Polyethylene resin composition

By controlling the crystal structure of the polyethylene resin, a polyethylene resin composition that meets specific conditions is prepared, which solves the problem of difficulty in taking into account both tensileability and TVOC emissions in the prior art, and achieves polyethylene with high mechanical strength and low TVOC emissions Vinyl resin composition for the production of excellent stretch films.

CN118974161APending Publication Date: 2024-11-15LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032056.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-20
Filing Date
2023-12-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing polyethylene resin compositions are difficult to meet both excellent stretchability and low total volatile organic compound (TVOC) emission requirements when manufacturing the stretched film.

Method used

By controlling the crystal structure, an ethylene homopolymer or ethylene/C4 to C10α-olefin copolymer that meets the specific TREF analysis conditions is prepared to ensure that the first crystalline polymer content is between 0.1% and 1.8% and the second crystalline polymer content is between 20 % to 40%, density above 0.940 g/cm3 and melt index between 0.1 g/10 min to 10 g/10 min.

Benefits of technology

It is achieved to significantly reduce TVOC emissions while maintaining excellent mechanical strength, and to improve the tensileability and physical properties of the stretched film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005067774050000181
    Figure BDA0005067774050000181
  • Figure BDA0005067774050000191
    Figure BDA0005067774050000191
  • Figure BDA0005067774050000211
    Figure BDA0005067774050000211
Patent Text Reader

Abstract

Provided is a polyethylene resin composition which exhibits reduced TVOC and excellent stretchability and thus can be used in the manufacture of a stretched film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is based on and claims the benefit of priority of Korean Patent Application Nos. 10-2022-0189077 and 10-2023-0187174, filed on December 29, 2022 and December 20, 2023, respectively, the disclosures of which are hereby incorporated herein by reference in their entirety.

[0003] The present invention relates to a polyethylene resin composition that exhibits reduced total volatile organic compound (TVOC) emissions and excellent stretchability and can be used to manufacture stretch films. Background Art

[0004] With recent consumer concerns about the environment, easily recyclable single-material packaging is gaining attention. Typically, in the food packaging and distribution industry, there is a trend to manufacture "all-PE" films using only the common material polyethylene (PE).

[0005] In the past, composite materials of BOPA, BOPET, BOPP, etc., with a printing layer applied, have been used for multilayer film packaging materials. In order to replace the composite materials with PE, they need higher physical properties than the existing PE blown films.

[0006] Meanwhile, a biaxially oriented polyethylene (BOPE) film is manufactured by stretching a cast sheet in the machine direction (MD) and the transverse direction (TD), and has significantly better tensile strength, impact strength, and transparency than existing blown films.

[0007] The key to developing high-density polyethylene (HDPE) for BOPE is to perform biaxial stretching from MD stretching to TD stretching.

[0008] Therefore, research and development are required to prepare polyethylene or a polyethylene resin composition having excellent stretchability. Summary of the invention

[0009] [Technical issues]

[0010] In order to solve the problems of the prior art, a polyethylene resin composition showing reduced TVOC and excellent stretchability is provided by controlling the crystal structure.

[0011] By using the polyethylene resin composition, a stretched film showing excellent stretchability is also provided.

[0012] [Technical solution]

[0013] In order to achieve the above object, a polyethylene resin composition comprising an ethylene homopolymer or an ethylene / C4 to C10 α-olefin copolymer and satisfying the following requirements (a1) to (a3) ​​is provided:

[0014] (a1) during temperature rising elution fractionation (TREF) analysis, in a TREF analysis graph having elution temperature (Te) as the x-axis and elution amount (dw / dt) as the y-axis, the content of the first crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 25° C. to the total peak area, is from 0.1% to 1.8%, and the content of the second crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 40° C. to the total peak area, is from 20% to 40%,

[0015] (a2) Density measured at 23°C according to ASTM D1505: 0.940 g / cm 3 above, and

[0016] (a3) Melt index (MI) measured according to ASTM D1238 (Condition E, 190°C, 2.16 kg load) 2.16 ): 0.1 g / 10 min or more and 10 g / 10 min or less.

[0017] Also provided is a stretched film comprising the polyethylene resin composition.

[0018] [Beneficial Effects]

[0019] According to the present invention, a polyethylene resin composition showing reduced TVOC and excellent stretchability is provided.

[0020] By using the polyethylene resin composition, a stretched film showing excellent stretchability is also provided. DETAILED DESCRIPTION

[0021] As used herein, the terms “first”, “second”, etc. are used to describe various components, and these terms are only used to distinguish a certain component from other components.

[0022] In addition, the terms used in this specification are only used to illustrate exemplary embodiments and are not intended to limit the present invention. Singular expressions may include plural expressions unless there is a different expression in the context. It must be understood that in this specification, the terms "comprising", "equipped with", "having" are only used to specify the presence of effective features, numbers, steps, components or combinations thereof, and do not preclude the possibility of the presence or addition of more than one different feature, number, step, component or combination thereof.

[0023] The present invention can be modified in various ways and has various forms, and specific exemplary embodiments will be explained and described in detail as follows. However, it should be understood that this description is not intended to limit the present invention to the specific forms disclosed, but on the contrary, it is intended to cover all modifications, equivalents and substitutes that fall within the spirit and scope of the present invention.

[0024] Hereinafter, the polyethylene resin composition of the present invention will be described in detail.

[0025] The polyethylene resin composition of the present invention comprises an ethylene homopolymer or an ethylene / C4 to C10 α-olefin copolymer and meets the following requirements (a1) to (a3):

[0026] (a1) during temperature rising elution fractionation (TREF) analysis, in a TREF analysis graph having elution temperature (Te) as the x-axis and elution amount (dw / dt) as the y-axis, the content of the first crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 25° C. to the total peak area, is from 0.1% to 1.8%, and the content of the second crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 40° C. to the total peak area, is from 20% to 40%,

[0027] (a2) Density measured at 23°C according to ASTM D1505: 0.940 g / cm 3 above, and

[0028] (a3) Melt index (MI) measured according to ASTM D1238 (Condition E, 190°C, 2.16 kg load) 2.16 ): 0.1 g / 10 min or more and 10 g / 10 min or less.

[0029] Generally, biaxially oriented polyethylene (BOPE) films are produced by stretching a cast sheet in the machine direction (MD) and the transverse direction (TD). As described, since biaxial stretching must proceed from MD stretching to TD stretching, PE used for BOPE requires excellent stretchability.

[0030] In order to ensure the stretchability of polyethylene (PE), there must be a structure that allows interlaminar lateral connection between lamellae in PE so that secondary crystallization occurs as late as possible in MD stretching, followed by TD stretching.

[0031] The polyethylene resin composition of the present invention is a semi-crystalline polymer and may include crystalline and amorphous regions. Specifically, in the crystalline region, polymer chains including ethylene repeating units or α-olefin repeating units fold to form bundles, thereby forming crystalline regions (or segments) in the form of sheets.

[0032] The inventors of the present invention have discovered that when the content of the crystalline polymer in the elution temperature range that affects the stretchability and TVOC properties is controlled within the optimal range by TREF analysis, better stretchability and TVOC properties can be achieved than those of the existing polyethylene resin composition having the same density and melt index, thereby completing the present invention.

[0033] Specifically, during the TREF analysis, a crystalline polymer eluted within an elution temperature range of 25°C to 30°C (hereinafter referred to as a "first crystalline polymer") is a soluble fraction. The content of the first crystalline polymer originates from the extremely low molecular weight region of the polyethylene resin composition and affects TVOC. Specifically, as the content of the first crystalline polymer decreases, TVOC decreases.

[0034] Furthermore, the crystalline polymer eluted in the elution temperature range of 40° C. to 90° C. (hereinafter referred to as “second crystalline polymer”) delays secondary crystallization during MD stretching and can improve stretchability through interlayer lateral bonding.

[0035] Therefore, by including 0.1% to 1.8% of a first crystalline polymer eluting in an elution temperature range of 25°C to 30°C and 20% to 40% of a second crystalline polymer eluting in an elution temperature range of 40°C to 90°C in a TREF analysis, the polyethylene resin composition of the present invention can improve stretchability and TVOC properties while maintaining excellent mechanical strength properties.

[0036] More specifically, in the polyethylene resin composition of the present invention, the content of the first crystalline polymer may be 0.1% or more, or 0.5% or more, or 0.7% or more, or 1.1% or more, and may be 1.8% or less, or 1.5% or less, or 1.4% or less. In addition, the content of the second crystalline polymer may be 20% or more, or 22% or more, or 25% or more, and may be 40% or less, or 35% or less, or 31% or less, or 30% or less.

[0037] When the content of the first crystalline polymer exceeds 1.8%, the content of TVOC increases. On the contrary, when the content of the first crystalline polymer is 0% or less than 0.1%, the content of TVOC decreases, but the extremely low molecular weight content does not exist or is extremely reduced, which may lead to an increase in processing load and a decrease in processability.

[0038] In addition, when the content of the second crystalline polymer is less than 20%, the stretchability is reduced due to the lack of heavy crystals acting as interlayer connectors. On the contrary, when the content of the second crystalline polymer exceeds 40%, during the film production process, the mechanical strength property is deteriorated due to the relative reduction of the extremely high molecular weight content that affects the mechanical strength.

[0039] Meanwhile, in the present invention, TREF analysis of the polyethylene resin composition can be performed using a TREF device of PolymerChar in a temperature range of -20°C to 130°C and using trichlorobenzene as a solvent. For example, in the present invention, the cooling rate in the crystallization step during the TREF analysis is set to 0.1°C / min. The detailed analysis method and conditions are described in detail in the following experimental examples.

[0040] Through the above TREF analysis, a TREF analysis graph with elution temperature (Te) (°C) as the x-axis and elution amount (dw / dt) as the y-axis is obtained, and from the TREF analysis graph, the contents of the first and second crystalline polymers are calculated respectively. Specifically, in the TREF analysis graph, the peaks in the elution temperature range of 25°C to 30°C are integrated to obtain the peak area, and then the percentage of the peak area in the corresponding temperature range relative to the total peak area is calculated, which is taken as the content (% or area %) of the first crystalline polymer. In addition, the peaks in the elution temperature range of 40°C to 90°C are integrated to obtain the peak area, and then the percentage of the peak area in the corresponding temperature range relative to the total peak area is calculated, which is taken as the content (% or area %) of the second crystalline polymer.

[0041] In addition to the above-mentioned crystal structure characteristics, the polyethylene resin composition of the present invention has a crystal structure of 0.940 g / cm 3 On the other hand, when the density of the polyethylene resin composition is less than 0.940 g / cm 3 When the film is made of polyurethane, the mechanical strength properties decrease during the film production process and the TVOC emissions increase due to the increase in the content of very low molecular weight polymers.

[0042] More specifically, the density of the polyethylene resin composition may be 0.940 g / cm 3 Above, or 0.945g / cm 3 Above, or 0.950g / cm 3 Above, or 0.954g / cm 3 Above, and can be 0.970g / cm 3 Below, or 0.965g / cm 3 Below, or 0.961g / cm 3 Below, or 0.960g / cm 3 Herein, the density is a value measured at a temperature of 23° C. according to the ASTM D1505 method.

[0043] In addition, the melt index (MI) of the polyethylene resin composition of the present invention is 2.16) is 0.1 g / 10 min to 10 g / 10 min, which is measured according to ASTM D1238 (condition E, 190° C., under a load of 2.16 kg). When the melt index of the polyethylene resin composition is less than 0.1 g / 10 min, since the melt index is too low, the sheet stretchability and film processability are deteriorated, and as a result, it is difficult to manufacture a stretch film. In addition, when the melt index of the polyethylene resin composition exceeds 10 g / 10 min, since the melt index is too high, the processability is deteriorated, and it is difficult to manufacture a stretch film.

[0044] More specifically, the melt index (MI 2.16 ) can be 0.1g / 10min or more, or 0.5g / 10min or more, or 0.7g / 10min or more, or 0.75g / 10min or more, or 0.77g / 10min or more, or 1g / 10min or more, and can be 10g / 10min or less, or 5g / 10min or less, or 3g / 10min or less, or 2.6g / 10min or less, or 2g / 10min or less, or 1.5g / 10min or less.

[0045] In addition, the MFRR (MI5 / MI 2.16 ) may be 2 to 5, which is obtained by dividing the melt index (MI5) measured at a temperature of 190° C. under a load of 5 kg by the melt index (MI5) measured at a temperature of 190° C. under a load of 2.16 kg according to the ASTM D1238 method. 2.16 ) to obtain the ratio.

[0046] More specifically, MFRR (MI5 / MI 2.16 ) can be 2 or more, or 2.5 or more, or 2.8 or more, or 3.5 or more, and can be 5 or less, or 4.8 or less, or 4.6 or less, or 4.52 or less, or 4.2 or less.

[0047] The polyethylene resin composition of the present invention can express excellent stretchability and physical properties by having the peak area distribution according to the melting temperature as described above as well as high density and an optimal melt index range.

[0048] Furthermore, the polyethylene resin composition of the present invention specifically includes an ethylene homopolymer or an ethylene / C4 to C10 α-olefin copolymer.

[0049] Specific examples of the C4 to C10 α-olefin monomers may include 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, and the like, and two or more thereof may be used.

[0050] More specifically, the polyethylene resin composition may include an ethylene homopolymer, an ethylene / 1-butene copolymer, or an ethylene / 1-hexene copolymer.

[0051] Meanwhile, the polyethylene resin composition of the present invention as described above may be prepared by a slurry polymerization method using a plurality of reactors.

[0052] Specifically, the polyethylene resin composition can be prepared by a preparation method comprising the following:

[0053] a first step of preparing a first polyethylene by introducing hydrogen into a first reactor in the presence of a Ziegler-Natta catalyst and conducting a first slurry polymerization of ethylene or ethylene and a C4 to C10 alpha-olefin first comonomer; and

[0054] The first polyethylene is transferred to a second reactor connected to the first reactor, and then only ethylene or ethylene and a C4 to C10 alpha-olefin second comonomer are introduced and a second slurry polymerization is carried out,

[0055] wherein the polymerization temperature (T1) and pressure (P1) during the first slurry polymerization reaction are higher than the polymerization temperature (T2) and pressure (P2) during the second slurry polymerization reaction, and

[0056] In the second slurry polymerization process, the polymerization temperature (T2) is 65°C or more and lower than 80°C, and the pressure (P2) is 3 kgf / cm 2 Up to 4.5kgf / cm 2 .

[0057] Therefore, in the second reactor, the first polyethylene transferred from the first reactor is further polymerized with ethylene or ethylene and C4 to C10 α-olefin comonomer introduced into the second reactor, thereby preparing a polyethylene resin composition satisfying the above-mentioned physical property requirements.

[0058] Specifically, since the method for preparing the polyethylene resin composition of the present invention is performed by slurry polymerization using a plurality of reactors, two or more reactors, for example, two or more continuous stirred tank reactors (CSTRs) may be used.

[0059] Specifically, in the above-mentioned preparation method, a first reactor in which a first slurry polymerization reaction for preparing a first polyethylene occurs and a second reactor connected to the first reactor and in which a second slurry polymerization reaction occurs may be used.

[0060] Furthermore, the polymerization process in the first and second reactors is performed by a slurry polymerization process.

[0061] In solution polymerization, the catalyst is activated by high temperature and high pressure reaction, and therefore, the prepared resin composition exhibits deteriorated stretchability due to narrow molecular weight distribution (MWD) and low content of high molecular weight tail. In contrast, in the slurry polymerization process of the present invention, polymerization is carried out at a relatively low temperature, and therefore, a molecular structure having a wide MWD and containing a large amount of high molecular weight tail required for the polyethylene resin composition for producing a transparent film can be ensured. As a result, the composition can exhibit excellent biaxial stretchability.

[0062] In addition, for the method for preparing the polyethylene resin composition of the present invention, the polymerization temperature (T1) and pressure (P1) during the first slurry polymerization reaction are higher than the polymerization temperature (T2) and pressure (P2) during the second slurry polymerization reaction, and the second slurry polymerization reaction is performed at a polymerization temperature (T2) of 65° C. and a pressure of 3 kgf / cm 2 Up to 4.5kgf / cm 2 The process is carried out under a pressure (P2).

[0063] As described above, the temperature and pressure conditions during the first slurry polymerization reaction are higher than those during the second slurry polymerization reaction, and the temperature and pressure during the second slurry polymerization reaction are controlled in an optimal range, thereby achieving an NCD structure having a high SCB content derived from the comonomer in the low molecular weight region and a bimodal molecular weight distribution. Since the SCB content is high in the low molecular weight region, the mobility of the tying molecules between crystals increases, and as a result, fibril formation is suppressed during stretching, which can be more conducive to stretching in the TD direction.

[0064] More specifically, the second slurry polymerization reaction is carried out under the following conditions: the polymerization temperature (T2) is 65°C or more, or 70°C or more, and is lower than 80°C, or 78°C or less, or 75°C or less, and the pressure (P2) is 3kgf / cm 2 Above, or 3.1kgf / cm 2 Above, and 4.5kgf / cm 2 Below, or 4.3kgf / cm 2 the following.

[0065] Meanwhile, during the first slurry polymerization process, the polymerization temperature (T1) may be 70° C. to 90° C., and the pressure (P1) may be 5 kgf / cm 2 Up to 10kgf / cm 2 More specifically, the polymerization temperature (T1) may be 70°C or more, 75°C or more, or 78°C or more, and may be 90°C or less, 85°C or less, or 80°C or less, and the pressure (P1) may be 5 kgf / cm 2 Above, or 6kgf / cm 2Above, or 6.5kgf / cm 2 Above, or 6.7kgf / cm 2 Above, and can be 10kgf / cm 2 Below, or 8kgf / cm 2 Below, or 7.7kgf / cm 2 Below, or 7.4kgf / cm 2 the following.

[0066] More specifically, while satisfying the polymerization temperature and pressure range in the first slurry polymerization reaction process and the polymerization temperature and pressure range in the second slurry polymerization reaction process, the difference (T1-T2) between the polymerization temperature (T1) in the first slurry polymerization reaction process and the polymerization temperature (T2) in the second slurry polymerization reaction process can be above 3°C, or above 4°C, or above 5°C, and can be below 10°C, or below 8°C, or below 6°C.

[0067] In addition, the difference (P1-P2) between the pressure (P1) during the first slurry polymerization reaction and the pressure (P2) during the second slurry polymerization reaction may be 2 kgf / cm 2 Above, or 3kgf / cm 2 Above, or 3.1kgf / cm 2 Above, or 3.6kgf / cm 2 Above, and can be 6kgf / cm 2 Below, or 5kgf / cm 2 Below, or 4kgf / cm 2 Below, or 3.9kgf / cm 2 the following.

[0068] When the conditions during the first and second slurry polymerizations satisfy the above requirements, the above-mentioned comprehensive physical properties of the polyethylene resin composition can be easily achieved.

[0069] Furthermore, for the method for preparing the polyethylene resin composition of the present invention, in the first and second slurry polymerization processes, only ethylene may be introduced, or a C4-C20 α-olefin comonomer may be introduced together with ethylene.

[0070] In the above preparation method, the input amount of ethylene introduced into the first slurry polymerization reaction may be greater than the input amount of ethylene introduced into the second slurry polymerization reaction. In this case, the above comprehensive physical properties of polyethylene can be more easily achieved.

[0071] Additionally, comonomers may be introduced into one or more of the polymerization reactions in the first slurry polymerization reaction and the second slurry polymerization reaction.

[0072] More specifically, a comonomer may be introduced during the first slurry polymerization reaction. As described, when a comonomer is introduced during the first slurry polymerization reaction, an NCD structure with a high SCB content derived from the comonomer in the low molecular weight region and a bimodal molecular weight distribution may be achieved. As a result, stretching in the TD direction may be more favorable.

[0073] In addition, when the comonomer is further introduced, the total amount of ethylene introduced into the first and second reactors and the total amount of the comonomer may satisfy a weight ratio of 1:0.001 to 1:0.1, and more specifically, a weight ratio of 1:0.01 to 1:0.1, or a weight ratio of 1:0.012 to 1:0.05, or 1:0.012 to 1:0.025, or 1:0.012 to 1:0.02. When the total amount of ethylene introduced into the first and second reactors and the total amount of the comonomer satisfy the above weight ratio range, the physical properties of the above-mentioned polyethylene resin composition can be more easily achieved.

[0074] Hereinafter, each step will be described in detail.

[0075] In the preparation method of the polyethylene resin composition of the present invention, the first step is a step of preparing a first polyethylene by introducing hydrogen into a first reactor in the presence of a Ziegler-Natta catalyst and conducting a first slurry polymerization reaction of ethylene and a C4 to C10 α-olefin comonomer (hereinafter referred to as "the first comonomer").

[0076] The Ziegler-Natta catalyst used to prepare the first polyethylene may specifically be a magnesium-supported titanium catalyst. In addition, the magnesium-supported titanium catalyst may further contain a halogenated hydrocarbon.

[0077] Specifically, the magnesium-supported titanium catalyst comprises a solid magnesium carrier. Examples of the magnesium carrier may include magnesium, magnesium oxide, magnesium chloride or silicon dioxide-magnesium oxide, and any one thereof or a mixture of two or more thereof may be used. Wherein, in view of the catalytic activity and the physical properties of the polyethylene resin composition that are easy to achieve the best, the magnesium carrier may be magnesium or magnesium chloride.

[0078] Meanwhile, the magnesium-supported titanium catalyst comprises a titanium-containing compound represented by the following chemical formula (1) as a main catalyst:

[0079] [Chemical formula 1]

[0080] Ti(OR 1 ) m X 1 4-m

[0081] In Chemical Formula 1,

[0082] R 1are the same or different and are alkyl groups having 1 to 10 carbon atoms,

[0083] X 1 is a halogen atom, more specifically Cl, Br or I, and

[0084] m is an integer of 0-4.

[0085] In Chemical Formula 1, R 1 Specifically, it may be an alkyl group having 1 or more, 2 or more, or 3 or more carbon atoms and 10 or less, 8 or less, or 5 or less carbon atoms.

[0086] In addition, X 1 It may specifically be Br or Cl, and more specifically Cl.

[0087] Specific examples of the titanium-containing compound may include titanium tetrachloride (TiCl 4 ) or titanium oxychloride, and any one of them or a mixture of both may be used.

[0088] In addition, based on the content of Mg in the magnesium support and the content of Ti in the titanium-containing compound, the catalyst containing the titanium-containing compound contains Mg:Ti in a molar ratio of 1:1 to 10:1, or 2:1 to 7:1, or 4:1 to 5:1. When contained within the above molar ratio range, excellent catalytic activity can be achieved.

[0089] Furthermore, the shape of the catalyst is not particularly limited but may be, for example, in the form of spherical fine particles.

[0090] Furthermore, the average particle size of the catalyst may be 5 to 100 μm, more specifically 5 μm or more, 8 μm or more, or 10 μm or more, and may be 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 13 μm or less.

[0091] Meanwhile, the average particle size of the catalyst in the present invention can be measured by scanning electron microscope (SEM) observation. Specifically, after obtaining an SEM image of more than 100 catalyst particles, random straight lines are drawn, and the average particle size of the catalyst particles can be calculated from the length of the corresponding straight line, the number of particles included in the straight line, and the magnification.

[0092] In addition, the magnesium-supported titanium catalyst may further contain a halogenated hydrocarbon.

[0093] The halogenated hydrocarbons change the electrical properties of titanium by coordinating around titanium as active sites, and a large amount of halogenated hydrocarbons create ample three-dimensional space between titanium atoms, thereby greatly improving the catalytic activity during polyethylene polymerization.

[0094] The halogenated hydrocarbon may specifically be an alkane having 1 to 12 carbon atoms, a cycloalkane having 3 to 12 carbon atoms, an alkene having 2 to 12 carbon atoms, an alkyne having 2 to 12 carbon atoms, or an aromatic hydrocarbon having 6 to 30 carbon atoms substituted with one or more halogen groups. The halogen group may be fluorine, chlorine or bromine.

[0095] Specific examples may include bromoform, tetrachloroethane, hexachloroethane, pentachloroethane, 1,1,2,2-tetrachloroethane, 1-bromo-1-chloroethane, 1,2-dibromoethane, 1,2-dichloroethane, ethyl bromide, hexachloropropane, 1,2,3-trichloropropane, 1,2-dichloropropane, 1-chloropropane, 2-chloropropane, chlorobutane, dichlorobutane, 1-chloro-2-methylpropane, n-butyl chloride, tert-butyl chloride, 1-chloro-3-methylbutane, 1-chloropentane, 1,5-dichloropentane, bromopropane, Pentane, neopentyl chloride, 1-chloroheptane, cyclopropyl bromide, cyclobutyl chloride, cyclohexyl chloride, cyclohexyl bromide, vinylidene chloride, 1,2,3,3-tetrachloropropene, 1,2-dibromo-1-propene, 1,3-dichloropropene, hexachloro-1,3-butadiene, 2-bromo-2-butene, propargyl chloride, chlorobenzene, tetrachlorobenzene, trichlorobenzene, dichlorobenzene, 4-chlorobenzyl chloride, benzyl chloride, or 1,1-dichloro-2-phenylcyclopropane, and one of them or a mixture of two or more thereof may be used.

[0096] Based on 1 mol of the titanium-containing compound as the main catalyst, the content of the halogenated hydrocarbon can be more than 0.1 mol, or more than 0.12 mol, or more than 0.13 mol, and can be less than 500 mol, or less than 100 mol, or less than 50 mol, or less than 10 mol, or less than 1 mol, or less than 0.5 mol.

[0097] The Ziegler-Natta catalyst can be prepared by a preparation method including: a carrier treatment step of mixing and reacting the raw material of the magnesium carrier with an alcohol; and a titanium-containing compound loading step of reacting the product obtained by the above step with a titanium-containing compound represented by Chemical Formula 1, and further including a step of contacting and reacting with a halogenated hydrocarbon in the carrier treatment step or the titanium-containing compound loading step or after the titanium-containing compound loading step. Therefore, before the first step, the preparation method of the polyethylene resin composition of the present invention includes a step of preparing a Ziegler-Natta catalyst, specifically, including a carrier treatment step and a titanium-containing compound loading step, and may further include a step of contacting and reacting with a halogenated hydrocarbon in the carrier treatment step or the titanium-containing compound loading step or after the titanium-containing compound loading step.

[0098] Specifically, the support treatment step for preparing the Ziegler-Natta catalyst may be performed by mixing and reacting a raw material of the magnesium support with an alcohol in a non-polar solvent.

[0099] Specific examples of alcohols may include methanol, ethanol, 1-propanol, isopropanol, n-butanol, isobutanol, 1-pentanol, isopentanol, n-hexanol, 1-octanol, 2-ethyl-1-hexanol, etc., and one or a mixture of two or more thereof may be used. Among them, ethanol or 2-ethyl-1-hexanol may be used.

[0100] The amount of the alcohol used may be 1 mol or more, or 1.5 mol or more, or 2 mol or more, and may be 10 mol or less, or 8 mol or less, or 6 mol or less, based on 1 mol of the raw material of the magnesium carrier.

[0101] Meanwhile, the raw material of the magnesium support may include the magnesium support itself, such as magnesium, magnesium oxide, magnesium chloride or silica-magnesium oxide, etc., or a magnesium alcoholate such as magnesium ethoxide, and one or a mixture of two or more thereof may be used. For example, when magnesium alcoholate is used as the raw material of the magnesium support, it is converted into magnesium chloride by titanium tetrachloride (TiCl4) introduced as a main catalyst, and is included in the catalyst finally prepared as a support.

[0102] The method of mixing the raw material of the magnesium support with alcohol can be specifically performed as follows: the alcohol is added to a slurry prepared by mixing the raw material of the magnesium support with a non-polar solvent such as hexane, or a solution obtained by dissolving the alcohol in a non-polar solvent is added to the slurry, and then the solution is stirred at a temperature of 20° C. to 150° C. until it becomes a transparent solution. As a result of the above mixing, a homogeneous solution of the magnesium support is obtained, and in the solution, an adduct in which the crystals of the magnesium support are surrounded by the alcohol molecules is formed.

[0103] Next, the titanium-containing compound supporting step for preparing the Ziegler-Natta catalyst is performed by reacting the reaction product of the magnesium support and alcohol produced in the support treatment step with a titanium-containing compound.

[0104] Specifically, a titanium compound or a solution of a titanium compound dissolved in a nonpolar solvent is directly added to the reaction product of the magnesium support and alcohol generated in the support treatment step, and reacted at -50°C to 120°C or -20°C to 80°C.

[0105] The type and content of the titanium-containing compound are as described above.

[0106] Furthermore, when the titanium-containing compound is introduced, the reaction product of the magnesium support and the alcohol generated in the support treatment step may be stirred at 10 rpm to 500 rpm, or 50 rpm to 400 rpm.

[0107] Meanwhile, when preparing the Ziegler-Natta catalyst, the halogenated hydrocarbon is introduced when adding alcohol to the magnesium support in the support treatment step; the halogenated hydrocarbon is introduced when introducing the titanium-containing compound in the titanium-containing compound loading step; or after completing the step of loading the titanium-containing compound, a step of adding the halogenated hydrocarbon and reacting can be further performed.

[0108] The type and content of the halogenated hydrocarbon are as described above.

[0109] The Ziegler-Natta catalyst prepared by the above preparation method can be used as it is in the polyethylene polymerization process, or can be used as a slurry in a non-polar solvent.

[0110] In addition, the Ziegler-Natta catalyst may be used together with an organic metal compound represented by the following Chemical Formula 2 as a co-catalyst:

[0111] [Chemical formula 2]

[0112] R 2 n MX 2 (3-n)

[0113] In chemical formula 2,

[0114] M is selected from the group consisting of elements of Groups IB, IIA, IIIB and IVB of the Periodic Table,

[0115] R 2 are the same or different and are alkyl groups having 1 to 10 carbon atoms,

[0116] X 2 is a halogen, and

[0117] n is an integer of 1 to 3.

[0118] In Chemical Formula 2, M is specifically aluminum, R 2 is an alkyl group having 1 to 5 carbon atoms or 2 to 4 carbon atoms, and X 2 It is Cl or Br.

[0119] Specific examples of the organometallic compound represented by Chemical Formula 2 may include triethylaluminum, methylaluminum dichloride, methylaluminum dibromide, dimethylaluminum chloride, dimethylaluminum bromide, propylaluminum dichloride, propylaluminum dibromide, butylaluminum dichloride, butylaluminum dibromide, dibutylaluminum chloride, dibutylaluminum bromide, isobutylaluminum dichloride, isobutylaluminum dibromide, diisobutylaluminum chloride, diisobutylaluminum bromide, hexylaluminum dichloride, hexylaluminum dibromide, dihexylaluminum chloride, dihexylaluminum bromide, octylaluminum dichloride, octylaluminum dibromide, dioctylaluminum chloride, and dioctylaluminum bromide, and any one of them or a mixture of two or more thereof may be used.

[0120] At the same time, since the co-catalyst affects the polymerization activity of the magnesium-supported catalyst, the polymerization activity of the catalyst can be further improved by controlling the content of the co-catalyst. For example, for the organic metal compound represented by Chemical Formula 2, the amount of aluminum used can be 3 mol or more, or 10 mol or more, or 25 mol or more, and can be 200 mol or less, or 100 mol or less, relative to 1 mol of titanium in the catalyst.

[0121] The cocatalyst can be added to the polyethylene polymerization reaction after mixing with the Ziegler-Natta catalyst, or can be added separately before or after adding the Ziegler-Natta catalyst. Therefore, the preparation method of the polyethylene resin composition of the present invention can also include the step of adding the cocatalyst when preparing the first polyethylene in the first step.

[0122] Meanwhile, the polymerization reaction in the first step is a copolymerization reaction of ethylene and α-olefin, and the input amount of ethylene and the first comonomer can be determined in consideration of the physical properties to be achieved by the first polyethylene and the final polyethylene resin composition. For example, in the present invention, the content of the first comonomer introduced into the first reactor can be 0.01 wt % to 5 wt % based on the total weight of the ethylene introduced into the first reactor. When introduced within the above content range, the comprehensive physical properties of the above-mentioned polyethylene resin composition can be easily achieved, and as a result, due to the increase in low molecular weight and low crystalline content ratio, the increase in the stretch ratio in the TD direction can be achieved.

[0123] Furthermore, the polymerization reaction in the first step is carried out under the condition of introducing hydrogen.

[0124] Since the input amount of hydrogen affects the physical properties of the copolymer prepared, the input amount is appropriately determined according to the physical properties to be achieved. For example, in the present invention, based on the gross weight of the monomers including ethylene and α-olefins introduced into the first and second reactors, the input amount of hydrogen can be 0.001 wt % to 0.5 wt %. When hydrogen is introduced within the above range, the comprehensive physical properties of the above-mentioned polyethylene resin composition can be easily achieved. More specifically, the introduction amount of hydrogen can be more than 0.001 wt %, or more than 0.01 wt %, or more than 0.05 wt %, or more than 0.07 wt %, and can be less than 0.5 wt %, or less than 0.3 wt %, or less than 0.1 wt %, or less than 0.09 wt %.

[0125] Furthermore, in the polymerization reaction in the first step, the temperature and pressure conditions and the kind and input amount of the first comonomer are as defined above.

[0126] The first polyethylene is prepared by a polymerization reaction under the above preparation conditions.

[0127] Next, the second step is carried out in a second reactor connected to the first reactor.

[0128] Specifically, the first polyethylene prepared in the first step is transferred to a second reactor connected to the first reactor, ethylene and a C4 to C10 α-olefin second comonomer are introduced, and a second slurry polymerization reaction is performed.

[0129] In the second reactor, an additional polymerization reaction occurs between the first polyethylene transferred from the first reactor and the ethylene or C4 to C10 alpha-olefin second comonomer introduced into the second reactor.

[0130] The second slurry polymerization reaction may be carried out in the presence of a catalyst.

[0131] In this case, the catalyst that can be used is the Ziegler-Natta catalyst as described in step 1. Therefore, the Ziegler-Natta catalysts used for the first and second slurry polymerization reactions may be the same or different from each other. When the same Ziegler-Natta catalyst is used in the first and second slurry polymerization reactions, it is easier to control the physical properties of the polyethylene resin composition to be prepared, and thus achieve the above physical property requirements.

[0132] In addition, the second slurry polymerization reaction can be carried out under the condition of adding hydrogen or not adding hydrogen. For example, when adding hydrogen, the addition amount of hydrogen can be 0.001 wt% to 0.05 wt% based on the total weight of monomers including ethylene and α-olefin second comonomer introduced into the second reactor.

[0133] Furthermore, during the polymerization reaction in the second step, the temperature and pressure conditions and the kind and content of the second comonomer are as defined above.

[0134] Meanwhile, the preparation method of the present invention may further include a step of melting and extruding the obtained polymerization product after completing the polymerization reaction in the second step.

[0135] The pellet-type polyethylene resin composition can be prepared through the above melting and extrusion steps.

[0136] Since the polymer product after the polymerization reaction in the second step is obtained in the form of powder, the types of applicable antioxidants are limited. In addition, since the content of the antioxidant varies greatly depending on the powder, the articles manufactured using the polymer product vary greatly in their physical properties. In contrast, when the melting and extrusion process is performed, the components including the antioxidant are uniformly mixed, and the resulting article can have uniform physical properties.

[0137] Meanwhile, as used herein, pellets or pellet-types are small particles or small pieces formed by extrusion of raw materials, and include all shapes defined as pellets in the art, including round, flat, thin-sheet, polygonal, rod-shaped, etc. The size of the pellets is appropriately determined according to the use and shape, and is not specifically limited, but the pellets in the present invention are defined as having an average diameter of 2 mm or more, thereby distinguishing from powders having a small average diameter of about 1 mm. In this regard, the "diameter" is the longest distance in any straight-line distance of the outer peripheral surface of the pellets, and can be measured using an imaging microscope, etc.

[0138] The melt extrusion process can be performed using a conventional extruder, and the specific method and conditions are not particularly limited as long as the morphological conditions of the pellets are met.

[0139] In addition, during the melt extrusion process, one or more additives such as antioxidants, neutralizers, slip agents, anti-caking agents, UV stabilizers, antistatic agents, etc. may be added. Therefore, the prepared polyethylene resin composition may further contain one or more additives, such as antioxidants, neutralizers, slip agents, anti-caking agents, UV stabilizers, and antistatic agents, etc. At the same time, in the present invention, the additives do not affect the physical properties of the polyethylene resin composition, and when the resin composition is used to manufacture an article, the processability and quality of the manufactured article can be improved.

[0140] For example, the antioxidant may include phenolic antioxidants; phosphorus antioxidants; amine antioxidants, etc., and any one of them or a mixture of two or more thereof may be used. Specific examples of the antioxidant may include phenolic antioxidants, such as pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] or 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, etc.; phosphorus antioxidants, such as tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, and bis(2,4-diisopropylphenylphenyl)pentaerythritol diphosphite, etc.; or amine antioxidants, such as phenylnaphthylamine, 4,4'-(α,α-dimethylbenzyl)diphenylamine, and N,N'-di-2-naphthyl-p-phenylenediamine, etc., and any one of them or a mixture of two or more thereof may be used. In addition, commercially available Irganox can be used TM 1010 (manufactured by BASF), Irganox TM 3114 (manufactured by BASF), Irganox TM 1076 (manufactured by BASF), Irgafos TM 168 (manufactured by BASF), Irgafos TM626 (manufactured by BASF) or Cyanox TM 1790 (manufactured by CYTEC). Wherein, the polyethylene resin composition may include a mixture of a first phenolic antioxidant and a second phosphorus antioxidant. In this regard, based on the total weight of the polymerized product produced by the secondary polymerization, the addition amount of the first phenolic antioxidant may be 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and may be 500 ppm or less, or 300 ppm or less. Based on the total weight of the polymerized product produced by the secondary polymerization, the addition amount of the second phosphorus antioxidant may be 100 ppm or more, or 300 ppm or more, or 500 ppm or more, and may be 1000 ppm or less, or 700 ppm or less. Therefore, based on the total weight of the resin composition, the content of the first phenolic antioxidant of the polyethylene resin composition can be greater than 50 ppm, or greater than 200 ppm, or greater than 250 ppm, and can be less than 500 ppm, or less than 300 ppm, and the content of the second phosphorus antioxidant can be greater than 100 ppm, or greater than 300 ppm, or greater than 500 ppm, and can be less than 1000 ppm, or less than 700 ppm.

[0141] In addition, neutralizing agent can include calcium stearate (Ca-St), calcium palmitate, zinc stearate, zinc palmitate or hydrotalcite (hydroxy magnesium aluminum carbonate) etc., and can use any one or a mixture of two or more thereof. In addition, commercially available DHT-4A (manufactured by KYOWA) etc. can be used. Based on the gross weight of the polymerized product produced by secondary polymerization, the addition of neutralizing agent can be more than 100ppm, or more than 300ppm, or more than 500ppm, and can be less than 1000ppm, or less than 700ppm. Therefore, based on the gross weight of resin combination, the content of the neutralizing agent of polyethylene resin combination can be more than 100ppm, or more than 300ppm, or more than 500ppm, and can be less than 1000ppm, or less than 700ppm.

[0142] In addition, the melting and extrusion process may be performed according to a conventional method, for example, using an extruder such as a twin-screw extruder at an extrusion temperature of 180° C. to 220° C., or 180° C. to 210° C.

[0143] The polyethylene resin composition satisfying the above physical property requirements is prepared using the above preparation method. The prepared polyethylene resin composition exhibits excellent stretchability and TVOC properties, and when a biaxially stretched film is manufactured, there is no need to worry about defects such as breakage and shrinkage during stretching in the TD direction. In addition, the manufactured biaxially stretched film can exhibit excellent stretchability and tensile strength.

[0144] As used herein, the term "volatile organic compounds (VOC)" may be defined as all organic compounds that exist in the atmosphere in a gaseous state. VOC is used to collectively refer to all organic substances that can exist in a gaseous state at room temperature and pressure, such as hydrocarbons consisting only of carbon and hydrogen, halogenated hydrocarbons, and hydrocarbons containing nitrogen or sulfur. In a broad sense, semi-volatile compounds may also be included. For example, in the present invention, volatile organic compounds may be byproducts of thermal decomposition of organic solvents and curing agents, or byproducts generated by addition reactions, etc.

[0145] Specifically, the total volatile organic compound (TVOC) emission of the polyethylene resin composition calculated by gas chromatography / mass spectrometry-thermal desorption (GC / MS-TD) analysis after exposure to a temperature of 200° C. for 10 minutes is 150 μg / g or less, or 110 μg / g or less. The smaller the TVOC emission, the better the polyethylene resin composition, so the lower limit is not particularly limited, but can be, for example, 10 μg / g or more, or 50 μg / g or more.

[0146] Meanwhile, in the present invention, the TVOC emission amount (μg / g) of the polyethylene resin composition can be determined as follows: by dissolving the polyethylene resin composition in a toluene standard solution to prepare a sample, exposing the sample to a high temperature of 300°C for 10 minutes, and then analyzing it using gas chromatography / mass spectrometry-thermal desorption (GC / MS-TD), and based on the chromatogram obtained as a result of the above analysis, the VOC values ​​(μg / g) of the individual substances generated in the measured sample are calculated according to the following equation 1, and they are added.

[0147] [Equation 1]

[0148] VOC 化合物 =[(A 化合物 / A 标准 )×C 标准 ] / W 样品

[0149] VOC 化合物 : Measures the amount of volatile organic compounds (VOCs) generated in a sample after exposure to high temperatures

[0150] A 化合物 : Measure the peak areas of individual substances generated in a sample after exposure to high temperatures

[0151] A 标准 : Peak area of ​​toluene standard solution before exposure to high temperature

[0152] C 标准 : Weight of toluene introduced using toluene standard solution (μg)

[0153] W 样品:Measure the weight of the sample (g)

[0154] The peak areas of individual substances generated in the measurement sample and the peak area of ​​the toluene standard solution were obtained by integrating each peak.

[0155] In addition, as the toluene standard solution, only toluene or a solvent such as methanol is used, and its concentration can be about 0.1 μg / μL or more, or about 0.2 μg / μL or more, or about 0.5 μg / μL or more, or about 0.7 μg / μL or more, or about 0.8 μg / μL or more, or about 1.0 μg / μL or more, or about 1.2 μg / μL or more, and can be about 3.5 μg / μL or less, or about 3.0 μg / μL or less, or about 2.8 μg / μL or less, or about 2.5 μg / μL or less, or about 2.2 μg / μL or less, or about 2.0 μg / μL or less, or about 1.9 μg / μL or less, or about 1.7 μg / μL or less, or about 1.5 μg / μL or less, or about 1.4 μg / μL or less.

[0156] The analysis method by GC / MS-TD and the method for calculating TVOC emissions are described in detail in the following experimental examples.

[0157] According to the present invention, there is provided a stretched film produced using the polyethylene resin composition.

[0158] The stretched film may specifically be a uniaxially stretched film or a biaxially stretched film.

[0159] By including the polyethylene resin composition satisfying the above comprehensive physical property requirements, the stretched film exhibits excellent stretchability and TVOC properties. Specifically, the maximum stretching ratio of the stretched film in the transverse direction (TD) is 6 to 8 times.

[0160] Hereinafter, preferred exemplary embodiments will be provided for better understanding of the present invention. However, the following exemplary embodiments are provided only for easier understanding of the present invention, but the content of the present invention is not limited thereto.

[0161] <Preparation of Catalyst>

[0162] Preparation Example 1

[0163] 34 g of anhydrous magnesium chloride (99% by weight or more, water content less than 1%) was placed in a 2-liter Buchi reactor dried with nitrogen, and 600 mL of purified hexane with a water content of less than 0.5 ppm was also placed in the reactor. To the resulting reaction product, 175 mL of anhydrous 2-ethyl-1-hexanol was added under stirring, and then stirred at a temperature of 130° C. for about 2 hours to prepare a homogeneous solution of a magnesium carrier.

[0164] While stirring the homogeneous solution at a temperature of 35°C and a speed of 200rpm, 200mL of TiCl4 was slowly added within 1 hour and stirred for another hour. In the process, a solid material was produced. After the solid material was precipitated, the liquid portion was removed and the separated solid material was washed several times with hexane until the titanium concentration in the washing solution was less than 0.5mmol. To the washed solid material, a total volume of 1 liter of purified hexane was added. The titanium concentration in the resulting hexane slurry was 30mM. To the hexane slurry, 7mL of cyclohexyl chloride was added at a temperature of 40°C and stirred for 1 hour to obtain a Ziegler-Natta catalyst supported on magnesium chloride.

[0165] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 4:1, and the average size of the catalyst particles was 8 μm.

[0166] Preparation Example 2

[0167] A Ziegler-Natta catalyst supported on magnesium chloride was prepared in the same manner as in Preparation Example 1, except that magnesium chloride was changed to magnesium ethoxide.

[0168] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 5:1, and the average size of the catalyst particles was 10 μm.

[0169] Preparation Example 3

[0170] A Ziegler-Natta catalyst supported on magnesium chloride was prepared in the same manner as in Preparation Example 1, except that anhydrous 2-ethyl-1-hexanol was changed to ethanol.

[0171] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 4.5:1, and the average size of the catalyst particles was 13 μm.

[0172] <Preparation of Polyethylene Resin Composition>

[0173] Example 1

[0174] The high density polyethylene resin composition was prepared by a process for preparing polyethylene by polymerization in the presence of a Ziegler-Natta catalyst system in a bimodal slurry process using two 100 L continuously stirred tank reactors (CSTRs).

[0175] Specifically, in the first reactor, the first polyethylene is prepared by conducting a polymerization reaction under the conditions shown in Table 1 below in the presence of ethylene, the Ziegler-Natta catalyst prepared in Preparation Example 1, an aqueous TEAL solution (30 mmol / hr) as a co-catalyst, hydrogen and a comonomer.

[0176] In the second reactor, a second polyethylene was prepared by conducting a secondary polymerization reaction under the conditions shown in the following Table 1. Here, the first polyethylene polymerized in the first reactor was fed into the second reactor connected in series to conduct secondary polymerization.

[0177] Based on the total weight of the polymerization product obtained as a result of the secondary polymerization, 250 ppm of BASF's Irganox 101 as a first antioxidant, 500 ppm of BASF's Irgafos 168 as a second antioxidant and 500 ppm of calcium stearate (Ca-St) as a neutralizer were fed and mixed, and then extruded at an extrusion temperature of 190° C. using a twin-screw extruder (TEK 30MHS, manufactured by SMPLATECH, with a diameter of 32 pi, L / D=40) to prepare a pellet-type polyethylene resin composition.

[0178] Examples 2 to 4 and Comparative Examples 1 to 9

[0179] Each polyethylene resin composition was produced in the same manner as in Example 1, except that the conditions were changed as shown in Table 1 and Table 2 below.

[0180] [Table 1]

[0181]

[0182] [Table 2]

[0183]

[0184] In Tables 1 and 2, the ethylene:comonomer weight ratio is the weight ratio of the total amount of ethylene introduced into the first and second reactors to the total amount of comonomer including the first and second comonomers.

[0185] The input amount of hydrogen (wt%) is expressed as a percentage of the total weight of hydrogen input based on the total weight of ethylene introduced into the first and second reactors.

[0186] Experimental Example 1

[0187] The physical properties of the polyethylene resin compositions prepared in Examples and Comparative Examples were measured as follows, and the results are shown in Table 3 below.

[0188] (1) Density: measured according to ASTM D1505 method.

[0189] (2) Melt Index (MI 2.16 ): Measured according to ASTM D1238 (Condition E, at 190 °C under a load of 2.16 kg).

[0190] (3) MFRR (MI 21.6 / MI 2.16 ): Measure MI5 at 190 °C under a load of 5 kg and measure MI 2.16 at 190 °C under a load of 2.16 kg respectively according to ASTM D1238 method. After that, obtain it by dividing MI 21.6 by MI 2.16 .

[0191] (4) TREF Analysis:

[0192] Temperature Rising Elution Fractionation (TREF) analysis is carried out in the temperature range of -20 °C to 130 °C using the TREF equipment of PolymerChar and using trichlorobenzene as the solvent. At this time, the cooling rate in the crystallization step is 0.1 °C / min, and the analysis is carried out under the following conditions.

[0193] Specifically, dissolve 30 mg of the polyethylene resin composition sample in 20 mL of trichlorobenzene solvent at 150 °C for 20 minutes. Introduce the solvent into the TREF column, then cool it to -20 °C at a cooling rate of 0.1 °C / min and hold for 2 minutes. Thereafter, while heating from -20 °C to 130 °C at a rate of 0.1 °C / min, apply the solvent trichlorobenzene to the column at a flow rate of 0.5 mL / min to measure the concentration of the eluted polymer. From the measurement results of the concentration, obtain the TREF analysis graph with the elution temperature (Te) (°C) as the x-axis and the elution amount (dw / dt) as the y-axis.

[0194] <TREF Measurement Conditions>

[0195] Dissociation Rate: 40 °C / min

[0196] Stable Rate: 40 °C / min

[0197] Crystallization Rate 1: 0.1 °C / min

[0198] Elution Rate: 1 °C / min

[0199] Cleaning Rate: 30 °C / min

[0200] Dissociation Temperature: 150 °C

[0201] Stable Temperature: 140 °C

[0202] Crystallization Temperature: 35 °C

[0203] Elution starting temperature: 35°C

[0204] Elution temperature: 140°C

[0205] Temperature after elution: 150℃

[0206] Cleaning temperature: 150℃

[0207] Dissociation time: 60min

[0208] Stabilization time: 20min

[0209] Crystallization time: 10min

[0210] Time before injection: 10 minutes

[0211] Soluble fraction time: 10 min

[0212] Elution time: 10min

[0213] Cleaning time: 10 minutes

[0214] Cleaning cycles: 1

[0215] Furthermore, from the TREF analysis chart, the content of the fraction eluted in the elution temperature range of 25° C. to 30° C. (i.e., the first crystalline polymer fraction) and the content of the fraction eluted in the elution temperature range of 40° C. to 90° C. (i.e., the second crystalline polymer fraction) were calculated respectively.

[0216] Specifically, in the TREF analysis chart, the peak in the elution temperature range of 25° C. to 30° C. is integrated to obtain the peak area, and then the percentage of the peak area in the corresponding temperature range relative to the total peak area is calculated, which is taken as the content (% or area %) of the first crystalline polymer. In addition, the peak in the elution temperature range of 40° C. to 90° C. is integrated to obtain the peak area, and then the percentage of the peak area in the corresponding temperature range relative to the total peak area is calculated, which is taken as the content (% or area %) of the second crystalline polymer.

[0217] [Table 3]

[0218]

[0219] Experimental Example 2

[0220] The sheet stretchability, film stretchability, and TVOC emission of the polyethylene resin compositions prepared in Examples and Comparative Examples were evaluated according to the following methods, respectively.

[0221] (1) Sheet stretchability [%]

[0222] A polyethylene resin composition sheet (sheet thickness: 2 mm) was produced at a temperature of 190° C. using an Auto Press (Collin, Lab line P300s), and then cut according to ASTM D882 standard to prepare a sheet sample for measurement.

[0223] The sheet prepared above was fixed horizontally on a Zwick tensile tester (UTM), and then a tensile test was performed by pulling the upper part of the sheet at room temperature (23±5° C.). The stress (%) until the sheet broke when pulled at a tensile speed of 50 mm / min was measured and expressed as the sheet stretchability.

[0224] (2) Film stretchability

[0225] For each of the polyethylene resin compositions of Examples and Comparative Examples, a cast sheet having a thickness of 0.72 mm was produced using Bruckner's Lab extruderline (L / D ratio: 42, screw diameter: 25 mm, melt / T die temperature: 250°C).

[0226] When the cast sheet thus produced was biaxially stretched into a film having a final thickness of about 20 μm using Bruckner's Lab Stretcher KARO 5.0, the maximum stretching ratio (magnification) that could be stretched in the TD direction without breaking the film or causing defects was measured. Prior to biaxial stretching, the cast sheet was preheated at 120° C. for 60 seconds and stretched sequentially in the MD→TD directions.

[0227] However, the polyethylene resin compositions of Comparative Examples 8 and 9 had poor processability due to excessively low or high melt index, resulting in failure to produce stretched films.

[0228] <Measurement conditions>

[0229] Sample size (width × height): 90mm × 90mm

[0230] Stretch:

[0231] Elongation: 4 times in MD direction, 2-9 times in TD direction

[0232] Stretching speed: 300% / s

[0233] Stretching temperature: 120℃

[0234] Preheating temperature: 120℃

[0235] Warm-up time: 60s

[0236] (3) TVOC emissions [μg / g]

[0237] TVOC (total volatile organic compound) emissions can be analyzed by gas chromatography / mass spectrometry-thermal desorption (GC / MS-TD) after exposing the polyethylene resin compositions of Examples and Comparative Examples to high temperatures, and the TVOC emissions are calculated by adding the values ​​of individual VOCs generated from the measured samples.

[0238] Specifically, samples prepared by dissolving the polyethylene resin compositions of Examples and Comparative Examples in a toluene standard solution (toluene only) at a concentration of 20 mg / 10 mL were respectively placed in a GC oven and exposed to high temperature under the following conditions, followed by GC / MS-TD analysis.

[0239] [GC / MS-TD analysis conditions]

[0240] -Sample amount: 20mg

[0241] - GC oven (high temperature exposure condition): After holding at 50°C for 5 minutes, the temperature was increased to 300°C at a rate of 10°C / min and held at 300°C for 10 minutes.

[0242] -Temperature and time of GC / MS-TD analysis: 200℃ and 10min

[0243] - Column: HP-5MS (manufactured by Agilent Technologies)

[0244] -Toluene standard solution

[0245] Based on the chromatogram obtained as a result of the above analysis, VOC values ​​(μg / g) of individual substances generated in the measurement sample were calculated according to the following Equation 1 and then added to calculate the TVOC emission amount.

[0246] [Equation 1]

[0247] VOC 化合物 =[(A 化合物 / A 标准 )×C 标准 ] / W 样品

[0248] VOC 化合物 : The amount of volatile organic compounds (VOC) of a single substance generated from the measurement sample (μg / g)

[0249] A 化合物 : Peak area of ​​a single substance generated from the measured sample

[0250] A 标准 : Peak area of ​​toluene standard solution

[0251] C 标准: Weight of toluene used (μg)

[0252] W 样品 : Measure the weight of the sample (g) (in this experimental example, the weight of the sample is 20 mg, i.e., 0.02 g)

[0253] At the same time, the peak area of ​​the individual substances generated in the measurement sample and the peak area of ​​the toluene standard solution are obtained by integrating each peak.

[0254] [Table 4]

[0255]

[0256] In Table 4, "ND" means not measured.

[0257] As experimental results, the resin compositions of Examples 1 to 3 of the present invention exhibited excellent stretchability and greatly reduced TVOC emissions when manufacturing a stretched film, compared with the resin composition of the comparative example.

Claims

1. A polyethylene resin composition comprising an ethylene homopolymer or an ethylene / C4 to C10 α-olefin copolymer and meeting the following requirements (a1) to (a3): (a1) during temperature rising elution fractionation (TREF) analysis, in a TREF analysis graph having elution temperature (Te) as the x-axis and elution amount (dw / dt) as the y-axis, the content of the first crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 25° C. to the total peak area, is from 0.1% to 1.8%, and the content of the second crystalline polymer, which is defined as the ratio of the peak area of ​​the fraction eluting in the elution temperature range of 40° C. to the total peak area, is from 20% to 40%, (a2) Density measured at 23°C according to ASTM D1505: 0.940 g / cm 3 above, and (a3) Melt index (MI) measured according to ASTM D1238 (Condition E, 190°C, 2.16 kg load) 2.16 ): 0.1 g / 10 min or more and 10 g / 10 min or less.

2. The polyethylene resin composition according to claim 1, wherein The polyethylene resin composition has a content of the first crystalline polymer of 0.5% to 1.5%, and a content of the second crystalline polymer of 20% to 35%.

3. The polyethylene resin composition according to claim 1, wherein The density of the polyethylene resin composition is 0.950 g / cm 3 Up to 0.970g / cm 3 .

4. The polyethylene resin composition according to claim 1, wherein The polyethylene resin composition has a melt index (MI) measured according to ASTM D1238 (condition E, 190° C., under a load of 2.16 kg). 2.16 ) is 0.5g / 10min to 3g / 10min.

5. The polyethylene resin composition according to claim 1, wherein The MFRR (MI 21.6 / MI 2.16 ) is 2 to 5, which is the melt index (MI) measured at a temperature of 190° C. under a load of 21.6 kg according to the ASTM D1238 method. 21.6 ) divided by the melt index (MI) measured at a temperature of 190°C under a load of 2.16 kg 2.16 ) and the ratio obtained.

6. The polyethylene resin composition of claim 1, comprising an ethylene homopolymer, an ethylene / 1-butene copolymer or an ethylene / 1-hexene copolymer.

7. The polyethylene resin composition according to claim 1, wherein The total volatile organic compound emission of the polyethylene resin composition is 150 μg / g or less, which is determined as follows: the polyethylene resin composition is dissolved in a toluene standard solution to prepare a sample, the sample is exposed to a temperature of 300° C. for 10 minutes, and then analyzed using gas chromatography / mass spectrometry-thermal desorption, and from the above analysis, the amount (μg / g) of volatile organic compounds of individual substances generated in the measured sample is calculated according to the following equation 1 and added together: [Equation 1] YOU 化合物 =[(A 化合物 / THE 标准 )×C 标准 ] / W 样品 VOC 化合物 : The amount of volatile organic compounds (VOC) of a single substance generated from the measurement sample (μg / g) A 化合物 : Peak area of ​​a single substance generated from the measured sample A 标准 : Peak area of ​​toluene standard solution C 标准 : Weight of toluene used (μg) W 样品 : Measure the weight of the sample (g). A stretched film comprising the polyethylene resin composition according to claim 1.

9. The stretched film according to claim 8, wherein The maximum stretching ratio of the stretched film in the transverse direction (TD) is 6 to 8 times.

10. The stretched film according to claim 8, wherein The stretched film is a uniaxially stretched film or a biaxially stretched film.