Method for producing expandable polyamide-based resin particles, method for producing expanded polyamide-based resin particles, and expanded polyamide-based resin particles

CN118974154APending Publication Date: 2024-11-15JSP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030878.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing polyamide resin foaming method, it is difficult for the foaming agent to fully impregnate into the central area of ​​the pellet, resulting in uneven residual parts of the unexpanded part and uneven diameter of the cell, and it is difficult to expand when heated with steam, and has low productivity.

Method used

By adding carbon black to polyamide resin particles, its moisture content and carbon black content are increased, the inorganic physical foaming agent in the gas phase is used to impregnate at a lower temperature and in a shorter time, and the particles are foamed by heating. Form a uniform closed bubble cell.

Benefits of technology

It is possible to fully impregnate the foaming agent at low temperature and in a short time, and obtain polyamide resin expanded beads with low apparent density and uniformly distributed cells, which improve productivity, and achieve excellent expansion effect even with steam heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974154A_ABST
    Figure CN118974154A_ABST
Patent Text Reader

Abstract

The method for manufacturing foamable polyamide-based resin particles according to the present invention comprises impregnating polyamide-based resin particles with an inorganic physical blowing agent in a gas phase, wherein the polyamide-based resin particles have a moisture content of at least 2.5 mass% and contain 0.5-10 mass% of carbon black. Polyamide-based resin foamed particles are obtained by heating and foaming the foamable polyamide resin particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing expandable polyamide resin particles, a method for producing expanded polyamide resin beads, and expanded polyamide resin beads. Background Art

[0002] Polyamide resins have high heat resistance and are excellent in abrasion resistance, chemical resistance, etc. The foamed products obtained by foaming polyamide resins have these excellent properties and are light in weight. Therefore, polyamide resin foamed products are expected to be used in automotive parts and other applications. For example, Patent Document 1 discloses polyamide resin expanded beads having excellent formability and capable of obtaining expanded bead molded products.

[0003] Specifically, Patent Document 1 discloses a method for manufacturing pre-expanded beads, which includes charging polyamide pellets into a pressure vessel at 10°C, blowing 4 MPa of carbon dioxide gas therein, allowing the pellets to stand therein for 12 hours to absorb the carbon dioxide gas, transferring the carbon dioxide-impregnated pellets to a foaming device, and blowing 200°C air into the foaming device for 20 seconds.

[0004] Prior art documents

[0005] Patent Documents

[0006] Patent Document 1: International Publication No. WO2020 / 031803 Summary of the invention

[0007] Problems to be solved by the present invention

[0008] However, the method of Patent Document 1 has the problem that an unexpanded portion remains in the central portion of the pre-expanded beads and the cell diameter varies greatly. In addition, when steam is used as a heating medium, expansion itself tends to become difficult. These problems are considered to be due to the fact that it is difficult for carbon dioxide gas, which is a foaming agent, to be sufficiently impregnated into the central region of the polyamide pellets. On the other hand, if the impregnation time is made sufficiently long, it may be possible to impregnate the central region of the polyamide pellets with the foaming agent, but in this case, the problem of significantly reduced productivity is caused.

[0009] The present invention is made in view of the above problems, and its objective problem is to provide a method for producing expandable polyamide resin particles, in which a blowing agent is fully impregnated inside at a lower temperature and / or in a shorter time than those in conventional methods. Another objective problem of the present invention is to provide a method for producing polyamide resin expanded beads, which have uniform closed cells throughout the expanded beads and have a small apparent density. Still another objective problem of the present invention is to provide polyamide resin expanded beads that can provide foamed molded products with excellent surface properties, mechanical strength, lightness, and heat resistance.

[0010] Means of solving the problem

[0011] According to the present invention, there are provided the following method for producing expandable polyamide-based resin particles, method for producing expanded polyamide-based resin beads, and expanded polyamide-based resin beads.

[0012] [1] A method for producing expandable polyamide resin particles,

[0013] It includes impregnating polyamide resin particles with an inorganic foaming agent in a gas phase,

[0014] The polyamide resin particles have a moisture content of 2.5% by mass or more and contain carbon black in an amount of 0.5% by mass or more and 10% by mass or less.

[0015] [2] The method according to [1] above, wherein the impregnation is performed at a temperature higher than a temperature of a storage modulus change point of the polyamide-based resin particles.

[0016] [3] The method according to [1] or [2] above, wherein the impregnation is performed at a temperature 30°C higher than the storage modulus change point of the polyamide-based resin particles and not higher than 120°C.

[0017] [4] The method according to any one of [1] to [3] above, wherein the immersion is performed at a temperature of not lower than 20°C and not higher than 120°C.

[0018] [5] The method according to any one of [1] to [4] above, wherein the carbon black has a carbon black content of 50 m 2 / g or more and 200m 2 / g or less BET specific surface area.

[0019] [6] The method according to any one of [1] to [5] above, wherein the polyamide-based resin particles have a moisture content of 5% by mass or more and 20% by mass or less.

[0020] [7] The method according to any one of [1] to [6] above, wherein the polyamide-based resin particles are obtained by a method comprising the following steps:

[0021] (a) providing carbon black-containing polyamide-based resin pellets, the pellets having a carbon black content of 0.5% by mass or more and 10% by mass or less, and

[0022] (b) Wetting the carbon black-containing polyamide-based resin pellets to a moisture content of 2.5% by mass or more.

[0023] [8] A method for producing polyamide-based resin expanded beads, comprising heating the expandable particles according to any one of [1] to [7] above to foam and expand the expandable particles.

[0024] [9] An expanded bead having a plurality of cells and comprising a polyamide-based resin and carbon black,

[0025] The carbon black is contained in the expanded beads in an amount of 0.5% by mass or more and 10% by mass or less based on 100% by mass of the expanded beads,

[0026] The expanded beads have a mass of 100 kg / m 3 Above and 800kg / m 3 The following apparent density, closed cell content of 80% or more, average cell diameter D of all cells of the expanded beads and average cell diameter Dc of cells located in the central region of the expanded beads,

[0027] The ratio Dc / D is 0.7 or more and 1.3 or less.

[0028]

[10] The expanded particles according to the above [9], which can be obtained according to the method of the above [8].

[0029] Effects of the Invention

[0030] According to the method for manufacturing expandable polyamide resin particles of the present invention, expandable polyamide resin particles whose interior is fully impregnated with an inorganic physical foaming agent can be obtained at a lower temperature and / or in a shorter time than in conventional methods. By heating the expandable polyamide resin particles using, for example, hot air or an oil bath, polyamide resin expanded beads having a low apparent density and uniform closed cells formed throughout the expanded beads can be obtained. In addition, even when the expandable polyamide resin particles are heated using steam as a heating medium, polyamide resin expanded beads having a low apparent density can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a graph plotting the change in storage modulus change point temperature of a film formed from polyamide resin particles as a function of moisture content.

[0032] Figure 2 This is a graph schematically showing the relationship between the storage modulus and temperature of a film formed of polyamide-based resin particles, which is measured in accordance with JIS K7095 (2012).

[0033] Figure 3 This is a SEM photograph of the cross section of the expanded beads obtained in Example 1.

[0034] Figure 4 is a cross-sectional SEM photograph of the expanded beads obtained in Comparative Example 1.

[0035] Figure 5 This is a SEM photograph of the cross section of the expanded beads obtained in Comparative Example 3. DETAILED DESCRIPTION

[0036] Hereinafter, a method for producing expandable particles comprising a polyamide-based resin and a method for producing polyamide-based resin expanded beads of the present invention will be described in detail.

[0037] As used herein, "A to B" showing a numerical range is synonymous with "A above and B below" and refers to a numerical range that includes the endpoints A and B of the numerical range. In the specification and claims, the singular form (one, a, the) includes plural references unless the context clearly dictates otherwise. Thus, for example, an expandable particle includes two or more expandable particles. Unless otherwise expressly stated herein or clearly contradicted by the context, the singular form is intended to include plural references. In addition, unless the context clearly indicates otherwise, the upper and lower limits of all range limits disclosed in the specification and claims are intended to be independently combinable with each other to define the sub-ranges contained therein.

[0038] The method for producing expandable polyamide resin particles (hereinafter also referred to as "expandable particles") of the present invention includes impregnating polyamide resin particles (hereinafter also referred to as "resin particles") with an inorganic physical foaming agent in a gas phase. Importantly, the polyamide resin particles have a moisture content of 2.5% by mass or more and contain 0.5 to 10% by mass of carbon black. By using resin particles having a moisture content and a carbon black content within a specific range, expandable particles in which a foaming agent is uniformly impregnated into the interior thereof can be produced. The method for producing polyamide resin expanded beads (hereinafter also referred to as "expanded beads") includes heating and expanding expandable particles. The resulting expanded beads form uniform cells throughout the beads and have a high closed cell content and a small apparent density.

[0039] The resin particles, the expandable particles obtained from the resin particles, and the expanded beads obtained from the expandable particles each contain a polyamide resin. The polyamide resin can be a single type of resin or a mixed resin of two or more types. Examples of polyamide resins include polyamides and polyamide copolymers, wherein polyamide copolymers are preferred. Such polyamides include homopolymers such as poly(6-aminocaproic acid), also known as poly(caprolactam) (polycaproamide, nylon 6), poly(laurolactam) (nylon 12), poly(hexamethylene adipamide) (nylon 66), poly(7-aminoheptanoic acid) (nylon 7), poly(8-aminooctanoic acid) (nylon 8), poly(9-aminononanoic acid) (nylon 9), poly(10-aminodecanoic acid) (nylon 10), poly(11-aminoundecanoic acid) (nylon 11), poly(hexamethylene sebacamide) (nylon 610), poly(decamethylene sebacamide) (nylon 1010), poly(hexamethylene nonamide) (nylon 69), poly(tetramethylene adipamide) (nylon 46), poly(tetramethylene sebacamide) (nylon 410), poly(pentamethylene adipamide) (nylon 56), and poly(pentamethylene sebacamide) (nylon 510).

[0040] Polyamide copolymer refers to a copolymer having two or more types of repeating units, wherein at least a portion of the repeating units each have an amide bond. Examples of polyamide copolymers include polycaproamide / polyhexamethylene adipamide copolymers (nylon 6 / 66), caprolactam / hexamethylenediaminoadipamide / laurolactam (nylon 6 / 66 / 12), and caprolactam / laurolactam copolymers (nylon 6 / 12).

[0041] In the present invention, these polyamides and polyamide copolymers can be used alone or in combination of two or more. Among the polyamide resins mentioned above, from the perspective of excellent foaming properties, polyamide resins selected from one or a combination of two or more of nylon 6, nylon 66, nylon 6 / 66 / 12 and nylon 6 / 66 are preferred, and nylon 6 / 66 is more preferred. In addition, from the same perspective, the polyamide copolymer is preferably a random copolymer in which different types of amides are randomly repeated.

[0042] In order to improve the heat resistance of the finally obtained expanded beads or expanded beads molded articles, the polyamide resin preferably has a melting point of 180° C. or higher, more preferably 185° C. or higher, and even more preferably 190° C. or higher. On the other hand, in order to reduce the load on the equipment used for heating the expandable polyamide resin particles impregnated with the inorganic physical foaming agent with a heating medium, the melting point is preferably 280° C. or lower, more preferably 260° C. or lower, even more preferably 240° C. or lower, and particularly preferably 220° C. or lower.

[0043] Incidentally, when the polyamide resin constituting the resin pellets is composed of a single type of polyamide resin, the melting point of the polyamide resin refers to the melting point of the polyamide resin. When the resin pellets are composed of a mixture of two or more types of polyamide resins, the melting point of the polyamide resin refers to the melting point of the mixture that has been kneaded in advance using, for example, an extruder.

[0044] The melting point of polyamide resin is measured according to JIS K7121 (1987). Specifically, the polyamide resin sample is heated and melted from 30 ° C at a heating rate of 10 ° C / min to a temperature 30 ° C higher than the melting end temperature (first heating) by heat flux differential scanning calorimetry, and then kept at this temperature for 10 minutes, and then cooled to 30 ° C at a cooling rate of 10 ° C / min, and then heated again at a heating rate of 10 ° C / min to a temperature 30 ° C higher than the melting peak end temperature to obtain a second heating DSC curve. The peak top temperature (melting peak temperature) of the melting peak of the second heating DSC curve is defined as the melting point. When the DSC curve has multiple melting peaks, the melting point is the peak top temperature of the melting peak with the largest area. The polyamide resin used for measurement has a moisture content of less than 1000 mass ppm. A high-sensitivity differential scanning calorimeter "EXSTARDSC7020" (manufactured by SII Nano Technology Inc.) can be used as a measuring device.

[0045] The flexural modulus of the polyamide resin is preferably 1000 MPa or more, more preferably 1050 MPa or more, still more preferably 1100 MPa or more, and particularly preferably 1200 MPa or more. When the flexural modulus of the polyamide resin is within this range, the polyamide resin hardly shrinks even when exposed to room temperature after expansion, so expanded beads with low apparent density can be easily obtained. The upper limit of the flexural modulus of the polyamide resin is generally about 3000 MPa. Incidentally, amide elastomers generally have a flexural modulus of about 600 MPa or less.

[0046] The flexural modulus of the polyamide-based resin is measured in accordance with JIS K7171 (2016). The polyamide-based resin used for the measurement has a water content of 1000 mass ppm or less.

[0047] The density of polyamide resin is preferably 1050 kg / m 3 More preferably 1100 kg / m 3 On the other hand, the upper limit is about 1300 kg / m 3 , preferably 1200kg / m 3 By the way, the density of amide elastomer is about less than 1050kg / m 3The density of the polyamide-based resin can be measured based on the method described in ISO 1183-3.

[0048] The resin particles used in the method of the present invention may contain other polymers such as thermoplastic resins except polyamide resins and thermoplastic elastomers, as long as they do not adversely affect the purpose and effect of the present invention. Examples of other thermoplastic resins include polyethylene resins, polypropylene resins, polystyrene resins, vinyl acetate resins, thermoplastic polyester resins, acrylate resins, methacrylate resins and polyphenylene sulfide resins. Examples of thermoplastic elastomers include styrene thermoplastic elastomers, olefin thermoplastic elastomers and amide thermoplastic elastomers. Based on 100 parts by mass of resin particles in a dry state, the content of the other polymers is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, still more preferably 5 parts by mass or less, and particularly preferably 0 parts by mass. That is to say, it is particularly preferred that the resin particles do not substantially contain any polymer except polyamide resins.

[0049] In addition, resin particles can be added with common additives as needed, such as cell control agents, end-capping agents, antistatic agents, conductivity imparting agents, weathering agents, lubricants, antioxidants, ultraviolet absorbers, flame retardants, metal passivators, colorants (pigments, dyes, etc.), crystal nucleating agents and fillers. The example of cell control agent includes inorganic control agents such as talcum, sodium chloride, calcium carbonate and silicon oxide, titanium oxide, gypsum, zeolite, borax, aluminum hydroxide, alum and carbon, and organic cell control agents such as phosphoric acid compounds, amine compounds and polytetrafluoroethylene (PTFE). The addition amount of these various additives varies with the purpose of use of the resulting molded product, but based on 100 parts by mass of resin particles, preferably less than 25 parts by mass, more preferably less than 15 parts by mass, and more preferably less than 10 parts by mass, particularly preferably less than 5 parts by mass. The optional components (other polymers and additives) mentioned above are added in the process of manufacturing resin particles, and are mixed and kneaded with polyamide resins.

[0050] As described above, the method for producing expandable particles of the present invention includes impregnating resin particles having a water content of 2.5% by mass or more and containing 0.5 to 10% by mass of carbon black with an inorganic physical foaming agent in a gas phase.

[0051] In a preferred embodiment of the present invention, the resin particles are obtained by a method comprising the following steps: (a) a carbon black-containing polyamide resin pellet manufacturing step in which carbon black-containing polyamide resin pellets are manufactured; and (b) a wetting step in which the obtained carbon black-containing polyamide resin pellets are wetted. Expandable particles can be obtained by performing a blowing agent impregnation step (c) in which the wetted resin particles obtained in the wetting step (b) are impregnated with an inorganic physical blowing agent in a gas phase. In addition, expanded beads can be obtained by performing a foaming step (d) in which the expandable particles are heated. The carbon black-containing polyamide resin pellet manufacturing step (a), the wetting step (b), the blowing agent impregnation step (c) and the foaming step (d) will be described in detail below.

[0052] Preparation steps of carbon black-containing polyamide resin pellets (a):

[0053] A preferred method for manufacturing carbon black-containing polyamide resin pellets (hereinafter also referred to as CB-containing pellets) is as follows. First, polyamide resin, carbon black and optional additives such as cell control agents and end-capping agents blended as needed are melted and kneaded using an extruder to obtain a melt-kneaded product. The melt-kneaded material is then extruded into strips through a small hole in a die head attached to the tip of the extruder, and the strips are then cut into pellets of a predetermined size to obtain CB-containing pellets. The method of cutting the extruded melt-kneaded product may be, for example, a strip cutting method, in which the extruded strip-shaped melt-kneaded product is cooled in water and cut into a predetermined weight using a pelletizer; a hot cutting method, in which the melt-kneaded product is cut immediately after being extruded into the gas phase; and an underwater cutting method (UWC method), in which the melt-kneaded product is cut immediately after being extruded into water.

[0054] In the present invention, as described above, it is required that the resin particles have a moisture content of 2.5% by mass or more and contain a predetermined amount of carbon black in addition. By including a predetermined amount of carbon black in the resin particles, the foaming agent can be more uniformly impregnated into the interior of the resin particles compared to the case of wet state resin particles not containing carbon black. As a result, the obtained expanded beads are fully foamed inside thereof, and therefore, more uniform cells are formed throughout the expanded beads. In addition, expanded beads having a high closed cell content and a low apparent density can be more easily obtained.

[0055] Carbon black is a material generally used as a colorant. Although the reason why carbon black exhibits the above-mentioned unique effects is not clear, it is presumed that the reason is that by including carbon black in the resin particles, the impregnation efficiency of the wetted resin particles with the blowing agent will be improved, by including a predetermined amount of carbon black and water, the viscoelasticity of the resin particles will become a state that is conducive to foaming, and by appropriate plasticization of the polyamide-based resin in a wet state, the nucleation effect of the carbon black will work well to serve as a foaming starting point.

[0056] The carbon black content in the resin particles is 0.5 to 10% by mass. When the carbon black content is too small, the foaming agent will be difficult to be uniformly impregnated into the resin particles, and therefore, the uniformity of the cell diameter of the resulting expanded beads may deteriorate. For this reason, the content is preferably 1% by mass or more, more preferably 1.5% by mass or more, and more preferably 2% by mass or more. On the other hand, when the carbon black content is too large, the formability may deteriorate. For this reason, the content is preferably 8% by mass or less, more preferably 5% by mass or less, and more preferably 4.5% by mass or less, particularly preferably 3% by mass or less. The upper limit and lower limit of the above range can be arbitrarily combined to define the preferred range of content. Therefore, the preferred carbon black content range is, for example, 1 to 10% by mass, 1.5 to 10% by mass, 2 to 8% by mass, 0.5 to 8% by mass, 1.5 to 8% by mass, 1.5 to 4.5% by weight, and 2 to 3% by weight.

[0057] As used in this specification and claims, "carbon black content" refers to the percentage of carbon black in CB-containing pellets based on the mass of CB-containing pellets, and can be determined according to the amount of carbon black blended when manufacturing CB-containing pellets. "Carbon black content" can also be defined as its content based on the mass of "resin pellets in a dry state". As used herein, "resin pellets in a dry state" refers to a state in which the moisture content in the resin pellets is less than 2.5% by mass.

[0058] The production method and composition of carbon black are not particularly limited. For example, channel carbon black, roll carbon black, furnace carbon black, thermal carbon black, acetylene black, Ketjen black can be used. In addition, these carbon blacks can be subjected to hydrophilization, hydrophobization, oxidation, reduction, acidification, alkalization or organic treatment. From the perspective of excellent dispersibility in polyamide resins, furnace carbon black is a preferred carbon black.

[0059] For the reason of improving the efficiency of impregnation of the foaming agent into the wet resin particles, the dibutyl phthalate (i.e., DBP) oil absorption of carbon black is preferably less than 150 mL / 100 g, more preferably 130 mL / 100 g or less, and still more preferably 110 mL / 100 g or less. The lower limit of the oil absorption is preferably 80 mL / 100 g. The DBP oil absorption is a value measured according to ASTM D2414-79.

[0060] For the same reasons as above, the BET specific surface area of ​​carbon black is preferably 200 m 2 / g or less, more preferably 150m 2 / g or less, and more preferably 100m / g or less 2 / g or less. The lower limit is preferably 50m 2 The BET specific surface area of ​​carbon black is a value measured by the BET method according to ASTM D-3037.

[0061] Carbon black can be selected from those listed above. Carbon black is preferably blended with the polyamide resin in the form of a masterbatch because the carbon black can be more uniformly dispersed in the polyamide resin. The concentration of carbon black in the masterbatch is preferably 10% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 60% by mass or less. The base resin of the masterbatch may be a resin other than the polyamide resin.

[0062] Wetting step (b):

[0063] In the wetting step, the CB-containing pellets obtained in step (a) are wetted to obtain resin particles having a moisture content of 2.5% or more by mass. In the present specification and claims, the term "wetting" refers to the process of impregnating the CB-containing pellets with water or water vapor to obtain resin particles having a desired moisture content of 2.5% or more.

[0064] When using dry polyamide resin particles having a moisture content of less than 2.5% by mass, it is difficult to fully impregnate the inorganic physical foaming agent into the interior of the resin particles, and therefore, such resin particles may be difficult to foam and expand. Even if expanded beads are obtained, unfoamed portions may remain inside the expanded beads or the cell diameter may become quite uneven.

[0065] Wetting can be achieved using any commonly known means as long as it can adjust the moisture content of the resin particles to the desired range. For example, a first wetting method can be used, in which the CB-containing pellets are allowed to stand under standard conditions (e.g., 1 atm, temperature 23°C, humidity 50%) for more than 12 hours, preferably more than 24 hours; a second wetting method, in which the CB-containing pellets are allowed to stand under high temperature and high humidity conditions (temperature above 23°C, such as 40°C, humidity above 50%, such as 80%) for at least 3 hours, preferably at least 5 hours; a third wetting method, in which the CB-containing pellets are immersed in water and allowed to stand, for example, for 10 seconds to 4 hours; a fourth wetting method, in which the CB-containing pellets are put into a bag or container together with water and stirred or mixed by hand or mechanically; and a fifth wetting method, in which water is sprayed onto the CB-containing pellets by spraying or spraying. These first to fifth wetting methods can also be performed in combination as appropriate.

[0066] According to these wetting methods, the moisture content of the entire resin particles can be adjusted to a desired range while suppressing the variation in moisture content between the obtained resin particles. Therefore, in the blowing agent impregnation step (c) described below, the blowing agent can be sufficiently impregnated into the interior of the resin particles even in a short time and / or under low temperature conditions.

[0067] The first method is suitable for obtaining resin particles having a moisture content of about 2.5% to 4% by mass. The second to fourth methods are suitable for obtaining resin particles having a moisture content of 4% or more, or 4.5% or more by mass. The second or third wetting method is preferred because resin particles having a uniform moisture content can be obtained in a shorter time. In the first and second wetting methods, the CB-containing pellets are wetted in a chamber maintained under predetermined conditions, wherein the resin particles are contained in an open or unsealed container, bag, tray, etc.

[0068] The water content of the resin particles is preferably 3.0% by mass or more, more preferably 4.0% by mass or more, more preferably 4.5% by mass or more, still more preferably 5.0% by mass or more, and particularly preferably 8.0% by mass or more, because the resin particles can be fully impregnated with an inorganic physical foaming agent in the foaming agent impregnation step (c) after the wetting step (b). The upper limit of the water content is not particularly limited, but is generally 20% by mass. In order to make the expandable particles obtained in the foaming agent impregnation step (c) less likely to adhere in the foaming step (d), the upper limit is preferably 18% by mass or less, more preferably 16% by mass or less. The above upper and lower limits of the water content can be arbitrarily combined to define the preferred range of the water content. Therefore, the preferred range of the water content of the resin particles is, for example, 3 to 20% by mass, 4.5 to 20% by mass, 5 to 20% by mass, 5 to 18% by mass, 8 to 20% by mass, 8 to 18% by mass, and 8 to 16% by mass.

[0069] In the present invention, a halogen moisture meter may be used as a measuring device to measure the moisture content of the resin particles. A specific example of the measuring device is a halogen moisture meter (HX204) manufactured by METTLER TOLEDO, in which the moisture content is measured based on heating with a halogen lamp.

[0070] Specifically, the moisture content of resin particles can be measured as follows. First, about 2.0g of resin particles are sampled, and the moisture attached to the surface of the resin particles is removed by wiping with a wipe such as paper or cloth to obtain a resin particle sample. The weight of the sample (W0) is measured and placed in a halogen moisture meter. Next, the sample is heated to a temperature of 100°C and maintained at 100°C for 60 seconds until the weight no longer changes. Thereafter, the sample is further heated to 160°C and maintained at 160°C for 90 seconds until the weight no longer changes to obtain an anhydrous sample. The weight (W1) of the anhydrous sample is measured. Based on the weight of the sample before heating, the percentage of weight loss of the sample due to heating ((W0-W1) / W0×100) (%) is defined as the moisture content (%). The moisture content of the polyamide film described below is determined by the same method as the moisture content of the resin particles, except that the weight of the measured sample is about 0.5g.

[0071] In the present invention, the physical foaming agent can be efficiently impregnated into the resin particles. The reason for this is believed to be that the gas barrier properties of polyamide-based resins deteriorate when the resin is in a wet state. In the case of polyolefin resins, polystyrene resins, etc., which are generally used as base resins for expanded beads, such a phenomenon that the gas barrier properties of the resin deteriorate in a wet state does not occur.

[0072] Although impregnation of polyamide resin pellets with inorganic physical foaming agents in the gas phase has been conventionally performed, it has now been found that there is a problem of low productivity. The inventors have studied the cause of this problem and found that the gas barrier properties of polyamide resins are significantly higher than those of polyolefin resins such as polypropylene resins, and therefore it is difficult to impregnate resin particles with a foaming agent. In other words, since polyamide resins have high gas barrier properties, it is difficult to impregnate the foaming agent into the resin when attempting to impregnate the resin with a foaming agent in the gas phase. Therefore, when the expandable particles obtained are heated and foamed, the unfoamed portion may remain in the central area of ​​the expanded beads, so that a large change in the pore diameter may occur. In addition, when steam is used as a heating medium, it is difficult to foam the expandable beads themselves.

[0073] In this case, the process of impregnating polyamide-based resin pellets with an inorganic physical foaming agent is conventionally performed under high pressure for a long time or under high temperature conditions.

[0074] The present inventors have found that when a polyamide resin contains a large amount of water, its gas barrier properties are reduced and impregnation with an inorganic physical foaming agent can be promoted. Specifically, it has been found that by setting the carbon black content of polyamide resin particles within a specific range and by controlling the water content thereof to a specific value or more, impregnation of the foaming agent in the gas phase into the resin particles is promoted. The present invention has been completed based on these findings.

[0075] In addition, as will be described below, it has been found that the temperature of the storage modulus change point of the resin particles in the wet state, which is determined by the dynamic viscoelasticity measurement using dynamic mechanical analysis (DMA), is often lower than that of the polyamide resin particles (i.e., CB-containing pellets) before moisture absorption. At a temperature equal to or higher than the storage modulus change point temperature, the gas barrier properties of the polyamide resin particles will decrease. Therefore, when the temperature of the storage modulus change point is lower than room temperature, even under relatively low temperature conditions such as room temperature, the blowing agent can be more efficiently impregnated into the CB-containing pellets. Similarly, the blowing agent can be effectively impregnated into the CB-containing pellets even in a short time. As a result, the resin particles obtained by wetting the CB-containing pellets can be easily impregnated with a large amount of blowing agent.

[0076] The resin particles may be resin particles having a single-layer structure, or may be multilayer resin particles having a multilayer structure. The multilayer structure refers to a structure having a core layer and a covering layer covering the core layer, wherein the core layer and the covering layer are made of polyamide resins having different properties. When expanded in the foaming step described below, the multilayer resin particles will produce expanded beads having a foamed core layer in a foamed state and a covering layer covering the foamed core layer. When the resin particles are multilayer resin particles, it is preferred that the melting point (Tms) of the polyamide resin constituting the coating layer is lower than the melting point (Tmc) of the core layer, and more preferably 20°C or more lower than the melting point (Tmc), because this can improve the welding properties between the expanded beads while maintaining heat resistance. In order to suppress the peeling between the covering layer and the core layer, [(Tmc)-(Tms)] is preferably 40°C or less. In addition, in order to improve the welding properties, it is also preferred that the covering layer of the expanded beads is in a non-foamed state. The non-foamed state may include a state in which the cells have disappeared after foaming and a state in which the cells are partially present in the layer.

[0077] Multilayer resin particles can be manufactured by using multilayer CB-containing pellets. Multilayer CB-containing pellets can be obtained by conventional methods. For example, in the above-mentioned CB-containing pellet manufacturing step (a), polyamide resin, carbon black and optional components blended as needed are melt-kneaded in the first extruder to form a core layer forming melt, and a cover layer forming melt is prepared in the second extruder. Then, these melts are introduced into a third extruder equipped with a die head for forming a double-layer strip, where they are merged in the die head. The combined stream is extruded through the small hole of the fixture attached to the extruder tip in the form of a strip with two layers, and the extruded strip is cut.

[0078] The ratio of the length L of the resin particles to the diameter D of the resin particles (aspect ratio L / D) is preferably 1.1 or more, more preferably 1.2 or more. When the aspect ratio L / D of the resin particles is within this range, the impregnation efficiency of the inorganic physical foaming agent in the gas phase can be further improved in the foaming agent impregnation step described below. The upper limit of the aspect ratio L / D is 2.5, more preferably 2.0, and still more preferably 1.5, because the resultant can be efficiently filled into the mold in the in-mold molding of the expanded beads, which will be described below.

[0079] The aspect ratio L / D of the resin particles can be determined as follows. Use, for example, a caliper to measure the maximum length L of each resin particle of 50 randomly selected resin particles obtained in the wetting step and the maximum width D of the resin particles in a direction perpendicular to the direction of the maximum length L, and calculate the ratio L / D. The arithmetic mean of the L / D values ​​of these 50 resin particles is defined as the aspect ratio of the resin particles. The maximum length L of the resin particles is generally about 1.5 to 2.1 mm, preferably 1.6 to 1.8 mm.

[0080] Incidentally, the aspect ratio L / D of the resin pellets is almost the same as that of the CB-containing pellets. Therefore, in the CB-containing pellet manufacturing step, the aspect ratio of the resin pellets can be controlled by adjusting the discharge speed of the kneaded melt extruded from the small holes of the die head, the winding speed of the strip, etc.

[0081] Blowing agent impregnation step (c):

[0082] In the blowing agent impregnation step (c), resin particles having a moisture content of 2.5% by mass or more and a carbon black content of 0.5 to 10% by mass are impregnated with an inorganic physical blowing agent (hereinafter also simply referred to as a blowing agent).

[0083] The expandable particles obtained by impregnating the resin particles with the blowing agent according to the method of the present invention are fully impregnated with the blowing agent into the inside thereof. Therefore, by heating the expandable particles using a heating medium such as hot air or an oil bath, expanded beads having a high content of closed cells, uniformly distributed closed cells therein, and a low apparent density can be obtained. In addition, even when steam is used as a heating medium to expand the expandable particles, expanded beads with a low apparent density can be obtained.

[0084] In the blowing agent impregnation step (c), the resin particles are placed in, for example, a pressure-resistant container, and the blowing agent is injected under pressure to impregnate the resin particles with the blowing agent in a gas phase to obtain expandable particles.

[0085] Examples of the blowing agent include carbon dioxide, nitrogen, helium, argon and air. Among them, carbon dioxide or air is preferred, and carbon dioxide is more preferred because it has little impact on the environment, is non-flammable and is excellent in safety.

[0086] The impregnation efficiency of the above-described blowing agent into the resin particles is strongly affected by the impregnation temperature, the moisture content of the resin particles, and the carbon black content of the resin particles.

[0087] In the blowing agent impregnation step (c), the resin particles are preferably impregnated with the blowing agent at a temperature higher than the temperature of the storage modulus change point (hereinafter also referred to simply as the change point temperature). That is, in the blowing agent impregnation step (c), the temperature in the pressure-resistant container in which the impregnation is performed is preferably set higher than the temperature of the storage modulus change point of the resin particles, because this will improve the impregnation efficiency of the blowing agent.

[0088] That is, the storage modulus changing point temperature (hereinafter also simply referred to as the changing point temperature) measured by the dynamic viscoelasticity measurement of the resin particles can be suitably used as an index for setting the impregnation temperature in the blowing agent impregnation step (c).

[0089] Figure 1 A graph is drawn to show the relationship between the moisture content and the change point temperature, wherein the horizontal axis represents the moisture content of the film made of the resin particles and the vertical axis represents the change point temperature. Figure 1 As shown in , the higher the moisture content of the resin particles, the lower the change point temperature. In addition, at a temperature higher than the change point temperature, the gas barrier properties of the resin particles decrease. Therefore, if the temperature is higher than the change point temperature of the resin particles, the gas barrier properties of the resin particles will decrease, so that the foaming agent can be more efficiently impregnated into the resin particles.

[0090] By the way, according to the dynamic viscoelasticity measurement using dynamic mechanical analysis (DMA), in addition to the storage modulus, the elastic loss modulus and the loss tangent can also be determined. Among these physical property values, the change point temperature of the storage modulus is the lowest temperature at which the molecular motion of the resin material to be measured begins to change (elastic modulus change). When the temperature is higher than the change point temperature, the foaming agent can be fully impregnated into the resin particles at low temperatures (e.g., room temperature) and / or in a short time. Therefore, in the present invention, the storage modulus change point temperature of the resin particles is used as an indicator for determining the lower limit temperature at which the foaming agent can be efficiently impregnated into the resin particles.

[0091] The changing point temperature of the resin particles refers to the storage modulus changing point temperature (glass transition temperature determined from a storage modulus versus temperature curve) determined by dynamic mechanical analysis (DMA) according to JIS K7095 (2012).

[0092] Since it is difficult to use resin particles as samples for DMA, the resin particles are formed into film samples. The relationship expression between the change point temperature and the moisture content of the film sample is determined by DMA measurement, and the change point temperature of the resin particles is calculated based on the relationship expression. That is, the change point temperature of the resin particles is determined as follows. CB-containing pellets are used-the resin particles to be measured are prepared therefrom. The CB-containing pellets are divided into multiple groups. These groups of CB-containing pellets are wetted under different conditions to obtain multiple groups of resin particles with different moisture contents. Each group of resin particles is formed into a film with different moisture content. The moisture content and storage modulus of each film are measured. Based on the measurement results obtained, the relationship between the moisture content and the change point temperature is plotted, wherein the horizontal axis is the moisture content and the vertical axis is the change point temperature (for example, Figure 1 ). Next, the relationship expression established between the moisture content and the change point temperature is determined using the graph. On the other hand, the moisture content of the resin particles whose change point temperature is to be determined is measured. From the obtained measurement value, the change point temperature of the resin particles is determined by calculation using the relationship expression.

[0093] More specifically, the relationship between the moisture content of the resin particles and the temperature of the change point of the target resin particles is determined as follows. Use a hot press heated to 210°C to compress the multiple groups of resin particles with different moisture contents obtained as described above to obtain films with different moisture contents and sizes of 100 mm long, 100 mm wide and 0.4 mm thick. Film sample S1 (length 40 mm, width 50 mm, thickness 0.4 mm) for measuring moisture content and film sample S2 (length 40 mm, width 5 mm, thickness 0.4 mm) for measuring storage modulus are cut from each film. The moisture content of each film sample S1 is measured by the method described above. The storage modulus of each film sample S2 is measured as follows. The film sample S2 is fixed with a clamp, and the temperature is raised from -80°C to 130°C at a rate of 2°C / min in tension mode at a constant frequency (1 Hz), and its storage modulus is measured at the same time. Then, the measurement results are plotted with the vertical axis as the storage modulus and the horizontal axis as the temperature to obtain a temperature-storage modulus curve A, as shown in FIG. Figure 2 As the DMA apparatus, for example, a viscoelasticity measuring apparatus DMA7100 manufactured by Hitachi High-Tech Science Co., Ltd. can be used.

[0094] exist Figure 2 In the curve graph, the straight line L1 extending from the straight line portion before the first sudden drop in the storage modulus to the high temperature side intersects with the straight line L2 extending to the low temperature side after the first sudden drop in the storage modulus at the intersection B. The temperature of the intersection B is defined as the change point temperature of the storage elastic modulus. When multiple change point temperatures appear, the change point temperature on the lowest temperature side is adopted. DMA measurement is performed on 10 samples S2 obtained from a film with the same moisture content, and the arithmetic mean of the 10 temperature change measurement values ​​obtained is taken as the storage modulus change point temperature of the film.

[0095] The above measurements were performed on a plurality of films having different water contents, and the change point temperature was determined for each film. The change point temperature was plotted as a function of the water content. Figure 1 An example of a graph showing the relationship between moisture content and change point temperature is shown, wherein moisture content is plotted on the horizontal axis and change point temperature is plotted on the vertical axis. A relationship expression between moisture content and change point temperature is determined based on the graph. The change point temperature of the desired resin particles is determined by measuring the moisture content of the desired resin particles and calculating from the obtained moisture content value using the relationship expression.

[0096] Next, the relationship between the water content and the impregnation efficiency of the foaming agent will be described. The higher the water content of the resin particles, the higher the impregnation efficiency of the foaming agent. Moreover, the higher the water content of the resin particles, the lower the change point temperature of the resin particles. Therefore, the resin particles can be efficiently impregnated with the foaming agent even at low temperatures, or the time for impregnating the resin particles with the foaming agent can be shortened without raising the temperature. From this point of view, the water content of the resin particles is preferably 3.0% by mass or more, as described above.

[0097] On the other hand, the moisture content of the resin particles is not particularly limited. However, the upper limit of the moisture content is generally 20% by mass because as the moisture content increases, the degree of decrease in the change point temperature decreases and reaches an equilibrium state, such as Figure 1 In addition, since blocking easily occurs in the foaming step as the water content increases, the upper limit of the water content is preferably 18% by mass or less, as described above.

[0098] The reason why the storage modulus change point temperature decreases as the moisture content of the resin particles increases is believed to be that the presence of water molecules weakens the intermolecular interaction caused by hydrogen bonding between molecules of the polyamide resin, and thus the molecular motion of the polyamide resin changes.

[0099] In the blowing agent impregnation step (c), the temperature inside the pressure-resistant container is preferably adjusted to a value higher than the storage modulus change point temperature of the resin particles, as described above. In addition, in order to more efficiently impregnate the resin particles with the blowing agent, it is preferred that the temperature inside the pressure-resistant container is adjusted to a value higher than the change point temperature of the resin particles for more than 50% of the total time of the blowing agent impregnation step. As used herein, the term "total time of the blowing agent impregnation step" refers to the time from the start of the blowing agent impregnation step to the completion of the removal of the expandable particles from the pressure-resistant container.

[0100] In addition, the term "start of the blowing agent impregnation step" refers to the time point when the state in which the water content of the resin particles loaded into the pressure-resistant container reaches 2.5% by mass or more and the state in which the blowing agent is injected into the pressure-resistant container are both established for the first time. In this case, either the time point in which the water content of the resin particles reaches 2.5% by mass or more or the time point in which the blowing agent is injected can occur first. Specifically, for example, the blowing agent can be injected after the resin particles having a water content of 2.5% by mass or more have been loaded into the pressure-resistant container. Alternatively, the resin particles having a water content of less than 2.5% by mass can be first loaded into the pressure-resistant container, and after the inorganic physical blowing agent is injected into the pressure-resistant container, a treatment to increase the water content of the resin particles in the pressure-resistant container to 2.5% by mass or more can be performed at any time. "The time exceeding 50% of the total time of the blowing agent impregnation step" can be a continuous time during the entire implementation period or the sum of the intermittent time.

[0101] In order to more efficiently impregnate a larger amount of blowing agent, it is preferred that the temperature in the pressure vessel during the blowing agent impregnation step be maintained above the storage modulus change point temperature of the resin particles for more than 70% of the total impregnation time, more preferably more than 80%, particularly preferably more than 90%, and most preferably substantially 100%.

[0102] During a time period exceeding 50% of the total impregnation time of the above-mentioned blowing agent impregnation step, the temperature in the pressure-resistant container may be adjusted to a constant value or may be changed. Incidentally, during the blowing agent impregnation step, the moisture content of the resin particles may change over time, so that the change point temperature may change accordingly. Therefore, the change point temperature of the resin particles, which is an index for setting the temperature in the pressure container, will change with the change in the moisture content of the resin particles in the pressure container. Therefore, it is preferable to sample the resin particles from the pressure-resistant container during the blowing agent impregnation step and measure the moisture content thereof as needed, and it is preferable to determine the change point temperature based on the measured moisture content and adjust the temperature in the pressure-resistant container to be equal to or higher than the change point temperature.

[0103] As described above, the change point temperature of the resin particles in the wet state is lower than the change point temperature of the resin particles in the dry state. Therefore, compared with the case of using the resin particles in the dry state, the blowing agent impregnation step (c) in the method of the present invention can be performed at a lower temperature and / or in a shorter time. As a result, the load on the device such as the pressure-resistant container can be reduced and the productivity can be improved. In addition, the discoloration due to the deterioration of the resin can be suppressed.

[0104] The temperature in the pressure-resistant container in the blowing agent impregnation step is not particularly limited, but as described above, it is preferable to impregnate the blowing agent at a temperature higher than the changing point temperature of the resin particles. In order to easily manage the impregnation temperature, it is preferable to impregnate the resin particles with the blowing agent at a temperature higher than the changing point temperature of the resin particles at the beginning of the blowing agent impregnation step.

[0105] Furthermore, during the foaming agent impregnation step, the moisture content of the resin particles in a wet state in the pressure-resistant container may gradually decrease, so that the change point temperature of the resin particles tends to increase. To cope with this, the temperature in the pressure-resistant container may be set high in advance at the start of the foaming agent impregnation process, so that even if the change point temperature increases, the resin particles can be sufficiently impregnated with the inorganic physical foaming agent without any particular problem. Furthermore, the impregnation efficiency of the foaming agent can be further improved, and thus the impregnation time of the foaming agent can be shortened and the impregnation amount of the foaming agent can be increased.

[0106] More specifically, the impregnation temperature of the blowing agent is more preferably equal to or higher than a temperature 10°C higher than the temperature at the change point at the start of the blowing agent impregnation step, still more preferably equal to or higher than a temperature 25°C higher than the temperature at the change point at the start of the blowing agent impregnation step, still still more preferably equal to or higher than a temperature 30°C higher than the temperature at the change point at the start of the blowing agent impregnation step, and particularly preferably equal to or higher than a temperature 45°C higher than the temperature at the change point at the start of the blowing agent impregnation step. On the other hand, in order to reduce the load on the pressure-resistant container and the like, the temperature of the blowing agent impregnation step is preferably equal to or lower than a temperature 100°C higher than the temperature at the change point at the start of the blowing agent impregnation step, more preferably equal to or lower than a temperature 80°C higher than the temperature at the change point at the start of the blowing agent impregnation step, still more preferably equal to or lower than a temperature 75°C higher than the temperature at the change point at the start of the blowing agent impregnation step, and particularly preferably equal to or lower than a temperature 70°C higher than the temperature at the change point at the start of the blowing agent impregnation step.

[0107] In the present invention, it is most preferred that the temperature in the pressure-resistant container in the blowing agent impregnation step is set to be at least 30° C. higher than the change-point temperature at the start of the blowing agent impregnation step for more than 50% of the total execution time of the blowing agent impregnation step. For example, when the change-point temperature of the resin particles at the start of the blowing agent impregnation step is -10° C., it is preferred that the temperature in the pressure-resistant container during the blowing agent impregnation process is set to 20° C. or higher and maintained at 20° C. or higher for more than 50% of the total execution time of the blowing agent impregnation process.

[0108] In the present invention, at the initial stage of the blowing agent impregnation step, it is more preferred to adjust the temperature in the pressure vessel to a temperature higher than the storage modulus change point temperature of the resin particles in a wet state. As used herein, the initial stage of the blowing agent impregnation step refers to the time from the start to the time when 5% of the total implementation time of the blowing agent impregnation step has passed, preferably to the time when 3% has passed, more preferably to the time when 1% has passed, and most preferably to the time when the blowing agent impregnation step starts.

[0109] Furthermore, it is more preferred to start the impregnation of the inorganic physical foaming agent at a temperature 30° C. or higher than the change point temperature at the beginning of the foaming agent impregnation step, and to continue to maintain this temperature until the final stage of the foaming agent impregnation step. As used herein, the final stage of the foaming agent impregnation step refers to the time from the start of the total time of the foaming agent impregnation step when 95% to 100% has passed, preferably when 97% to 100% has passed, and more preferably when 99% to 100% has passed.

[0110] The upper limit of the temperature in the blowing agent impregnation step is not particularly specified, and can be determined in consideration of the relationship with other conditions such as the moisture content of the resin particles and the blowing agent impregnation time. However, from the viewpoint of reducing the load on the apparatus and suppressing discoloration due to resin degradation, the impregnation temperature in the blowing agent impregnation step is preferably 150° C. or lower, more preferably 120° C. or lower, even more preferably 100° C. or lower, still even more preferably 80° C. or lower, particularly preferably 50° C. or lower, and most preferably 30° C. or lower.

[0111] Next, the pressure in the pressure-resistant container during the foaming agent impregnation step will be described. As the foaming agent is injected, the pressure in the pressure-resistant container in which the resin particles are loaded will increase. As a result, the resin particles are impregnated with the foaming agent. The relationship between the injection of the foaming agent and the temperature regulation in the pressure-resistant container is not particularly limited. The injection of the foaming agent and the temperature regulation may be started at the same time, or either one may be started first. The temperature regulation may be started first, and the injection of the foaming agent may be started after the temperature reaches a predetermined temperature. Incidentally, the rate of increase of the pressure of the foaming agent injected into the pressure-resistant container is not particularly limited.

[0112] As the foaming agent is injected, the pressure in the pressure container increases. The pressure in the pressure container is not particularly limited, but is preferably in the range of 2.0 MPa (G) or more and 6.0 MPa (G) or less, and more preferably in the range of 3.0 MPa (G) or more and 5.0 MPa (G) or less. It is preferred that the pressure in the pressure container is kept constant throughout the foaming agent impregnation step. However, the pressure in the pressure container may vary.

[0113] As a result of the blowing agent impregnation step (c), expandable resin particles which are foamable by heating are obtained.

[0114] In the blowing agent impregnation step, the blowing agent may be impregnated into the resin particles in a gaseous state or in a liquid state. However, from the perspective of further improving the impregnation efficiency of the blowing agent, it is preferred that part or all of the blowing agent is impregnated into the resin particles in a gaseous state. It is more preferred that all of the blowing agent is impregnated into the resin particles in a gaseous state. Furthermore, from the perspective of ensuring that the blowing agent remains in a gaseous state to further improve the impregnation efficiency into the resin particles, it is preferred that the blowing agent is preheated to a temperature equal to or higher than the impregnation temperature and then injected into the pressure-resistant container.

[0115] (d) Foaming step

[0116] The foaming step is a step of heating and foaming the expandable particles obtained in the above-mentioned blowing agent impregnation step to obtain polyamide-based resin expanded beads. The foaming step (d) is preferably performed as soon as possible after the above-described blowing agent impregnation step (c).

[0117] The method for heating the expandable particles is not particularly limited. For example, a method in which the expandable particles are heated by supplying high-temperature air (hot air foaming), a method in which the expandable particles are heated by immersing them in high-temperature oil (oil bath foaming), and a method in which the expandable particles are heated by feeding steam (steam foaming) can be mentioned. In addition, high-frequency waves and infrared rays, for example, can be used to heat the expandable particles. By heating the expandable particles using hot air or an oil bath, polyamide resin expanded beads having low apparent density and uniform closed cells formed throughout the beads can be obtained. Since such expanded beads are easier to obtain, the temperature of the hot air supplied during hot air foaming is preferably 180 to 300°C, more preferably 200 to 280°C, and even more preferably 220 to 250°C. In addition, for the same reason, based on the melting point of the polyamide resin constituting the resin particles, the temperature of the hot air supplied during hot air foaming is preferably between a temperature of 10°C higher than the melting point and a temperature of 100°C higher than the melting point, and more preferably between a temperature of 20°C higher than the melting point and a temperature of 80°C higher than the melting point.

[0118] In the past, when attempting to produce expanded beads by supplying steam as a heating medium to expandable particles, the foaming itself was sometimes difficult. On the other hand, according to the present invention, even when steam is used as a heating medium, expanded beads having a low apparent density can be produced. From the viewpoint of the ability to more easily obtain such expanded beads, the temperature of the steam supplied in the steam foaming is preferably 100 to 180° C., more preferably 120 to 150° C.

[0119] The foaming step may be performed under pressure. The pressure in this case is not particularly limited, but may be adjusted, for example, within a range of about 0.03 to 0.4 MPa. In addition, the heating time may be, for example, within a range of 5 to 120 seconds.

[0120] The expanded beads of the present invention have a plurality of cells and are composed of a polyamide-based resin and carbon black, wherein the carbon black is contained in an amount of 0.5% by mass or more and 10% by mass or less based on 100% by mass of the expanded beads. 3 Up to 800kg / m 3 The invention has an apparent density of , a closed cell content of more than 80%, an average cell diameter D of all cells thereof and an average cell diameter Dc in its central region, wherein Dc / D is 0.7 to 1.3.

[0121] The apparent density of the expanded beads is 800kg / m 3 Below, more preferably 750kg / m 3 Below, more preferably 600kg / m 3 Below, still more preferably 550kg / m 3 Below, particularly preferably 500kg / m3 By molding such expanded beads in a mold, a polyamide resin expanded beads molded product having excellent lightness can be obtained. The lower limit of the apparent density of the obtained expanded beads is not particularly limited, but is generally 100 kg / m 3 , preferably 200kg / m 3 , and more preferably 300 kg / m 3 By further applying internal pressure to the expanded beads and heating them to further reduce their weight, expanded beads having an even lower apparent density (secondary expanded beads) can be produced.

[0122] The apparent density of the expanded beads is measured by the following method. 3 The expanded beads of which the weight Wp has been measured are sampled and their weight Wp is measured. The expanded beads whose weight Wp has been measured are immersed in a measuring cylinder filled with water at a temperature of 23°C using a wire mesh. Taking the volume of the wire mesh into account, the volume Vp [cm 3 ]. Divide the weight Wp [g] of the expanded beads by the volume Vp (Wp / Vp) and convert the unit appropriately to [kg / m 3 The expanded beads for measurement were aged in an oven at 80°C for 12 hours and then slowly cooled to a dry state.

[0123] Preferably, the closed cell content of the expanded beads of the present invention is 70% or more, more preferably 80% or more. When the closed cell content falls within this range, the formability of the expanded beads becomes better, and therefore, the expanded beads molded product obtained by molding the expanded beads in a mold has excellent surface properties and welding properties.

[0124] The closed cell content can be determined using an air comparative pycnometer based on Procedure C described in ASTM-D2856-70. The expanded beads used for measurement were aged in an oven at 80°C for 12 hours and then slowly cooled to a dry state.

[0125] The average cell diameter D of the expanded beads of the present invention is preferably 50 to 300 μm, more preferably 80 to 250 μm, still more preferably 100 to 200 μm, from the viewpoint of formability of the expanded beads.

[0126] The average cell diameter D of the expanded beads can be determined as follows. First, cut one of the expanded beads into two almost equal halves so that the cut surface passes through its approximate center. Take one of the cross sections with a scanning electron microscope so that the cross section appears completely in the photograph. On the captured image, draw eight line segments that extend radially from the center of the captured image to its periphery and are spaced almost equiangularly from each other (the spacing angle is close to 45 degrees). Then count the total number of cells intersecting with these eight line segments and measure the total length of these eight line segments. Divide the measured total length by the total number of cells counted to obtain the cell diameter of the expanded beads. Repeat a similar procedure for 10 randomly selected expanded beads. The arithmetic mean of the cell diameters of these ten expanded beads is defined as the average cell diameter D of the expanded beads.

[0127] It is also preferred that the ratio of the average cell diameter Dc at the central region of the expanded beads to the average cell diameter D of the expanded beads (Dc / D) is preferably 0.7 to 1.3, more preferably 0.8 to 1.2. The fact that the ratio (Dc / D) falls within this range means that a uniform cell structure is formed throughout the expanded beads.

[0128] The average cell diameter Dc of the cells located in the central area of ​​the expanded beads can be determined as follows. First, one of the expanded beads is cut into two almost equal halves so that the cut surface passes through its central portion. One of the cross sections is photographed with a scanning electron microscope so that the cross section appears completely in the photograph. On the photographed image, the shortest line segment is drawn from the approximate center point of the image to the periphery (cell membrane) of each cell located near the center point. Among the cells present near the center, 10 cells are selected in the order of the minimum value of the shortest line from the approximate center to the periphery. Next, a rectangle is drawn that circumscribes each of the 10 selected cells, and the short and long sides of each rectangle are measured and averaged to obtain the cell diameter of each cell. The cell diameters of the ten selected cells are averaged to obtain the cell diameter of the cells located in the central area of ​​the expanded beads. A similar procedure is repeated for 10 randomly selected expanded beads. The arithmetic mean of the cell diameters of the cells located in the central area of ​​these ten expanded beads is defined as the average cell diameter Dc of the cells located in the central area of ​​the expanded beads.

[0129] By heating the expandable particles produced by the method of the present invention with hot air or an oil bath as a heating medium, expanded beads having a closed cell content of more than 80% and a Dc / D ratio of 0.7 to 1.3 can be easily obtained.

[0130] The expanded beads of the present invention can be used to manufacture polyamide resin expanded beads molded products (hereinafter also referred to as expanded beads molded products or molded products). In the molded product, a plurality of the expanded beads of the present invention are fused to each other. The method for manufacturing the molded product is not particularly limited, and a generally known method can be used. For example, in-mold molding can be mentioned as a preferred method for manufacturing molded products. Particularly preferred is the in-mold molding method using steam. According to this method, the polyamide resin constituting the expanded beads is plasticized with steam, and therefore, the molding pressure during in-mold molding can be reduced. The obtained molded product has excellent lightness and high heat resistance.

[0131] In the in-mold forming method, any known method can be adopted as a method for filling expanded beads into a mold. For example, the following methods can be used: a method in which the expanded beads are pressurized with pressurized gas to apply a predetermined internal pressure to the cells thereof while preventing the secondary expansion force of the expanded beads from excessively increasing in consideration of the weldability of the expanded beads in the expanded beads molded product (pressure pretreatment forming); a method in which the expanded beads compressed with pressurized gas are filled into a mold in a pressurized mold, and then the pressure in the mold is released (compression filling); and a method in which the mold is opened in advance before the expanded beads are filled into the mold to increase the forming space, and the mold is closed after the expanded beads are filled into the mold to mechanically compress the expanded beads (cracking filling).

[0132] The molded article obtained from the expanded beads of the present invention has high heat resistance, excellent wear resistance, chemical resistance, and also has excellent tensile strength and welding properties between the expanded beads. Therefore, the molded article can be advantageously used as, for example, automobile parts and electrical products.

[0133] Example

[0134] The following non-limiting examples will further illustrate the present invention.

[0135] Examples 1 to 4 and Comparative Examples 1 to 4

[0136] CB-containing pellets manufacturing steps (a):

[0137] As a polyamide resin, a polyamide 6 / 66 copolymer (polyamide 6 / polyamide 66 = 85 / 15; "UBE Nylon 5033B" manufactured by Ube Industries, Ltd., melting point 197° C., density 1,140 kg / m 3, flexural modulus 1,300 MPa, MFR 3.5 g / 10 min), 5.6 mass % of a masterbatch (the base resin is an acrylonitrile-styrene copolymer; the carbon black content in the masterbatch is 45 mass %), 8,000 ppm by mass of "Talcan Powder PK-S" (manufactured by Hayashi Kasei Co., Ltd.) as a cell control agent, and 10,000 ppm by mass of "Stabaxol P" (manufactured by Rhein Chemie Inc.) as a terminal blocking agent were fed into an extruder and melt-kneaded. The kneaded mixture was extruded from the extruder in the form of strands. After cooling in water, the strands were cut with a pelletizer so that l / d was 1.2, and dried to obtain pellets each having an average weight of 2 mg. The obtained pellets were dried at a temperature of 100° C. and a humidity of 23% for 12 hours to obtain CB-containing pellets (resin pellets in a dry state) containing 2.5% by weight of carbon black. In Comparative Examples 2 and 3, carbon black was not added.

[0138] Melting point determination of polyamide resin:

[0139] The polyamide resin is placed in a dryer to avoid hydrolysis under high temperature and high humidity conditions, and is evacuated under a nitrogen atmosphere to reduce the moisture content to less than 1000ppm by mass. The obtained polyamide resin is used as a measurement sample. According to JIS K7121 (1987), a differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nanotechnology Inc.) is used to measure the melting point of the polyamide resin according to the aforementioned method. Specifically, according to the heat flux differential scanning calorimetry, the sample is heated and melted from 30°C at a heating rate of 10°C / min to a temperature 30°C higher than the melting peak end temperature (the first temperature increase), then kept at this temperature for 10 minutes, cooled to 30°C at a cooling rate of 10°C / min, and heated again to a temperature 30°C higher than the melting peak end temperature at a heating rate of 10°C / min to obtain a second DSC curve. The temperature at the melting peak vertex of the obtained DSC curve (melting peak temperature) is determined as the melting point of the polyamide resin.

[0140] Wetting step (b):

[0141] The CB-containing pellets obtained in the above step (a) were wetted as raw materials in different ways shown below to obtain resin pellets having the moisture content shown in Tables 1 and 2. That is, in Examples 1, 3 and 4, the wetting was performed by completely immersing the CB-containing pellets in 15°C water contained in a container for the time shown in Tables 1 and 2 (the aforementioned third wetting method). In Example 2 and Comparative Example 3, the wetting was performed by allowing the CB-containing pellets to stand for the time shown in Table 1 under the conditions of a temperature of 23°C and a relative humidity of 50% (the aforementioned first wetting method). In Comparative Examples 1, 2 and 4, the wetting was performed by allowing the CB-containing pellets to stand for the time shown in Tables 1 and 2 under the conditions of a temperature of 80°C and a relative humidity of 23%. The moisture content of the obtained resin pellets was measured. In addition, based on the moisture content value obtained, the change point temperature of its storage modulus was calculated from the relational expression shown below. The results are as shown in Tables 1 and 2.

[0142] Blowing agent impregnation step (c):

[0143] Resin particles (180 g) having a moisture content shown in Tables 1 and 2 are fed into a pressure-resistant container having a capacity of 3 L and set at an impregnation temperature shown in Tables 1 and 2. Tables 1 and 2 also show the difference between the impregnation temperature and the storage modulus change point temperature of the resin particles (impregnation temperature-change point temperature). While closing the pressure-resistant container containing the resin particles, carbon dioxide as a foaming agent is injected to impregnate the resin particles with the foaming agent at the impregnation temperature shown in Tables 1 and 2. The pressure of carbon dioxide as a foaming agent in the pressure-resistant container (foaming agent impregnation pressure) is kept constant at 4.0 MPa (G). Tables 1 and 2 show the impregnation time (the time from the injection of the foaming agent to the removal of the resin particles impregnated with the foaming agent from the pressure-resistant container). The impregnation temperature is kept constant at the temperature shown in Tables 1 and 2. The expandable particles impregnated with carbon dioxide are taken out from the pressure-resistant container immediately after the impregnation time shown in Tables 1 and 2.

[0144] Foaming step (d):

[0145] Using expandable particles impregnated with carbon dioxide as a foaming agent, expanded beads are manufactured as follows. In Examples 1 to 3 and Comparative Examples 1 to 3, 180 g of expandable particles impregnated with carbon dioxide are foamed and expanded by blowing hot air at the temperature shown in Table 1 as a heating medium for the time shown in Table 1 to obtain expanded beads. The resulting expanded beads are aged in an oven at 80°C for 12 hours, and then slowly cooled to obtain expanded beads in a dry state. In Example 4 and Comparative Example 4, steam is used instead of hot air. That is, steam at the temperature shown in Table 2 is blown onto the expandable particles as a heating medium for the time shown in Table 2 to foam them.

[0146] In Examples 1 to 3 and Comparative Examples 1 to 3, the change point temperature and L / D of the resin particles were measured, and the apparent density, expansion ratio, closed cell content, average cell diameter D, and cell diameter Dc at the center of the expanded beads in the dry state obtained by hot air foaming were measured. The results are shown in Table 1. In addition, the appearance of the expanded beads obtained in Examples 1 to 3 was observed. The evaluation results are shown in Table 1. The expanded state of the expanded beads obtained in Comparative Examples 1 and 2 was extremely poor and had many unexpanded parts. Therefore, the average cell diameter was difficult to measure, so it was not measured. In addition, the appearance of the expanded beads obtained in Comparative Examples 1 to 3 was not evaluated.

[0147]

[0148] Furthermore, the apparent density and expansion ratio of the expanded beads in a dry state obtained by steam foaming as described above were measured in Example 4 and Comparative Example 4. The results are shown in Table 2.

[0149] Table 2

[0150]

[0151] In Table 1, the physical properties of the polyamide-based resin particles and the polyamide-based resin expanded beads were measured by the following methods.

[0152] Aspect ratio of resin particles L / D:

[0153] The maximum length L and the maximum width D in the direction perpendicular to the maximum length L of each of 50 randomly selected resin particles obtained in the wetting step were measured with a caliper, and the ratio L / D was calculated. The arithmetic mean of the L / D values ​​of these 50 resin particles was taken as the aspect ratio of the resin particles.

[0154] Moisture content of resin particles:

[0155] The moisture content of the resin particles is measured using a halogen moisture meter. As a measuring device, a "halogen moisture meter (HX204) manufactured by METTLER TOLEDO" is used, which measures the moisture content based on halogen lamp heating. The measurement is carried out according to the method described above. Specifically, first, about 2.0g of resin particles are sampled. The water attached to the surface of the resin particles is removed by wiping with a Kimwipe manufactured by Nippon Paper Crecia Co., Ltd. to obtain a measurement sample. The weight of the sample is measured and placed in a halogen moisture meter. The sample is then heated to a temperature of 100°C and maintained at 100°C for 60 seconds until the weight no longer changes. The sample is further heated to 160°C and maintained at 160°C for 90 seconds until the weight no longer changes. The weight of the dry sample is measured. Based on the weight of the sample before heating, the percentage of weight loss of the sample due to heating is defined as moisture content (%). In addition to the weight of the sample being 0.5g, the moisture content of the polyamide film described later is determined in the same manner as the moisture content of the polyamide resin particles.

[0156] The method for measuring the temperature of the storage modulus change point of the resin pellets is changed:

[0157] With reference to JIS K7095 (2012), the temperature of the storage modulus change point of the resin particles is measured by dynamic mechanical analysis (DMA). As a DMA measuring device, a viscoelasticity measuring device DMA7100 manufactured by Hitachi High-Tech Science Co., Ltd. is used. The CB-containing pellets obtained in the above step (a) are moistened in various ways to obtain four groups of resin particles with different moisture contents. Each group is compressed with a hot press heated to 210°C to obtain four polyamide films with a length of 100mm, a width of 100mm, and a thickness of 0.4mm. From each polyamide film, a film sample S1 (length 40mm x width 50mm x thickness 0.4mm) is cut for determining the moisture content of the polyamide film and ten film samples S2 (length 40mm x width 5mmx thickness 0.4mm) are used to determine the temperature of the storage modulus change point of the polyamide film. The moisture content of the film sample S1 is measured by the method described above. On the other hand, each film sample S2 is fixed with a fixture of the viscoelasticity measuring device. DMA measurements were performed in tension mode at a constant frequency (1 Hz) by increasing the temperature from -80°C to 130°C at a rate of 2°C / min. Figure 2 As shown in FIG. , the measurement results are plotted with the vertical axis being the storage modulus and the horizontal axis being the temperature, resulting in a graph A showing the relationship between temperature and storage modulus. Figure 2In the above, the temperature at the intersection B between the straight line L1 extending from the straight line portion before the first sudden decrease in storage modulus to the high temperature side and the straight line L2 extending to the low temperature side after the first sudden decrease in storage modulus is taken as the temperature of the storage modulus change point. The above procedure is performed for 10 film samples S2, and the arithmetic mean of the obtained change point temperatures is defined as the temperature of the storage modulus change point of the corresponding polyamide film.

[0158] The above-mentioned change point temperature was measured for four polyamide films made of four resin particle groups having different moisture contents. A graph showing the relationship between moisture content and the change point of storage modulus was formed by plotting the measured values ​​of moisture content of the polyamide film on the horizontal axis and the measured values ​​of storage modulus on the vertical axis. The resulting graph is shown in FIG. Figure 1 From Figure 1 The following relational expression (1) was determined. Then, based on the moisture content values ​​of the resin particles of Examples 1 to 4 and Comparative Examples 1 and 4, the change point temperature of the storage modulus was calculated using the relational expression (1).

[0159] Y = -0.115x 3 +3.1758x 2 -29.636x + 57.014 (1)

[0160] in

[0161] y: Change point temperature of storage modulus of polyamide resin pellets (°C)

[0162] x: moisture content of polyamide resin particles (%).

[0163] For the storage modulus change point temperature of the resin particles not containing carbon black, the relationship expression (2) between the moisture content and the change point of the storage modulus is also obtained in the same manner as above. Then, based on the moisture content values ​​of the resin particles of Comparative Examples 2 and 3, the change point temperature of the storage modulus is calculated using the relationship expression (2).

[0164] Y = -0.089x 3 +2.3776x 2 - 23.146x + 49.619 (2)

[0165] Apparent density of expanded beads:

[0166] The measurement was performed by the method described above. Specifically, the expanded beads were first aged in an oven at 80°C for 12 hours and then slowly cooled to dry. 3The dried expanded beads are sampled and their weight Wp [g] is measured. The expanded beads are immersed in a measuring cylinder filled with water at a temperature of 23°C using a wire mesh. Taking the volume of the wire mesh into account, the volume of the expanded beads Vp [cm 3 The weight Wp of the expanded beads is divided by their volume Vp (Wp / Vp) and the unit is converted to [kg / m 3 ] to calculate the apparent density of the expanded beads.

[0167] Expansion ratio of expanded beads:

[0168] The dried expanded beads are placed in a 1L graduated cylinder in a naturally sedimented state until the 1L mark is reached. The mass of the expanded beads contained (W2 [g]) is then measured. The bulk density [kg / m2] of the expanded beads is determined by dividing the mass W2 [g] by the contained volume V2 (1 [L]) (W2 / V2) and performing appropriate unit conversion. 3 Then, the density of the polyamide resin constituting the expanded beads [kg / m 3 ] divided by the bulk density [kg / m 3 ] to determine the expansion ratio [times] of the expanded beads.

[0169] Closed cell content of expanded beads:

[0170] The closed cell content was measured using an air comparative pycnometer according to Procedure C described in ASTM-D2856-70 and was determined as follows. A bulk volume of about 20 cm 3 The expanded beads in a dry state are used as measurement samples, and their apparent volume Va is accurately measured by the ethanol immersion method described below. After thoroughly drying the measurement sample whose apparent volume Va has been measured, the true volume Vx of the measurement sample is measured using Accupic II1340 manufactured by Shimadzu Corporation according to Procedure C described in ASTM-D2856-70. Then, the closed cell content is calculated based on these volume values ​​Va and Vx using (5) shown below. The average value of five samples (N=5) is taken as the closed cell content of the expanded beads.

[0171] Closed cell content (%) = (Vx-W / ρ) x 100 / (Va-W / ρ) (5)

[0172] in:

[0173] Vx is the true volume of the expanded beads measured by the above method, which corresponds to the sum of the volume of the resin constituting the expanded beads and the total volume of all closed cells in the expanded beads (unit: cm 3 ),

[0174] Va is the apparent volume of the expanded beads measured from the rise in water level when the expanded beads are immersed in ethanol in a measuring cylinder (unit: cm 3 ),

[0175] W is the weight of the sample used for measurement (unit: g), and

[0176] ρ is the density of the resin constituting the expanded beads (unit: g / cm 3 ).

[0177] Average cell diameter D of expanded beads:

[0178] The average cell diameter D is determined by the method described above. Specifically, first, an expanded bead is divided into two approximately equal halves along a plane passing through its central area, and one of the cut surfaces is photographed using a scanning electron microscope so that the entire cross section is included. Next, eight equiangularly spaced line segments (i.e., 45 degrees apart) are drawn that extend radially from the approximate center of the obtained captured image to the outer peripheral surface of the expanded bead. Then, the number of cells intersecting with these eight line segments is counted. The total length of the eight line segments is also measured. The cell diameter of the expanded beads is determined by dividing the measured total length by the number of cells counted. A similar procedure is repeated for 10 randomly selected expanded beads. The arithmetic mean of the cell diameters of these 10 expanded beads is defined as the average cell diameter D of the expanded beads.

[0179] Average cell diameter Dc in the central region of the expanded beads:

[0180] The above method is used for measurement. Specifically, first, an expanded bead is divided into two approximately equal halves along a plane passing through its central area, and one of the cut surfaces is photographed using a scanning electron microscope so that the entire cross section is included. On the photographed image, the shortest straight line is drawn from its approximate center to the periphery (cell wall) of the cells present near the center, where ten cells are selected in ascending order of the shortest line. Draw a rectangle circumscribing each of the ten selected cells. Measure the length and width of each rectangle and take the average of these values ​​as the cell diameter. Take the average of the 10 measured cells as the cell diameter at the central area of ​​the expanded bead. Perform a similar operation on 10 randomly selected expanded beads. The arithmetic mean of the cell diameters at the central area of ​​these 10 expanded beads is defined as the average cell diameter Dc in the central area of ​​the expanded beads.

[0181] Surface appearance evaluation:

[0182] The surface appearance (uniformity of color density) of the expanded beads was evaluated by a sensory test. The uniformity of color density was evaluated by assigning a score ranging from 1 (lowest score; color density non-uniformity was obvious) to 5 (highest score; color density non-uniformity was not obvious) in increments of 1, and the average score of five panelists was calculated. When the calculated average score was 3.5 or more, the surface appearance of the expanded beads was evaluated as good, and when the average score was less than 3.5, it was evaluated as poor.

[0183] Example 1 is an example in which expandable particles and expanded beads are produced using resin particles having a carbon black content of 2.5% by mass and a water content of 10.2% by mass. Since the resin particles have a changing point temperature of -37°C and contain carbon black therein, expandable particles in which a foaming agent is uniformly impregnated into the interior thereof can be obtained under the conditions of 23°C and 24 hours of impregnation. By foaming the expandable particles with hot air, expanded beads having a very good foamed state can be obtained. Figure 3 A cross-sectional photograph of the expanded bead is shown.

[0184] Example 2 is an example in which expandable particles and expanded beads are produced using resin particles having a carbon black content of 2.5% by mass and a moisture content of 3.8% by mass. Since the resin particles have a changing point temperature of -16°C and contain carbon black therein, expandable particles in which a foaming agent is uniformly impregnated into the interior thereof can be obtained under the conditions of 23°C and 24 hours of impregnation. By foaming the expandable particles with hot air, expanded beads having an excellent foamed state can be obtained.

[0185] Example 3 is an example in which expandable particles and expanded beads are produced using resin particles having a carbon black content of 2.5% by mass and a water content of 13.8% by mass. Since the resin particles have a change point temperature of -49°C and contain carbon black therein, expandable particles in which a foaming agent is uniformly impregnated inside can be obtained under the conditions of an impregnation temperature of 23°C and a time as short as 6 hours. By foaming the expandable particles with hot air, expanded beads having an excellent foamed state can be obtained.

[0186] Comparative Example 1 is an embodiment in which the carbon black content is 2.5% by mass and the water content is as low as 0.31% by mass. Since the change point temperature of the resin particles is 48°C, expandable particles that are satisfactorily impregnated with a blowing agent cannot be obtained under the conditions of 23°C and 24 hours of impregnation. When the expandable particles are expanded with hot air, the obtained expanded beads have a high apparent density and a low closed cell content. In addition, the foaming state of the expanded beads is quite poor, and therefore the average cell diameter D and the cell diameter Dc in the center portion cannot be measured. Figure 4 A cross-sectional photograph of the expanded bead is shown.

[0187] Comparative Example 2 is an example in which carbon black is not blended and the moisture content is reduced to as low as 0.18% by mass. Since the change point temperature of the obtained resin particles is 46°C, the blowing agent cannot be satisfactorily impregnated under the impregnation conditions of 23°C and 24 hours. When the expandable particles are expanded with hot air, the obtained expanded beads have a high apparent density and a low closed cell content. In addition, the foaming state is poor, and therefore the average cell diameter D and the cell diameter Dc in the center portion cannot be measured.

[0188] Comparative Example 3 is an example in which expandable particles and expanded beads are manufactured using resin particles having a moisture content of 4.3% by mass and containing no carbon black. The change point temperature of the resin particles is -13°C. Expandable particles are obtained by impregnating the resin particles with a blowing agent under the conditions of 23°C and 24 hours of impregnation. Expanded beads can be obtained by foaming the expandable particles with hot air. However, since carbon black is not blended, the obtained expanded beads have a larger Dc / D than the expanded beads of Examples 1 to 3 and the uniformity of the cell diameter is poor. In addition, the expansion ratio is slightly low. Figure 5 A cross-sectional photograph of the expanded bead is shown.

[0189] Example 4 is an example in which expanded beads were produced in the same manner as Example 3 except that steam was used as the heating medium. By steam foaming, expanded beads having a small apparent density can be obtained.

[0190] Comparative Example 4 is an example in which expanded beads were produced in the same manner as in Comparative Example 1 except that steam was used as the heating medium. The resin particles were hardly foamed and the apparent density was large.

[0191] Examples 5 to 8 and Comparative Examples 5 and 6

[0192] Example 1 was repeated in the same manner as Example 1 except that the conditions of the CB-containing pellet manufacturing step (a), the wetting step (b), the blowing agent impregnation step (c) and the foaming step (d) were changed as shown in Table 3. In Table 3, the relational expression (3) when the carbon black content is 1.5% by mass and the relational expression (4) when the carbon black content is 5% by mass are as follows:

[0193] y = -0.0897x 3 +2.4171x 2 - 22.613x + 43.016 (3)

[0194] y= -0.189x 3 +4.6366x 2 - 36.404 x + 58.521 (4)

[0195] Where y represents the change point temperature (°C) of the storage modulus of the polyamide resin particles, and

[0196] x represents the moisture content (%) of the polyamide resin particles.

[0197] The physical properties of the obtained resin particles and expanded beads are shown in Table 3. Since the expanded states of the expanded beads obtained in Comparative Examples 5 and 6 were significantly poor, it was difficult to measure the average cell diameter thereof, and the appearance thereof was not evaluated.

[0198]

[0199] Explanation of Reference Symbols

[0200] L1: A straight line extending from the straight line portion before the first sudden drop in storage modulus to the high temperature side;

[0201] L2: A straight line extending from the straight line portion after the first sudden drop in storage modulus to the low temperature side;

[0202] A: Curve of storage modulus changing with temperature;

[0203] B: The intersection of straight lines L1 and L2

Claims

1. A method for producing expandable polyamide resin particles, The method comprises impregnating polyamide resin particles with an inorganic blowing agent in a gas phase, The polyamide resin particles have a moisture content of 2.5% by mass or more and contain carbon black in an amount of 0.5% by mass or more and 10% by mass or less. 2 . The method according to claim 1 , wherein the impregnation is performed at a temperature higher than a temperature of a storage modulus change point of the polyamide-based resin particles. 3 . The method according to claim 1 , wherein the impregnation is performed at a temperature that is 30° C. higher than a storage modulus change point of the polyamide-based resin particles and is not higher than 120° C.

4. The method according to any one of claims 1 to 3, wherein the impregnation is performed at a temperature of not less than 20°C and not more than 120°C.

5. The method according to any one of claims 1 to 4, wherein the carbon black has a 50 m 2 / g or more and 200m 2 / g or less BET specific surface area. 6 . The method according to claim 1 , wherein the polyamide-based resin particles have a moisture content of 5% by mass or more and 20% by mass or less.

7. The method according to any one of claims 1 to 6, wherein the polyamide resin particles are obtained by a method comprising the following steps: (a) providing carbon black-containing polyamide-based resin pellets, the pellets having a carbon black content of 0.5% by mass or more and 10% by mass or less, and (b) Wetting the carbon black-containing polyamide-based resin pellets to a moisture content of 2.5% by mass or more. 8 . A method for producing polyamide-based resin expanded beads, the method comprising heating the expandable particles according to any one of claims 1 to 7 to foam and expand the expandable particles.

9. An expanded bead having a plurality of cells and comprising a polyamide resin and carbon black, The carbon black is contained in the expanded beads in an amount of 0.5% by mass or more and 10% by mass or less based on 100% by mass of the expanded beads, The expanded beads have a mass of 100 kg / m 3 Above and 800kg / m 3 The following apparent density, closed cell content of 80% or more, average cell diameter D of all cells of the expanded beads and average cell diameter Dc of cells located in the central region of the expanded beads, The ratio Dc / D is 0.7 or more and 1.3 or less. 10 . The expanded beads according to claim 9 , which are obtainable by the method according to claim 8 .