer comprises lipoic acid or a derivative thereof.
7. The degradable polymer according to claim 1, wherein the organic sulfur monomer has a structure of formula (I): wherein R1, R2 and R3 are each independently selected from the group of hydrocarbon, substituted hydrocarbon, heterohydrocarbon and substituted heterohydrocarbon, optionally having a functional group selected from the group consisting of amino, ammonium, imino, amido, imide, nitrile, azo, azido, cyano, cyanoxy, isocyanate, isothiocyanate, hydrazide, nitro, nitroso, nitrosooxy, pyridyl, hydroxyl, alkoxy, carboxyl, ester, acyl, halogen, haloformyl, phosphino, phosphate, phospho, sulfide, disulfide, thiol, sulfonyl, sulfonyl, sulfinyl, alkenyl, alkynyl, allenyl and silyl. 8 . The degradable polymer according to claim 1 , wherein the degradable polymer comprises a combination of a styrene monomer and an organic monomer other than styrene in a molar ratio of at least 1 mol %.
9. The degradable polymer according to claim 1, wherein at least 1% of the bonds between repeating units of the main backbone of the degradable polymer are disulfide bonds.
10. The degradable polymer according to claim 1, wherein the number average molecular weight of the degradable polymer is greater than 100,000 Da. The degradable polymer according to claim 1 , wherein the degradable polymer is cross-linked. 12 . The degradable polymer according to claim 1 , wherein a ratio of a molecular weight of a degradation product of the degradable polymer relative to the degradable polymer is 0.001 to 0.
1.
13. A method for producing a degradable polymer, the method comprising polymerizing up to 50 mol % of an organic sulfur monomer containing a cyclic disulfide group with at least 50 mol % of at least one organic monomer selected from the group of acid functional monomers, base functional monomers, polar monomers, non-polar monomers, vinyl monomers or combinations thereof to obtain a degradable polymer having a main backbone containing disulfide bonds.
14. The process according to claim 13, wherein the polymerization is carried out in the presence of an azo or non-oxidizing initiator.
15. The method of claim 13, wherein the polymerization is solution polymerization or emulsion polymerization.
16. The method of claim 13, wherein the organosulfur monomer is polymerized in an amount of 25 mol% or less.
17. The method of claim 13, wherein the organic monomer is selected from the group consisting of styrene, acrylates, and vinyl acetate.
18. The method of claim 13, wherein the organic monomer is selected from the group consisting of n-butyl acrylate, tert-butyl acrylate, 1,4-butanediol diacrylate, and acrylic acid.
19. The method of claim 13, wherein the cyclic disulfide group comprises 1 to 8 carbon atoms.
20. The method of claim 13, wherein the organic sulfur monomer comprises lipoic acid or a derivative thereof.
21. The method of claim 13, wherein the organosulfur monomer has a structure of formula (I): wherein R1 is selected from the group of hydrocarbon, substituted hydrocarbon, heterohydrocarbon and substituted heterohydrocarbon, optionally having a functional group selected from the group consisting of amino, ammonium, imino, amido, imide, nitrile, azo, azido, cyano, cyanoxy, isocyanate, isothiocyanate, hydrazide, nitro, nitroso, nitrosooxy, pyridyl, hydroxyl, alkoxy, carboxyl, ester, acyl, halogen, haloformyl, phosphino, phosphate, phospho, sulfide, disulfide, thiol, sulfonyl, sulfonyl, sulfinyl, alkenyl, alkynyl, allenyl and silyl.
22. The method of claim 13, wherein the at least one organic monomer comprises a combination of a styrene monomer and an organic monomer other than styrene in a mass ratio of at least 1 mol%.
23. The method of claim 13, wherein at least 5% of the bonds between repeating units of the main backbone of the degradable polymer are disulfide bonds.
24. The degradable polymer of claim 1, further comprising cross-linking the degradable polymer.
25. A pressure-sensitive adhesive comprising the degradable polymer according to claim 1.
26. A method for recycling the degradable polymer according to claim 1, the method comprising: a) reducing the disulfide bonds of the degradable polymer to obtain degradation fragments of the degradable polymer, and b) repolymerizing the degradation fragments of the degradable polymer to obtain a recycled degradable polymer.
27. The method according to claim 26, further comprising: c) reducing disulfide bonds of the recycled degradable polymer to obtain degradation fragments of the recycled degradable polymer, and d) repolymerizing the degradation fragments of the recycled degradable polymer to obtain a twice recycled degradable polymer.
Citation Information
Cited By
Degradable mobile phone gum material and preparation process thereof
CN120082305A