Coating

The problem of applying anticorrosion primer on wet or rusty substrates is solved by using compositions of epoxy resins, silanes, microspheres and glycol ether solvents, achieving high solids content, low volatile organic compounds and low viscosity Coatings provide good corrosion resistance and long-term application.

CN118974182APending Publication Date: 2024-11-15JOTUN AS LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380032565.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-04-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively apply anticorrosion primer on wet, wet or rusty substrates, especially on steel surfaces after ultra-high pressure water spray, and there is hydrolytic instability in traditional curing agents such as ketoimine and aldehydeimine. Sexual and health risks issues.

Method used

Using primer coating compositions containing epoxy resin, silane, microspheres and glycol ether solvents, a coating with high solids content, low volatile organic compounds and low viscosity can be provided by mixing the two parts of the composition, which can be moisturized or grown The rusted substrate adheres and cures to provide good corrosion resistance.

Benefits of technology

Effective adhesion and curing on wet or rusty substrates is achieved, providing long-term application and good corrosion resistance, while reducing the content and viscosity of volatile organic compounds and improving the application characteristics of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070865870000091
    Figure BDA0005070865870000091
  • Figure BDA0005070865870000121
    Figure BDA0005070865870000121
  • Figure BDA0005070865870000131
    Figure BDA0005070865870000131
Patent Text Reader

Abstract

A primer coating composition comprising: (i) an epoxy resin; (ii) from 2.0 to 15 wt% of a silane; (iii) a curing agent; (iv) a glycol ether solvent; and (v) from 1.0 to 9.0 wt% of microspheres.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a primer coating composition which can be applied to a damp, wet, wet or rusted substrate to provide an anticorrosive primer layer on the substrate. The present invention requires a combination of epoxy resin, silane, microspheres and glycol ether solvent. Background Art

[0002] Before applying the primer, it is usually necessary to properly prepare the surface to achieve the appropriate roughness and cleanliness. This is usually achieved by cleaning and sandblasting. If the roughness and cleanliness are not adequate, the anti-corrosion primer cannot be expected to provide long-term protection of the substrate.

[0003] For poorly prepared surfaces, coatings with higher surface tolerance than ordinary epoxy primers are needed. Mastic-type epoxy primers have been found to be suitable for poorly prepared substrates. However, there is still a problem to be solved: applying coatings on wet or wet substrates or on rusted substrates (especially flash rusted surfaces).

[0004] In recent years, with the advent of surface preparation by ultra-high pressure water jetting (UHPWJ) instead of traditional sandblasting, the importance of solving this problem has increased. When the substrate is water-jetted, the steel surface profile is not roughened, and remnants of old paint may still remain on the substrate. Residual water also remains on the surface, and for the purpose of saving time and in order to minimize the amount of flash rust formed, it is preferred to coat the surface before drying. In hot climates, drying can occur quickly, but the result may be flash rust on the surface. It would be beneficial to provide a coating composition that can adhere to a moist or wet substrate, on a flash rusted substrate, and on a substrate with remnants of old paint.

[0005] Application of anticorrosive primers on UHPWJ substrates is a challenge due to residual water on the substrate and flash rust formation on wet steel. Therefore, a coating composition suitable for application on moist and wet substrates and also tolerant of old paint residues is beneficial. It would also be advantageous to have a coating composition that, in addition to excellent anticorrosion properties, has a high volume solids ratio (low content of volatile organic compounds (VOCs)), low density, low viscosity for good application properties, and a long pot life.

[0006] In order to tolerate moist and wet surfaces, curing agents based on ketimines or aldimines are usually used. Ketimines and aldimines hydrolyze in the presence of water to provide free amines and ketones or aldehydes. The released amines react with epoxy-functional resins, and the ketones or aldehydes preferably evaporate and leave the coating film. This makes ketimines and aldimines suitable for use on moist and wet substrates. A disadvantage of using ketimines and aldimines is the release of ketones and aldehydes, which are VOCs and have a negative impact on health and safety.

[0007] Furthermore, if a high wet film thickness is used, the release of the ketone or aldehyde is hindered by the thick film, which can lead to the entrapment of volatile components. In addition, since ketimines and aldimines are hydrolytically unstable, there may be challenges associated with their production and storage. Furthermore, since ketimines and aldimines need to be hydrolyzed to form free amines, a certain amount of moisture is required. Therefore, if the ketimine or aldimine cured product is used under too dry conditions, a very slow cure will result.

[0008] JP 2021143270 discloses an anticorrosion coating for marine structures that can be applied on wet substrates. The coating composition comprises a specific polyamine curing agent to provide a coating composition that can be applied on a wet surface.

[0009] JP6629540 discloses an anticorrosive coating composition that can be applied to a wet surface. Polyoxyalkylene polyamine, Mannich modified amine or ketimine curing agent is used to provide a coating that can be applied to a wet surface.

[0010] JP6629539 discloses a coating composition that can be applied to deteriorated paint without any pretreatment other than water washing. JP6629539 also achieves this by using polyoxyalkylene polyamines, Mannich modified amines or ketimine curing agents.

[0011] WO 2020 / 253732 discloses a coating composition capable of insulating steel from LNG leaks. WO 2020 / 253732 achieves this by using a low density filler and a Jeffamine curing agent.

[0012] WO 2012 / 035520 discloses impact-resistant multilayer coatings based on epoxy resins, microspheres and amine or isocyanate curing agents. Silanes and glycol ethers are of lesser importance.

[0013] US2020 / 017711 discloses a curable composition for footwear comprising an adhesive and a polysiloxane resin. Preferably, a polyurethane adhesive is used.

[0014] CN106024946 discloses a solar cell backing layer, wherein the pattern layer comprises a first main resin, the intermediate layer comprises a second main resin, and the weather-resistant layer comprises a fluororesin.

[0015] US2007 / 048445 discloses a sound-absorbing paint for vehicles. Example Epoxy resin is used.

[0016] WO 2020 / 065588 discloses compositions comprising amino-functional silanes and photoluminescent compounds.

[0017] The inventors have now designed a primer coating composition that is resistant to flash rust and wet or moist substrates, i.e., the primer layer composition of the present invention can be applied to a wet or rusted substrate and it adheres thereto. The coating composition of the present invention also has good application properties, long pot life and good corrosion protection properties. Without wishing to be bound by theory, we speculate that these effects are related to the specific solvents used in the coating composition and the defined levels of silane and microspheres. Summary of the invention

[0018] Therefore, from one aspect, the present invention provides a primer coating composition comprising:

[0019] (i) Epoxy resin;

[0020] (ii) 2.0 to 15 wt % of silane;

[0021] (iii) a curing agent;

[0022] (iv) glycol ether solvents; and

[0023] (v) 1.0 to 9.0 wt% of microspheres.

[0024] In any embodiment of the present invention, it is preferred that the glycol ether solvent has formula (I):

[0025] R-[O-R'] x -OH (I)

[0026] Wherein, x is 1 to 3;

[0027] R is C1-C 16 Aliphatic groups; and

[0028] R' is C1-C 16 Aliphatic group.

[0029] From one aspect, the present invention provides a primer coating composition comprising:

[0030] (i) Epoxy resin;

[0031] (ii) 2.0 to 15 wt % of silane;

[0032] (iii) a curing agent;

[0033] (iv) glycol ether solvents;

[0034] (v) 1.0 to 9.0 wt% microspheres; and

[0035] (vi) Hydrocarbon resins.

[0036] From one aspect, the present invention provides a primer coating composition comprising:

[0037] (i) Epoxy resin;

[0038] (ii) 2.0 to 15 wt % of silane;

[0039] (iii) a curing agent;

[0040] (iv) glycol ether solvents;

[0041] (v) 1.0 to 9.0 wt% microspheres; and

[0042] (vi) Reactive diluents.

[0043] From one aspect, the present invention provides a primer coating composition comprising:

[0044] (i) Epoxy resin;

[0045] (ii) 2.0 to 15 wt % of silane;

[0046] (iii) a curing agent;

[0047] (iv) glycol ether solvents;

[0048] (v) 1.0 to 9.0 wt % of microspheres;

[0049] (vi) hydrocarbon resins; and

[0050] (vii) Reactive diluents.

[0051] Viewed from another aspect, the present invention provides a kit suitable for preparing the primer coating composition of the present invention, comprising:

[0052] Component (A) comprising an epoxy resin; and

[0053] Component (B), comprising a curing agent;

[0054] wherein at least one of components (A) or (B) comprises silane, glycol ether solvent, and microspheres;

[0055] Such that when components (A) and (B) are mixed, the resulting primer layer composition comprises 2.0 to 15 wt % of silane and 1.0 to 9.0 wt % of microspheres.

[0056] Viewed from another aspect the invention provides a metal substrate coated with a primer coating composition as hereinbefore defined.

[0057] Viewed from another aspect the invention provides a metal substrate having a primer coating composition as hereinbefore defined which has been cured.

[0058] Viewed from another aspect, the invention provides a process for preparing a primer coating composition as hereinbefore defined comprising blending components (A) and (B):

[0059] wherein component (A) comprises an epoxy resin; and

[0060] Component (B) comprises a curing agent;

[0061] At least one of components (A) or (B) comprises silane, a glycol ether solvent and microspheres, such that when components (A) and (B) are mixed, the resulting primer layer composition comprises 2.0 to 15 wt % silane and 1.0 to 9.0 wt % microspheres.

[0062] Viewed from another aspect, the present invention provides a method for applying a primer coating composition to a substrate, comprising blending components (A) and (B):

[0063] wherein component (A) comprises an epoxy resin; and

[0064] Component (B) comprises a curing agent;

[0065] wherein at least one of components (A) or (B) comprises a silane; a glycol ether solvent and microspheres, such that when components (A) and (B) are mixed, the resulting primer layer composition comprises 2.0 to 15 wt % of the silane and 1.0 to 9.0 wt % of the microspheres; to form a primer layer composition;

[0066] The composition is applied to a substrate, for example by airless spraying and the coating is optionally allowed to cure. The substrate is desirably a wet and / or rusted substrate.

[0067] Viewed from another aspect, the invention provides a method for applying paint to a wet metal substrate comprising:

[0068] 1) Blending component A and component B;

[0069] wherein component (A) comprises an epoxy resin; and

[0070] Component (B) comprises a curing agent; and wherein at least one of components (A) or (B) comprises a silane, a glycol ether solvent, and microspheres, such that when components (A) and (B) are mixed, the resulting composition comprises 2.0 to 15 wt % of the silane and 1.0 to 9.0 wt % of the microspheres;

[0071] 2) applying the composition to a wet substrate, and

[0072] 3) Allow the composition to form a film and cure.

[0073] Viewed from another aspect, the present invention provides a kit suitable for preparing a primer coating composition as defined above, comprising component (A) and component (B), component (A) comprising:

[0074] (i) Epoxy resin;

[0075] (ii) silane;

[0076] (iii) glycol ether solvents; and

[0077] (iv) microspheres;

[0078] Component (B) comprises at least one curing agent.

[0079] Viewed from another aspect the invention provides the use of a primer coating composition as defined herein for application to a wet and / or rusted substrate.

[0080] In all embodiments, it is preferred that the epoxy resin is a liquid.

[0081] In all embodiments, preferably the solvent comprises propylene glycol n-butyl ether.

[0082] In all embodiments, preferably the silane is an epoxy silane.

[0083] definition

[0084] The present invention relates to a primer coating composition. The term coating composition is used to define a composition formed by a combination of a first composition (component A) and a second composition (component B). In order to prevent premature curing, the primer coating composition of the present invention is provided in two parts: a first composition (component A) comprising an epoxy resin and a second composition (component B) comprising a curing agent. The other components of the composition are preferably present in component (A), but can also be added via component (B). The weight percentages herein are based on the overall primer layer composition. The weight percentages of the components within components (A) and (B) can be easily determined based on the weight percentages in the final primer layer composition and the mixing ratio of components (A) and (B). DETAILED DESCRIPTION

[0085] The present invention relates to a primer coating composition for substrates such as metal substrates, especially steel substrates. The primer coating composition can be applied to a moist, wet or rusted substrate. The substrate can form part of any article to which a primer coating is to be applied, such as a large metal structure.

[0086] The primer coating composition forms an epoxy primer layer on the substrate. The primer layer can be coated with a top coat, a tie coat, an antifouling coating and an expansion coating as required. Therefore, the primer coating of the present invention can be the only layer applied to the substrate, or it can be a layer in a coating system comprising a primer coating and an additional layer. No additional top coat or outer coat is required. However, if the substrate is outside the hull of a ship, it should be understood that the primer will usually be coated with an antifouling paint, and optionally a tie coat between the primer layer and the antifouling layer. In addition, if the substrate is to be exposed to outdoor conditions (e.g., UV radiation from the sun), it is beneficial to apply the primer with a UV-resistant and weather-resistant top coat. The primer coating provides good corrosion protection.

[0087] In one embodiment, the primer coating composition can be applied as a single layer or as two or more layers. Two coats of the primer coating composition can be applied to the substrate. Two different primer coating compositions can also be applied.

[0088] The primer coating composition can also be overcoated with a topcoat. The primer coating composition can also be overcoated with a tie coat and an antifouling coat. The primer coating composition in these embodiments can itself be applied as a single coat or as two coats.

[0089] Suitable systems include:

[0090] 2 coats of primer + top coat.

[0091] 2 primer coats + tie coat + antifouling coat

[0092] 1 primer coat + top coat.

[0093] If the substrate is not the outside of the hull or if the substrate is not exposed to outdoor conditions (UV radiation from sunlight), an overcoat may not be needed. However, in order to ensure the weather resistance and UV resistance of the coating system, the primer coating composition is preferably overcoated with a topcoat. If an overcoat is present, any known overcoat may be used. It should be noted that the coating composition is preferably applied in two coatings, i.e. in two application steps. However, the composition can be applied alone in one coating.

[0094] Primer coating composition

[0095] The specific feature of the primer coating composition of the present invention is the high solid content and thus the low content of volatile organic compounds (VOC). The primer layer coating composition preferably has a solid content of at least 70 wt%, such as at least 75 wt%, more preferably at least 80 wt%. The solid volume (expressed in %) is generally referred to as "VS%". VS% is determined according to ASTM D5201–05a (2020). The primer coating composition has a volume solids % of at least 70%, such as at least 75%, preferably at least 80%.

[0096] High solid volume leads to lower VOC content. The VOC content is preferably 220 g / L or less, more preferably 200 g / L or less, even more preferably 180 g / L or less, such as 160 g / L or less. VOC can be determined theoretically (ASTM D5201-05a (2020)).

[0097] At 23°C, the primer coating composition of the present invention preferably has a pot life of at least 30 minutes, more preferably at least 60 minutes, such as 90 to 120 minutes. Pot life refers to the time after mixing the first and second components (A) and (B) that the composition can still be applied to a substrate by an airless spray process. If the composition cures too quickly, the coating composition has a very short pot life. Considering the time taken to coat large objects (such as ship hull sections) and the hose length of up to 150m supplying the spray gun, a pot life of less than 30 minutes is commercially challenging.

[0098] Many of the important properties of the compositions of the present invention are a result of the high solids and relatively low viscosity of the claimed compositions.

[0099] The viscosity of the primer coating composition measured immediately after mixing of the two components may be from 200 mPas to 1100 mPas at 23°C, such as from 200 mPas to 1000 mPas, especially from 450 mPas to 800 mPas.

[0100] It should be understood that the composition cures over time and therefore the viscosity of the composition increases during curing. The viscosity is the initial viscosity measured immediately after mixing and therefore before any significant degree of curing process occurs. Immediately after mixing means within 10 minutes after mixing.

[0101] The viscosity of the primer coating composition measured after 60 minutes is desirably less than 2200 mPas, more desirably less than 2000 mPas.

[0102] The pigment volume concentration of the primer coating composition of the present invention is preferably 30% to 45%, such as 32% to 42%.

[0103] Epoxy resin

[0104] The primer coating composition comprises a binder based on at least one epoxy resin. Mixtures of epoxy resins may also be used. If multiple epoxy resins are used, it is the combination of these epoxy resins that forms the binder in the primer layer composition.

[0105] Shortly before applying the primer layer composition to the substrate, a first composition (component A) containing an epoxy resin is mixed with a second composition (component B) containing a curing agent to form a primer layer composition. The primer layer composition is then applied to the substrate and cured to form a primer layer on the substrate.

[0106] The binder in the primer layer composition may include one or more than one epoxy resin. Ideally, the primer layer composition includes at least one liquid epoxy resin. The term liquid refers to the state of the epoxy resin at room temperature and 23° C., and a pressure of 1 atm.

[0107] The terms epoxy resin or epoxy adhesive are used interchangeably herein. Preferably, the epoxy resin is an aromatic or aliphatic epoxy adhesive, preferably containing more than one epoxy group per molecule. The epoxy groups may be in internal or terminal positions on the epoxy adhesive or bonded to a cyclic structure in the epoxy adhesive. Preferably, the epoxy adhesive contains at least two epoxy groups so that a cross-linked network can be formed.

[0108] It should be understood that the epoxy adhesives of the present invention also include adhesives having a conventional epoxy backbone but in which the epoxy end groups have been modified with acrylic or methacrylic functional groups which can be cured with the same curing agents as the epoxy groups.

[0109] Suitable aliphatic epoxy adhesives include epoxy adhesives and modified epoxy adhesives selected from alicyclic diglycidyl ethers, such as diglycidyl ethers based on hydrogenated bisphenol A, hydrogenated bisphenol F and dicyclopentadiene-based adhesives, glycidyl ethers, such as polyglycidyl ethers of polyols, epoxy-functional acrylic resins or any combination thereof.

[0110] Suitable aromatic epoxy adhesives include epoxy adhesives and modified epoxy adhesives selected from bisphenol type epoxy adhesives such as diglycidyl ethers of bisphenol A, bisphenol F and bisphenol S, resorcinol diglycidyl ether (RDGE), novolac type epoxy adhesives such as epoxy phenol novolac resins, epoxy cresol novolac resins and bisphenol A epoxy novolac resins, glycidyl ethers of dihydroxynaphthalene or any combination thereof.

[0111] In a preferred embodiment, the epoxy-based adhesive is an aromatic epoxy-based adhesive.Preferably, the aromatic epoxy-based adhesive is derived from a combination of a compound comprising at least one epoxy functional group and an aromatic co-reactant comprising at least two hydroxyl groups.

[0112] Preferred epoxy adhesives are bisphenol epoxy adhesives. Preferred epoxy-based adhesives are bisphenol A and bisphenol F epoxy adhesives or bisphenol A / F epoxy adhesives. In preferred embodiments, the epoxy-based adhesive is a bisphenol A epoxy resin, and most preferably, the epoxy-based adhesive is an epoxy resin based on unmodified liquid bisphenol A.

[0113] The epoxy-based adhesive may be a modified epoxy-based adhesive. Preferably, the epoxy-based adhesive is modified with fatty acid, polypropylene oxide and / or polyethylene oxide, acrylic acid, carboxylic acid or carboxyl-terminated butadiene acrylonitrile (CTBN).

[0114] The solid content of the epoxy-based adhesive is preferably greater than 70 wt%, preferably greater than 80 wt%, preferably greater than 90 wt%, and most preferably greater than 99 wt%. In another preferred embodiment, the epoxy-based adhesive contains no solvent.

[0115] Examples of suitable commercially available epoxy-based adhesives are:

[0116] -Bisphenol A epoxy adhesives: DER331 and DER332 from Olin Epoxy

[0117] - Adhesives based on bisphenol F epoxy resin: Epikote 862 from Hexion, DER354 from Olin Epoxy.

[0118] - A mixture of bisphenol A and bisphenol F epoxy adhesives: DER352 from Olin Epoxy, Epikote 235 from Hexion.

[0119] The epoxy adhesive can be a liquid epoxy adhesive, a semi-solid epoxy adhesive, or a solid epoxy adhesive or a combination thereof. It should be understood that "liquid" and "solid" refer to the physical state of the epoxy adhesive at ambient temperature and pressure (23°C and 1 atm). In a preferred embodiment, the epoxy adhesive is a liquid epoxy adhesive. In a preferred embodiment, the epoxy adhesive is a liquid bisphenol A epoxy resin.

[0120] The epoxy-based adhesive may have an epoxy equivalent weight (EEW) value of 140 to 1000. The EEW is particularly preferably less than 500, for example 150 to 270, especially 160 to 200.

[0121] The number of "epoxy equivalents" is the sum of the contributions from each of the one or more epoxy resins and any other components containing epoxides, such as silanes and reactive diluents. The contribution of each of the one or more epoxy resins to the epoxy equivalents is defined as the grams of epoxy resin divided by the epoxy equivalent weight of the epoxy resin, where the epoxy equivalent weight of the epoxy resin is determined as: grams of epoxy resin equals 1 mol of epoxide groups. For adducts with epoxy resins, the contribution of the reactants prior to adducting is used to determine the number of "epoxy equivalents" in the epoxy-based adhesive system.

[0122] The viscosity of the liquid epoxy-based adhesive is preferably 1000 to 20000 mPas, more preferably 2000 to 15000 mPas. Most preferably, a liquid bisphenol A type epoxy-based adhesive is used.

[0123] If liquid, semi-solid and solid epoxy adhesives are present in the epoxy adhesive system, preferably the liquid epoxy adhesive is in excess relative to the semi-solid and / or solid epoxy adhesive.

[0124] The epoxy resin is preferably present in an amount of 5.0 to 40 wt % of the primer coating composition, such as 10 to 40 wt % of the primer coating. More preferably, the epoxy resin is present in an amount of 20 to 40 wt %, especially 20 to 30 wt %. If a blend of epoxy resins is used, these percentages refer to the total epoxy resin content, i.e., the weight percentages of each are added together.

[0125] In a preferred embodiment, the epoxy adhesive comprises a bisphenol A based adhesive, such as 4,4'-isopropyldiphenol-epichlorohydrin resin, a bisphenol F based adhesive and / or a novolac based adhesive. In a preferred embodiment, the epoxy adhesive system comprises one or more bisphenol A epoxy based adhesives. Bisphenol A epoxy based adhesives are known to those skilled in the art and have the following general structure.

[0126]

[0127] In one embodiment, the epoxy-based adhesive system comprises one or more bisphenol F epoxy-based adhesives.

[0128] The bisphenol F epoxy-based adhesive may have an EEW value of 100 to 350. However, it is particularly preferred that the EEW is 300 or less, such as 100 to 300, especially 150 to 200. Preferably, the bisphenol F epoxy-based adhesive is a liquid.

[0129] The Mw of the bisphenol F resin may be greater than 300 g / mol. Preferred bisphenol F (4',4'-methylene bisphenol) epoxy adhesives are derived from a combination of bisphenol F and epichlorohydrin. The use of difunctional epoxy bisphenol F adhesives is particularly preferred.

[0130] Combinations of two or more bisphenol F adhesives may be used. The viscosity of the bisphenol F adhesive is preferably from 1000 to 10000 mPas, more preferably from 2000 to 5000 mPas.

[0131] Silane

[0132] The coating composition of the present invention further comprises at least one silane. Silanes can improve the drying performance at low temperatures, flexibility, adhesion to the substrate and corrosion resistance.

[0133] The silane may be provided as part of component A and / or as part of component B (preferably component A). Ideally, the silane is a silane containing epoxy groups. The silanes used in the present invention generally have a low Mw, such as less than 400 g / mol. Suitable silanes have the general formula (III) or (IV)

[0134] Y 2 (4-z) SiX z (III ) or

[0135] Y 2 (3-y) R 1 SiX y (IV)

[0136] Wherein, z is an integer from 1 to 3,

[0137] Wherein, y is an integer from 1 to 2,

[0138] R 2 is an alkylene radical having 1 to 12 C atoms, which optionally contains an ether or amino linker,

[0139] R 1 is a hydrocarbon radical having 1 to 12 C atoms;

[0140] Y is a functional group bonded to R which can react with a corresponding hardener or binder functional group and is preferably an amine or epoxy group, and

[0141] Each X independently represents a halogen group or an alkoxy group.

[0142] Isocyanate, epoxide, glycidyl ether, amino, hydroxyl, thiol, carboxyl, acrylate or methacrylate groups are preferred as functional group Y. The Y group may be bound to any part of the chain R. It will be appreciated that when Y represents an epoxy group, then R will have at least two carbon atoms to allow the formation of an epoxide ring system.

[0143] Particularly preferably, Y is an amino group or an epoxy group. The amino group is preferably NH2. Y is preferably an epoxy group.

[0144] If the Y group is an epoxide, then preferably the silane is provided separately from the amine based curing agent composition, for example together with an epoxy adhesive.Generally, in the kit of the invention the silane should not react with any component of the kit composition in which the silane is present.

[0145] Particularly preferably, X is an alkoxy group, such as a C1-6 alkoxy group, especially a methoxy group or an ethoxy group. It is also particularly preferred that two or three alkoxy groups are present. Thus, z is ideally 2 or 3, especially 3. The subscript y is preferably 2.

[0146] R 1 Preferably C 1-4 Alkyl groups, such as methyl.

[0147] R 2 is an alkylene radical having up to 12 carbon atoms. An alkylene radical refers to a radical containing only C and H atoms. It may contain an alkylene chain or a combination of an alkylene chain and a ring such as a phenylene or cyclohexylene ring. The term "optionally containing an ether or amino linker" means that the carbon chain may be interrupted by an -O- or -NH- group in the chain, for example to form silanes such as [3-(2,3-epoxypropoxy)propyl]trimethoxysilane: H2COCHCH2OCH2CH2CH2Si(OCH3)3. It is preferred if the group Y is not bound to a carbon atom to which such a linker as -O- or -NH- is bound.

[0148] Therefore, R 2 It can represent -(C6H4)-NH-(CH2)3- or (C6H4)-(CH2)3, etc.

[0149] R 2 Preferred are unsubstituted (obviously except for Y), unbranched alkylene chains having 2 to 8 C atoms, optionally containing ether or amino linkers.

[0150] Thus, a preferred silane formula has structure (V)

[0151] Y'-R 3 (4-z’) SiX' z’ (V)

[0152] Where z' is an integer from 2 to 3, R 3 is an unsubstituted, unbranched alkylene chain having 2 to 8 C atoms, optionally containing an ether or amino linker, and Y' is bonded to R 3 The amino or epoxy functional group on the group, and X' represents an alkoxy group.

[0153] Examples of such silanes are the many representatives of the following: products sold under the trade name Dynasylan(R) manufactured by Evonik Industries AG, Silquest(R) silanes manufactured by Momentive, and GENIOSIL(R) silanes manufactured by Wacker.

[0154] Specific examples include methacryloxypropyltrimethoxysilane (Dynasylan MEMO, Silquest A-174NT), 3-mercaptopropyltri(methyl)ethoxysilane (Dynasylan MTMO or 3201; Silquest A-189), (3-glycidyloxypropyl)trimethoxysilane (Dynasylan GLYMO, Silquest A-187), (3-glycidyloxypropyl)triethoxysilane (Dynasylan GLYEO), tris(3-trimethoxysilylpropyl)isocyanurate (Silquest Y11597), β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (Silquest A-186), γ-isocyanatopropyltrimethoxysilane (Silquest A-Link 35, Geniosil GF40), (methacryloyloxymethyl)trimethoxysilane (Geniosil XL 33), isocyanatomethyl)trimethoxysilane (Geniosil XL43), (3-aminopropyl)trimethoxysilane (Dynasylan AMMO; Silquest A-1110, (3-aminopropyl)triethoxysilane (DynasylanAMEO) or N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (Dynasylan DAMO, Silquest A-1120) or N-(2-aminoethyl)-3-aminopropyltriethoxysilane, triaminofunctional 3-[2-(2-aminoethylamino)ethylamino]propyltrimethoxysilane (Silquest A-1130), bis[3-(trimethoxysilyl)propyl]amine (Silquest A-1170), N-ethyl-3-trimethoxysilyl-2-methylpropylamine (Silquest A-Link 15), N-phenyl-3-aminopropyltrimethoxysilane (Silquest Y-9669), 4-amino-3,3-dimethylbutyltrimethoxysilane (Silquest Y-11637), (N-cyclohexylaminomethyl)triethoxysilane (Geniosil XL 926), (N-phenylaminomethyl)trimethoxysilane (Geniosil XL 973), Deolink Epoxy TE and Deolink Amino TE (DOG Deutsche Oelfabrik) and mixtures thereof. Oligomeric epoxy silanes, such as Coatosil MP 200 from Momentive, can also be used in the composition.

[0155] Specific silanes of interest include (3-glycidoxypropyl)triethoxysilane (H2COCHCH2OCH2CH2CH2Si(OCH2CH3)3, (3-glycidoxypropyl)trimethoxysilane (H2COCHCH2OCH2CH2CH2Si(OCH3)3).

[0156] Particular preference is given to using the silane (3-glycidyloxypropyl)trimethoxysilane. It is also possible to use mixtures of silanes.

[0157] The amount of silane present in the primer layer composition may be 2.0 to 15 wt %, preferably 2.5 to 10 wt %, more preferably 2.5 to 8.0 wt %, ideally 3.0 to 7.0 wt %, based on the total weight. If a blend of silanes is used, these percentages refer to the total silane content.

[0158] Therefore, the use of this amount of silane ensures that the primer layer composition of the present invention adheres to the underlying substrate, even when the substrate is wet or rusty when the composition is applied. If the content of silane in the primer layer composition is less than 2.0 wt%, adhesion failure occurs when the composition is applied to the target substrate.

[0159] Curing agent

[0160] The primer coating composition of the present invention comprises at least one curing agent. Ideally, it is based on amine and is not modified in any way to increase its compatibility with water. That is, there is no hydrophilic structural segment such as a polyether segment in the molecular structure of the curing agent. The curing agent is preferably selected from N-benzylated polyalkyleneamines, amine-epoxy adducts and / or phenalkamines.

[0161] Most preferably, the curing agent is a polyamine containing at least two amino groups. In order to obtain a crosslinked network, the curing agent must contain at least three "reactive" hydrogen atoms. "Reactive" hydrogen atoms refer to hydrogen atoms that are transferred from nucleophiles to the oxygen atoms of the epoxide during the ring-opening reaction. Therefore, the curing active amine group cannot be a tertiary amine. However, compounds containing tertiary amines can be added to the composition as curing accelerators. The curing agent usually contains at least two curing reactive functional groups.

[0162] In one embodiment, the curing agent comprises a benzylamine motif:

[0163]

[0164] The benzylamine in the curing agent may be optionally substituted on the ring, methylene linker, or N atom, although one active hydrogen must be retained. Suitable substituents include C1-15 alkyl, OH, O-C1-4-alkyl, halogen, cyano, amine and alkylamine groups (C1-4-N).

[0165] In a preferred embodiment, the curing agent is a polyamine curing agent comprising one or more benzylamine structures.

[0166] More specifically, the curing agent comprises two or more repeating units, that is, the curing agent is a polymer or an oligomer. Preferably, the curing agent is a polyamine polymer comprising a benzylamine structure on at least one end of the polyamine polymer chain. The polyamine polymer may comprise a benzylamine structure at both ends of the polymer chain. Each repeating unit may also comprise a benzylamine group. The benzylamine group may be substituted or unsubstituted.

[0167] In a preferred embodiment, the curing agent comprises at least two or more benzylamine structures.

[0168] In one embodiment, the curing agent comprises a benzylated polyalkylene polyamine structure as described in WO2017147138A. The benzylated polyalkylene polyamine structure preferably has a structure as shown below:

[0169]

[0170] Where R 1 is a substituted or unsubstituted benzyl group;

[0171] R 2 Independently selected from R 1 or a hydrogen atom or a group selected from C1-C16 linear, cyclic or branched alkyl, alkenyl and alkylaryl groups;

[0172] X, Y and Z are independently selected from C2-C10 alkylene and cycloalkylene, preferably ethylene, propylene, butylene, hexylene, cyclohexyl dimethylene and cyclohexylene;

[0173] y is an integer from 1 to 7;

[0174] z is an integer from 0 to 4.

[0175] Examples of suitable benzylated polyalkylene polyamine structures are benzylated polyethylene polyamines, benzylated polypropylene polyamines, benzylated polyethylene-polypropylene polyamines, and combinations thereof.

[0176] The limiting examples of polyethylene polyamines include ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), and other higher polyethylene polyamines. Suitable polypropylene polyamines include but are not limited to propylenediamine (PDA), dipropylenetriamine (DPTA), tripropylenetetramine and other higher polypropylene polyamines. Other polyalkylene polyamines include N-3-aminopropyl ethylenediamine, N, N'-bis (3-aminopropyl) ethylenediamine and N, N, N'-tri (3-aminopropyl) ethylenediamine, N-3-aminopropyl diethylenetriamine, N-3-aminopropyl-[N'-3-[N-3 aminopropyl] aminopropyl] diethylenetriamine, N, N'-bis (3-aminopropyl) diethylenetriamine, N, N-bis (3-aminopropyl) diethylenetriamine, N, N, N'-tri (3-aminopropyl) The invention also includes the following: N,N',N"-tris(3-aminopropyl)diethylenetriamine, N,N',N"-tris(3-aminopropyl)diethylenetriamine, N,N,N',N'-tetrakis(3-aminopropyl)diethylenetriamine, N,N-bis(3-aminopropyl)-[N'-3-[N-3-aminopropyl]aminopropyl]-[N'-3-aminopropyl]diethylenetriamine, and N-3-aminopropyl-[N'-3-[N-3-aminopropyl]aminopropyl]-[N'-3-aminopropyl]diethylenetriamine.

[0177] The benzylated polyalkylene polyamine structures are generally prepared by reductive amination of benzaldehydes (including both substituted and unsubstituted benzaldehydes) with polyalkylene polyamines. Examples of substituted benzaldehydes are benzaldehydes in which the aromatic ring is substituted with one or more halogen atoms, C1-C4 alkyl, methoxy, ethoxy, amino, hydroxyl or cyano groups. Preferred benzaldehydes are benzaldehyde and vanillin.

[0178] In another embodiment, the curing agent is an amine epoxy adduct, such as an adduct prepared by reacting a bisphenol A epoxy resin with a primary diamine. The amine epoxy adduct can be synthesized, for example, by reacting an epoxy resin with an excess of a primary diamine at 40° C. to 100° C. The reaction typically occurs in a solvent such as n-butanol or benzyl alcohol.

[0179] Preferably, bisphenol A epoxy resin has an EEW of less than 250 g / eq. Suitable primary diamines for synthesizing amine epoxy adducts can be ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), and other higher polyethylene polyamines. Aliphatic primary diamines such as 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,5-diamino-2-methylpentane, 1,6-hexanediamine and 2,2,4 (2,4,4)-trimethyl-1,6-hexanediamine can also be used. Primary diamines containing cyclic structures can also be used, such as 1,4-diaminocyclohexane, isophorone diamine (IPDA), 1,3-bis (aminomethyl) cyclohexane, 1,4-bis (aminomethyl) cyclohexane, 1,3-bis (aminomethyl) benzene, and 1,4-bis (aminomethyl) benzene. In a preferred embodiment, the primary diamine is a mixture of 1,5-diamino-2-methylpentane and isophoronediamine (IPDA).

[0180] The amine epoxy adduct preferably has an average molecular weight of 500 to 3000 g / mol, more preferably 600 to 2000 g / mol.

[0181] In another embodiment, the curing agent is a reaction product of phenol, formaldehyde and a primary diamine such as a Mannich base. The phenol can be an unsubstituted or substituted phenol, such as an alkylphenol, and in one embodiment, the phenol is cardanol. When the phenol is cardanol, the curing agent is called a phenalkamine. Mannich bases and phenalkamine curing agents are particularly suitable as curing agents under low temperature conditions (such as below 10°C). Therefore, the use of a phenalkamine curing agent forms a preferred aspect of the present invention.

[0182] In principle, any primary diamine can be used to synthesize phenalkamine curing agent. The non-limiting examples of primary diamines include ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA) and other advanced polyethylene polyamines. Aliphatic primary diamines such as 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,5-diamino-2-methylpentane, 1,6-hexanediamine and 2,2,4 (2,4,4)-trimethyl-1,6-hexanediamine. Primary diamines comprising cyclic structures can also be used, such as isophorone diamine (IPDA), 1,3-bis (aminomethyl) cyclohexanes, 1,4-bis (aminomethyl cyclohexanes), 1,3-bis (aminomethyl) benzenes and 1,4-bis (aminomethyl) benzenes. Phenalkamines based on 1,3-bis (aminomethyl) benzenes and ethylenediamines are preferred.

[0183] In another embodiment, the curing agent is not a polyoxyalkylene amine, such as a Jeffamine type curing agent.

[0184] In another embodiment, the curing agent is not a ketimine or aldimine.Ketimine or aldimine curing agents include the reaction product of reactants comprising a polyalkylpolyamine component and a ketone or aldehyde component.

[0185] In a preferred embodiment, the curing agent does not comprise polyoxyalkylene amines or ketimines or aldimines.

[0186] In a preferred embodiment, the curing agent composition is a mixture of an N-benzylated alkyleneamine and an amine epoxy adduct as described above, for example, mixed in a weight ratio of 40:60 to 60:40.

[0187] The curing agent composition preferably has an active hydrogen equivalent weight (AHEW) of 50-200 g / eq, more preferably 70-150 g / eq, most preferably 90-110 g / eq.

[0188] The number of "active hydrogen equivalents" for one or more curing agents is the sum of the contributions from each of the one or more curing agents. The contribution of each of the one or more curing agents to the active hydrogen equivalents is defined as the number of grams of curing agent divided by the active hydrogen equivalent of the curing agent, where the active hydrogen equivalent of the curing agent is determined as: grams of curing agent is equivalent to 1 mole of active hydrogen.

[0189] Preferably, the ratio of the hydrogen equivalent of the entire curing agent to the epoxy equivalent of the entire curing agent is in the range of 50:100 to 120:100.

[0190] Particularly preferred epoxy-based coating compositions have a ratio between the active hydrogen equivalent of the curing agent and the epoxy equivalent of the composition in the range of 60:100 to 110:100, such as 70:100 to 105:100, such as 80:100 to 95:100.

[0191] The viscosity of the curing agent composition is preferably between 200 mPas and 5000 mPas, more preferably 400 mPas to 2500 mPas, most preferably 500 mPas to 1500 mPas.

[0192] The curing agent is preferably present in an amount of 5.0 to 40 wt % of the primer coating composition, such as 8.0 to 40 wt % of the primer coating composition. More preferably, the curing agent is present in an amount of 10 to 30 wt %, especially 10 to 25 wt % of the primer coating composition. If a blend of curing agents is used, these percentages refer to the total curing agent content in the primer layer composition.

[0193] Commercial curing agents used in the present invention include Ancamine 1618, Ancamine 2422, Ancamine 2432, Ancamine 2519, Ancamine 2738, Ancamine 2739, Ancamine 2712M, all from Evonik, and NX-5594, GX-5135, GX-6027, NX-6654, NC-540, NC-541, NC-541LV, LITE 2001, LITE 2001LV and LITE 2002, all from Cardolite.

[0194] Solvents

[0195] The primer coating composition of the present invention comprises at least one glycol ether solvent. It has been found that the use of a glycol ether solvent enables a long pot life and is also important for allowing the primer layer composition to be applied to wet or rusted substrates. It also acts as a wetting agent for the extender in the formulation. Thus, this solvent ensures that the primer layer composition of the present invention adheres to the underlying substrate, even when the substrate is wet or rusted when the composition is applied. The glycol ether solvent should be liquid at room temperature and pressure (1 atm, 23°C).

[0196] The glycol ether solvent may be provided as part of Component A and / or as part of Component B (preferably Component A).

[0197] The glycol ether solvent of the present invention is preferably a solvent of formula (I):

[0198] R-[O-R'] x -OH (I)

[0199] Wherein, x is 1 to 3;

[0200] R is C1-C 16 Aliphatic groups; and

[0201] R' is C1-C 16 Aliphatic group.

[0202] Preferably, R and R' are independently C1-C 16 Straight-chain, cyclic or branched alkyl groups, such as C1-C 16 A straight chain or branched chain alkyl group.

[0203] Preferably, R and R' are independently C1-C8 linear, cyclic or branched alkyl groups, such as C1-C8 linear or branched alkyl groups.

[0204] Preferably, R and R' are independently C1-C6 linear or branched alkyl. Preferably, R' is an ethylene or propylene repeat unit. Preferably, x is 1 or 2, especially 1. If x is 2 or 3, then preferably all R' groups are the same.

[0205] Preferably, R is a C2-C8 linear, cyclic or branched alkyl group, such as a C2-C8 linear or branched alkyl group. Preferably, R is a C2-C6 linear or branched alkyl group.

[0206] The glycol ether solvent of the present invention is preferably a solvent of formula (II):

[0207] RO-R'-OH (II)

[0208] wherein R is a C1-C8 linear or branched alkyl group; and

[0209] R' is ethylene or propylene.

[0210] In a preferred embodiment, the solvent is an ethylene glycol ether or a propylene glycol ether, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monophenyl ether, propylene glycol methyl ether, propylene glycol monoethyl ether, propylene glycol n-propyl ether, propylene glycol n-butyl ether, propylene glycol phenyl ether, dipropylene glycol n-propyl ether, dipropylene glycol n-butyl ether or tripropylene glycol n-butyl ether.

[0211] In a preferred embodiment, the solvent comprises propylene glycol n-butyl ether.

[0212] The glycol ether solvent preferably has a boiling point of 250°C or less, preferably 50 to 200°C, such as 90 to 180°C.

[0213] The glycol ether solvent preferably has an Mw of 50 to 400 g / mol, more preferably 80 to 200 g / mol.

[0214] Other solvents may also be present. Other suitable solvents include aromatic hydrocarbons, aliphatic hydrocarbons, ketones, esters, alcohols and ethers. Examples of hydrocarbon solvents include toluene, xylene, light aromatic solvent naphtha [C8-C10] (Solvesso 100) and mineral spirits. Examples of ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, methyl isoamyl ketone. Examples of esters include ethyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, tert-butyl acetate and propylene glycol methyl ether acetate. Examples of alcohols include ethanol, propanol, isopropanol, n-butanol, isobutyl alcohol, sec-butyl alcohol, tert-butyl alcohol and benzyl alcohol.

[0215] Preferably xylene or n-butyl acetate or t-butyl acetate is mixed with the glycol ether solvent to achieve the desired surface tolerance and pot life of the coating composition. More preferably, the glycol ether solvent is propylene glycol ether for health and safety reasons. Propylene glycol ether has a good viscosity reducing effect on the composition. Dipropylene glycol ether and tripropylene glycol ether can be used, but (mono) propylene glycol ether is preferred due to the evaporation rate. Most preferably propylene glycol n-butyl ether.

[0216] The amount of glycol ether solvent (e.g., solvent of formula (I)) in the primer coating composition is 1.0 to 15 wt%, preferably 1.0 to 10 wt%, more preferably 2.0 to 8.0 wt%, ideally 2.0 to 6.0 wt%, based on the total weight of the coating composition. If a blend of glycol ether solvents is used, these percentages refer to the total content of any glycol ethers present.

[0217] The total amount of solvent in the primer coating composition is 2.0 to 15 wt%, preferably 5.0 to 15 wt%, more preferably 5.0 to 12 wt%, ideally 7.0 to 10.5 wt%, based on the total weight of the coating composition.

[0218] Microspheres

[0219] Primer coating compositions of the present invention include microspheres, such as organic or inorganic microspheres. These microspheres may be coated or uncoated. These microspheres may be hollow or solid. Suitable microspheres are glass beads, uncoated or coated hollow and solid ceramic beads, polymeric materials such as poly(methyl methacrylate), poly(methyl methacrylate-co-ethylene glycol dimethacrylate), poly(styrene-co-ethylene glycol dimethacrylate), poly(styrene-co-divinylbenzene), polystyrene, poly(vinyl chloride), poly(vinylidene fluoride) and poly(vinylidene chloride) beads.

[0220] Examples of commercially available hollow organic spherical filler particles are Grades E030, E055, E065-135D, E130-055D, E130-095D, E130-105D, E130-040D, E035-FR and E135-025D, all from Chase Corporation.

[0221] Preferably, the primer coating composition comprises solid or hollow inorganic spherical microspheres. Suitable solid or hollow, inorganic, spherical filler particles are commercially available. Examples of commercially available hollow, inorganic, spherical filler particles include Glass Bubbles S28HS, Micro Bubbles H38HS, Fillite Cenosphere, Poraver (expansion glass), Eccospheres, Q-Cel, Sphericel, Thermospheres, Omega shperes (available from, for example, 3M, SMC Minerals, Omya, Poraver, Trelleborg, Potters, Omega) and hollow glass spheres from Hollowlite.

[0222] Preferably the inorganic spherical microparticles are hollow. This means that the particles have a void or cavity in their center. The void or empty space is filled with a gas, preferably air. Preferred inorganic spherical filler particles for use in the present invention are substantially hollow. Therefore, preferably, the volume of the void or cavity is at least 70 vol% and more preferably at least 80 vol% of the total volume of the particles.

[0223] Preferably, the microspheres have a density as low as possible, for example, as indicated in the technical instructions provided by the supplier, the density of the microspheres may be, for example, 0.1-1 g / cm 3 , more preferably 0.2-0.8g / cm 3 , and still more preferably 0.3-0.5 g / cm 3 This may reflect the fact that the particles are hollow rather than solid.

[0224] Thus, the microspheres can ensure that the primer layer composition has a low density and high volume solids.Using microspheres, especially hollow microspheres, it is possible to keep the binder content low while keeping the filler content high.

[0225] Preferably, the microspheres present in the coating composition of the present invention have an isostatic compressive strength of at least 5000 psi, such as specified by the supplier in the technical data sheet. This is beneficial because it means that the filler particles are not crushed during processing and thus retain their ability to provide a low density coating composition. It is also advantageous that the microspheres do not change shape and / or size during processing so that they can be densely packed and achieve high build in the final coating formed.

[0226] The microspheres present in the coating composition of the present invention comprise glass, ceramic or plastic, and are more preferably composed of them. More preferably, the microspheres in the coating composition of the present invention comprise glass, and are also more preferably composed of them. This is because glass particles provide a good balance of compressive strength, hardness and conductivity. Optionally, the microspheres present in the coating composition of the present invention can be surface treated. Some examples of surface treatment include treatments for changing the hydrophobicity of the surface, improving compatibility with adhesives and / or promoting the incorporation of chemicals into the adhesive. Preferably the particles are treated with vinyl silane.

[0227] Therefore, in a preferred embodiment, the microspheres of the present invention are vinyl silane treated microspheres.

[0228] The microspheres present in the coating composition of the present invention are substantially spherical, and more preferably spherical. This is advantageous because it allows the particles to be packed more closely together in the coating composition of the present invention.

[0229] Viewed alternatively, the microspheres have a D10 diameter of 1 to 40 μm, more preferably 5 to 35 μm and even more preferably 10 to 30 μm, as determined by ISO 13320:2009 using a Malvern Mastersizer 2000.

[0230] Viewed alternatively, the microspheres have a D50 diameter of 10 to 80 μm, more preferably 20 to 70 μm and even more preferably 30 to 55 μm, as determined by ISO 13320:2009 using a Malvern Mastersizer 2000.

[0231] Preferably, the microspheres have a D90 diameter, determined by ISO 13320:2009 using a Malvern Mastersizer 2000, of 30 to 150 μm, more preferably 50 to 90 μm and even more preferably 50 to 80 μm.

[0232] Based on the total weight of the composition, the preferred coating composition of the present invention comprises 1.0-9.0 wt%, more preferably 2.0-8.0 wt%, and even more preferably 2.0-7.0 wt% microspheres. If the microsphere content exceeds the range in claim 1, the composition may fail the cathodic disbonding test.

[0233] Thus, this amount of microspheres ensures that the primer layer composition of the present invention provides corrosion protection to the underlying substrate, even when the substrate is wet or rusty when the composition is applied.

[0234] The microspheres may be provided as part of component A and / or as part of component B (preferably component A).

[0235] Hydrocarbon resin

[0236] The primer coating composition of the present invention may also include a hydrocarbon resin. A wide range of hydrocarbon resins are suitable for inclusion in the coating composition. The hydrocarbon resin may be a petroleum resin or a xylene formaldehyde resin.

[0237] Examples of petroleum resins suitable for use in the present invention include aromatic petroleum resins obtained by polymerizing a C9 fraction obtained from heavy oil produced as a by-product via naphtha cracking (e.g., a styrene derivative such as α-methylstyrene, o-, m-, p-cresol, indene, methylindene, cumene, naphthalene or vinyltoluene), and aliphatic petroleum resins obtained by polymerizing a C5 fraction such as 1,3-pentadiene or isoprene, 2-methyl-2-butene, cyclopentadiene, dicyclopentadiene or cyclopentene.

[0238] In the present invention, copolymer-type petroleum resins obtained by copolymerizing C9 fractions and C5 fractions, aliphatic petroleum resins in which a part of the conjugated dienes of the C5 fraction, such as cyclopentadiene or 1,3-pentadiene, are cyclically polymerized, resins obtained by hydrogenating aromatic petroleum resins, and alicyclic petroleum resins obtained by polymerizing dicyclopentadiene can also be used. Mixtures of diaryl and triaryl compounds obtained from the reaction of C9 blends under catalytic conditions can also be used.

[0239] Preferably, the hydrocarbon resin is a resin obtained by polymerizing a C9 fraction.The hydrocarbon resin may or may not contain OH-functional groups.

[0240] The hydrocarbon resin may have a viscosity of 10 to 10000 mPas. More preferably the low viscosity is 20-5000 mPas, most preferably 40-200 mPas.

[0241] The primer coating composition of the present invention preferably comprises 0 to 10 wt% hydrocarbon resin based on the total weight of the composition, preferably 2.0 to 7.0 wt% based on the total weight of the composition. If a blend of hydrocarbon resins is used, these weight percentages refer to the total content of the hydrocarbon resin.

[0242] The hydrocarbon resin may be provided as part of component A and / or as part of component B (preferably component A).

[0243] Examples of suitable commercially available hydrocarbon resins are Novares TL10, Novares LC 15, Novares L 100, and Novares LA 300 from Rain Carbon Inc., Hirenol PL-150 and Hikotack LP-9800S from Kolon Industries, and Epodil LV5 from Evonik.

[0244] Reactive diluent

[0245] The primer layer coating composition may further comprise a reactive diluent, preferably formed from a modified epoxy compound.

[0246] Examples of such reactive diluents include phenyl glycidyl ether, alkyl glycidyl ether (number of carbon atoms in the alkyl group: 1 to 16), glycidyl ester of Versatic acid (R 4 R 5 R 6 C-COO-Gly, where R 4 R 5 R 6 is an alkyl group such as C8 to C10 alkyl group and Gly is a glycidyl group), olefin epoxides (CH3-(CH2)n-Gly, wherein n=11 to 13, Gly: glycidyl group), 1,6-hexanediol diglycidyl ether (Gly-O-(CH2)6-O-Gly), neopentyl glycol diglycidyl ether (Gly-O-CH2-C(CH3)2-CH2-O-Gly), trimethylolpropane triglycidyl ether (CH3-CH2-C(CH2-O-Gly)3), and C1-20-alkylphenyl glycidyl ethers (preferably C1-5 alkylphenyl glycidyl ethers), such as methylphenyl glycidyl ether, ethylphenyl glycidyl ether, propylphenyl glycidyl ether and neodecanoic acid glycidyl ester. Another preferred option is Cardolite NC-513 derived from the reaction of epichlorohydrin with oil obtained from cashew nut shells.

[0247] Among the above reactive diluents, preferred are aliphatic reactive diluents. Preferably, the aliphatic reactive diluent is formed by the reaction of a compound containing at least one aliphatic epoxy functional group with an aliphatic alcohol or polyol, such as 1,6-hexanediol diglycidyl ether or 1,4-butanediol diglycidyl ether. Aliphatic glycidyl ethers with a chain length of 8-14 are also preferred. Preferred reactive diluents may be aliphatic because they contribute to the flexibility of the coating. p-TBPGE (p-tert-butylphenyl glycidyl ether) may also be used.

[0248] Preferably, the reactive diluent is multifunctional rather than monofunctional as this speeds up the drying process and increases the crosslinking density. This also contributes to better anti-corrosion properties.

[0249] The above-mentioned reactive diluents may be used alone or in combination of two or more diluents.

[0250] In the primer layer composition as a whole, the reactive diluent is desirably contained in an amount of 0 to 20% by weight, preferably 1.0 to 15% by weight, for example 2.0 to 10 wt%, especially 2.0 to 7.0 wt%. If a blend of reactive diluents is used, these percentages refer to the total content of the reactive diluent.

[0251] By adding the reactive diluent in the above amount, the viscosity of the primary primer layer composition is reduced to allow preparation of a high solid composition.

[0252] Preferably, the viscosity of the reactive diluent measured by the cone and plate method according to ISO 2884-1:2006 at 23°C and 50% RH is <100 cP, preferably <50 cP, most preferably <30 cP.

[0253] The epoxide equivalent weight (EEW) of the reactive diluent is preferably 100-500 g / eq, preferably 100-300 g / eq, most preferably 120-170 g / eq.

[0254] The reactive diluent may be provided as part of component A and / or as part of component B (preferably component A).

[0255] Fillers and Pigments

[0256] The coating composition optionally contains fillers, color pigments and anti-corrosion pigments.

[0257] Fillers include organic and inorganic fillers, the latter may be naturally occurring, ie mined, or of synthetic origin, and may or may not be surface treated.

[0258] Suitable types of inorganic fillers can be selected from the group of minerals: silicates, phyllosilicates, silicon dioxide, carbonates, barites, metal oxides, metals, phosphates, halides, sulfides and sulfates. Organic fillers can include organic polymers or polymer blends, graphite, graphene, graphene oxide, fullerenes, carbon nanotubes, carbon fibers and organic polymer particles, such as core-shell particles containing organic compounds such as dyes, resins and / or organic liquids.

[0259] The limiting examples of the filler that can be used in the coating composition according to the present invention are nepheline syenite, talc, plastorite, chlorite, olivine, mica, pyrophyllite, feldspar, bentonite, kaolin, mica / muscovite, clay, wollastonite, quartz, cristobalite, glass flakes, glass fiber, fumed silica, calcium silicate, pumice, diatomaceous earth, calcium carbonate, magnesium carbonate, calcium sulfate, dolomite, barium sulfate, iron oxide, mica iron oxide, zinc oxide, aluminum oxide, aluminum hydroxide, aluminum flakes, zinc flakes and solid silicone resins, which are usually the branched polysiloxanes of condensation. Some fillers such as fumed silica and clay can have thickening effect to coating composition. Inorganic core-shell particles comprising organic compounds such as dyes, resins and / or organic liquids can also be used.

[0260] Examples of preferred fillers are talc, feldspar, barium sulfate, wollastonite, mica, dolomite, and calcite. Particularly preferred is a combination of talc and dolomite (or calcite), such as a mixture of talc and dolomite or talc and calcite, or dolomite, calcite and talc.

[0261] The color pigment may be an inorganic pigment, an organic pigment or a mixture thereof. The pigment may be surface treated.

[0262] Representative examples of pigments include black iron oxide, red iron oxide, yellow iron oxide, titanium dioxide, zinc oxide, carbon black, graphite, red molybdate, yellow molybdate, zinc sulfide, antimony oxide, sodium aluminum sulfosilicate, quinacridone, phthalocyanine blue, phthalocyanine green, indanthrene blue, aluminum cobalt oxide, carbazole dioxazine, isoindoline orange, bis-acetoaceto-tolidiole, benzimidazolone, quinophthalone yellow, isoindoline yellow, tetrachloroisoindolinone, and quinophthalone yellow, metal flake materials (e.g., aluminum flakes). In a preferred embodiment, titanium dioxide is surface-treated with a silicone compound, a zirconium compound, an aluminum compound, or a zinc compound.

[0263] Anticorrosive pigments and / or additives may be included in the coating composition to improve its anticorrosive properties. The types of anticorrosive pigments and additives are not specifically limited and any suitable anticorrosive pigments and additives may be used. Anticorrosive pigments may be based on borates, borosilicates, phosphates, orthophosphates, polyphosphates, phosphosilicates, silicates combined with metals or metal cations such as zinc, aluminum, molybdenum, calcium, strontium, aluminum magnesium, and barium. Anticorrosive pigments may be modified, such as surface modified, and / or may include complex ions and chelates.

[0264] Non-limiting examples of suitable anti-corrosion additives may be imidazoles (in purified form or contained in a polymer or resin matrix) polymers and other organic substances such as C12-14-(tert-)-alkylamines, (2-benzothiazolylthio)-succinic acid, 4-oxo-4-p-tolylbutyric acid, adducts with 4-ethylmorpholine, (2-benzothiazolylthio)succinic acid, poly(3-ammoniopropylethoxysiloxane) dodecanoate, ammonium benzoate, and morpholine.

[0265] Examples of suitable commercially available anticorrosion pigments and additives may be: Halox 520, Halox 570, Halox 630, Halox 350, Halox 430, Halox 700, Halox BW-11 from Halox. Habicor CS, Habicor from Habicor Si, Habicor ZS, Habicor ZA, Habicor ZN, Habicor ZO, Habicor ZM, Habicor AZ, HabicorSP, Habicor CP4295, Habicor Habicor ZP3850, Habicor ZP3860, Habicor1000 and Habicor 1001, and AX1 from Hexigone.

[0266] The coating composition may comprise 0 to 15 wt%, such as 0.1-10 wt% of an anti-corrosion pigment / additive.The coating composition may comprise a loading of 0-10 wt% zinc phosphate and / or calcium phosphate.

[0267] Pigments and fillers may be added to the paint composition in powder form or as a slurry or concentrate.

[0268] The amount of the at least one filler or pigment is preferably in the range of 0.05 to 50 wt%, preferably in the range of 1 to 45 wt%, more preferably 5 to 40 wt%, and still more preferably 10 to 40 wt%, based on the total weight of the coating composition.

[0269] additive

[0270] The coating composition of the present invention optionally comprises one or more additives. The example of the additive that can be present in the coating composition of the present invention includes, rheology modifier such as thixotropic agent, thickener and anti-settling agent, dispersant, wetting agent, defoamer and plasticizer. Suitable additive need not be limited to the additive that is developed and sold for use in paint. If compatible with coating composition, the additive that is developed and sold for use in for example adhesive, building material, plastic / resin, drilling fluid, paper coating and pigment concentrate can be used. Because the efficiency of any additive used in coating composition may be affected by other raw materials and the additive comprised therein to a great extent, it is important to determine the suitable type and concentration of additive by testing. In many cases, it may be necessary and / or useful to add a variety of different additives (i.e. two or more defoamers or two or more rheology modifiers) of any given type to achieve desired performance / efficiency.

[0271] Defoamers and air release additives, referred to herein simply as defoamers, are commonly used in epoxy coatings to help release incorporated air during the manufacture and application of the coating composition. The type of defoamer is not particularly limited, and any suitable type may be used. Commonly used defoamers can be divided into mineral oil defoamers, silicon defoamers, and polymer defoamers. Commercially available defoamers typically contain mixtures of these types, usually in combination with solvents and solid particles. Non-limiting examples of defoamers that can be used are Byk-011, Byk-012, Byk-014, Byk-015, Byk-016, Byk-017, Byk-018, Byk-019, Byk-021, Byk-022, Byk-023, Byk-024, Byk-025, Byk-028, Byk-035, Byk-037, Byk-038, Byk-039, Byk-044, Byk-046, Byk-047, Byk-048, Byk-050, Byk-051, Byk-052, Byk-053, Byk-054, Byk-055, Byk-056, Byk-057, Byk-058, Byk-059, Byk-060, Byk-061, Byk-062, Byk-063, Byk-064, Byk-065, Byk-066, Byk-067 k-051N, Byk-052N, Byk-053N, Byk-054, Byk-055, Byk-057, Byk-070, Byk-072, Byk-077, Byk-081, Byk-085 , Byk-088, Byk-092, Byk-093, Byk-094, Byk-141, Byk-1610, Byk-1611, Byk-1615, Byk-1616, Byk-1617, By k-1630, Byk-1640, Byk-1650, Byk-1707, Byk-1709, Byk-1710, Byk-1711, Byk-1719, Byk-1723, Byk-1724, Byk-1730, Byk-1740, Byk-1751, Byk-1752, Byk-1758, Byk-1759, Byk-1760, Byk-1770, Byk-1780, Byk-178 1. Byk-1785, Byk-1786, Byk-1788, Byk-1789, Byk-1790, Byk-1791, Byk-1794, Byk-1795, Byk-1796, Byk-1 797, Byk-1799, Byk-A515, Byk-A525, Byk-A530, Byk-A535, Byk-A550, Byk-A555 and Byk-A560, Tego from Evonik Airex901W, Tego Airex 901W N, Tego Airex 902W, TegoAirex 902W N, TegoAirex 904W, Tego Airex 904W N, Airase 4500, Airase 4655, Airase5355, Airase 5655,Airase 8070, Surfonyl 104, Surfonyl 107L, Surfonyl 420, TegoFoamex 3062, Tego Foamex 8050, Tego Foamex 843, Tego Foamex 844, Tego Foamex845, Tego Foamex 883, Tego Foamex 1488, Tego Foamex 810, Tego Foamex 811, Tego Foamex 812, Tego Foamex 815, Tego Foamex 822, Tego Foamex 823 and Tego Foamex 825. ,

[0272] Rheology modifiers can be used to adjust the rheological curve of the coating composition to prevent sedimentation and floating problems, as well as to adjust flow and improve anti-sagging, processability, application characteristics and the stability of pigment and extender particles. The type of rheology modifier is not particularly limited and any suitable rheology modifier can be used, but should be selected based on the characteristics that need to be improved and based on the compatibility with the rest of the formulation. Non-limiting examples of suitable rheology modifiers can be organically modified clays, such as bentonite, hectorite and attapulgite clays, unmodified clays, organic wax thixotropes based on castor oil and castor oil derivatives, amide waxes, rheology modifiers based on acrylic acid, urea, modified urea, polyurethane, amide or polyamide backbones, and fumed silica. The active ingredient of the rheology modifier can be modified with functional groups such as polyether and alcohol groups, or surface treated with, for example, silanes similar to fumed silica. Non-limiting examples of commercially available rheology modifiers can be TS-610, TS-530, EH-5, H-5, and M-5 from Cabot and TS-610, TS-530, EH-5, H-5, and M-5 from Evonik. R972, R974, R976, R104, 200, 300, R202, R208, R805, R812, 816, R7200, R8200, R9200, R711, Bentone SD2 from Elementis, Exilva from Borregard, Crayvallac ultra and Crayvallac LV from Arkema. Preferably, the rheology modifier comprises micronized amide wax and / or fumed silica and / or clay. Preferably, the rheology modifier is present in the composition of the present invention in an amount of 0 to 10 wt%, more preferably 0.1 to 6 wt% and even more preferably 0.1 to 3.0 wt%, based on the total weight of the composition.

[0273] Wetting and dispersing agents can be added to the coating composition to promote the dispersion and wetting of pigment and filler particles, so that it is easier to break agglomerates in the production process, prevent reflocculation and sedimentation in wet paint and form Benard cell (Benard cell) in cured paint, reduce the viscosity of paint, and increase its color strength and color stability. Wetting and dispersing agents can be nonionic, cationic, anionic or comprise above-mentioned mixture. In addition, wetting and dispersing agents can be composed of polymer or non-polymeric organic molecules or their mixtures. The limiting examples of the wetting and dispersing agents of suitable types can be fatty acid, lecithin, polysorbate, polyacrylamide, polyether carboxylate, polycarboxylate, polyalkylene glycol, polyether and polyacrylate. Non-limiting examples of commercially available wetting and dispersing agents can be Disperbyk-102, Disperbyk-106, Disperbyk-109, Disperbyk-142, Disperbyk-161, Disperbyk-180, Disperbyk-182, Disperbyk-2000, Disperbyk-2014, Disperbyk 2055, Disperbyk-2059, Disperbyk-2070, Disperbyk-2152 from BYK, Colorol F from Evonik, Adlec soy lecithin and Yelkin soy lecithin from ADM. Preferably, the wetting and dispersing agent comprises soy lecithin. Preferably, the wetting and dispersing agent is present in an amount of 0 to 1.5 wt%, more preferably 0.1 to 1 wt%.

[0274] From another aspect, the present invention provides a primer coating composition comprising:

[0275] (i) 5.0 to 40 wt % of an epoxy resin;

[0276] (ii) 2.0 to 15 wt % of silane;

[0277] (iii) a curing agent;

[0278] (iv) 1.0 to 15 wt % of a glycol ether solvent;

[0279] (v) 1.0 to 9.0 wt % of microspheres;

[0280] (vi) 0 to 10 wt% of a hydrocarbon resin; and

[0281] (vii) 0 to 20 wt% of a reactive diluent.

[0282] From another aspect, the present invention provides a primer coating composition comprising:

[0283] (i) 10 to 40 wt % of an epoxy resin;

[0284] (ii) 2.5 to 10 wt % of silane;

[0285] (iii) a curing agent;

[0286] (iv) 1.0 to 10 wt % of a glycol ether solvent;

[0287] (v) 1.0 to 9.0 wt % of microspheres;

[0288] (vi) 0 to 10 wt% of a hydrocarbon resin; and

[0289] (vii) 0 to 15 wt% reactive diluent.

[0290] From another aspect, the present invention provides a primer coating composition comprising:

[0291] (i) 10 to 40 wt % of an epoxy resin;

[0292] (ii) 2.5 to 8.0 wt % of silane;

[0293] (iii) a curing agent;

[0294] (iv) 2.0 to 8.0 wt % of a glycol ether solvent;

[0295] (v) 2.0 to 8.0 wt % of microspheres;

[0296] (vi) 0 to 10 wt% of a hydrocarbon resin; and

[0297] (vii) 0 to 15 wt% reactive diluent.

[0298] From another aspect, the present invention provides a primer coating composition comprising:

[0299] (i) 10 to 40 wt % of an epoxy resin;

[0300] (ii) 2.5 to 8.0 wt % of silane;

[0301] (iii) a curing agent;

[0302] (iv) 2.0 to 6.0 wt % of a glycol ether solvent;

[0303] (v) 2.0 to 7.0 wt % of microspheres;

[0304] (vi) 0 to 10 wt% of a hydrocarbon resin; and

[0305] (vii) 2.0 to 10 wt% reactive diluent.

[0306] Preparation of primer composition

[0307] Primer compositions can be prepared by any suitable technology commonly used in the field of paint production. Therefore, various ingredients can be mixed together using a high-speed disperser, a ball mill, a bead mill, a three-roll mill, an in-line mixer, etc. Preferably, microspheres are added in the letdown stage of the coating composition. Paints according to the present invention can be filtered using bag filters, patron filters, line gap filters, wedge-shaped line filters, metal edge filters, EGLM turnoclean filters (from Cuno), DELTA strain filters (from Cuno), and Jenag Strainer filters (from Jenag), or filtered by vibration filtration.

[0308] The primer composition to be used in this article is conveniently prepared by mixing the components. For example, the first composition (component A) and the curing agent composition (component B) can be mixed by adding the curing agent component B to the epoxy component A and stirring until the mixture is uniform. The mixture is immediately ready for application, such as by spraying, but an induction time can also be given before application. Those skilled in the art can easily determine the mixing ratio based on the target percentage in the final primer layer composition and the amount and equivalent of the epoxy functional compound in component A before mixing and the amount and equivalent of the compound (comprising primary amine and secondary amine) containing active H in component B.

[0309] Application of primer composition

[0310] The primer composition can be applied to the substrate (particularly steel structure) by well-known standard application methods such as conventional air spray or by airless or air mix spray equipment or 2K airless spray pump (or alternatively by brush or roller, especially when used as a stripe coating). Preferably, the composition is applied under ambient conditions without preheating the coating composition.

[0311] The substrate is a substrate that may be wet or moist, or a rusted substrate, or both, such as a flash rusted substrate.

[0312] Film thickness

[0313] The coating is typically applied at a total dry film thickness of 75 to 800 μm, preferably 100 to 500 μm, such as 150 to 350 μm. Preferably, the dry film thickness of the primer layer is at least 100 μm. The applied film thickness may vary depending on the nature of the coated substrate and its predicted exposure. The desired film thickness may require application of multiple coats of the composition, e.g. two coats.

[0314] Curing

[0315] Once the substrate is coated with the coating, the coating must be cured. The primer layer may be spontaneously cured. Although radiation and heat may be used to accelerate curing, the compositions of the present invention cure at ambient temperature without further intervention.

[0316] While a single coat is preferably applied, because the volatile content of the coating of the present invention is so low, additional coats can be applied while the primer layer is "wet". Thus, there is no need to wait for the first coat to cure before applying additional coats. To build up layer thickness, it is known to apply multiple primer coats, but conventionally, each layer is cured (dried) before applying additional layers. In the present invention, additional layers can be applied over the wet (or uncured) primer layer. This speeds up the application process.

[0317] Thus, in another aspect, the present invention includes a method in which an additional coating of a primer layer coating composition is applied to a basecoat of a primer layer composition without an intermediate curing step. Viewed in an alternative manner, the present invention includes a method in which an additional coating of a primer layer coating composition is applied to a basecoat of a primer layer composition before the basecoat is cured.

[0318] The invention will now be described with reference to the following non-limiting examples.

[0319] Analytical methods

[0320] General method for preparing the composition

[0321] Component A of the primer layer is prepared by mixing all specified ingredients (in parts by weight) in a customary manner known to the person skilled in the art. Component A is then mixed before application with component B. The primer layer is usually applied to the steel substrate by airless spraying.

[0322] Calculation of Density, Solid Volume Percentage, Volatile Organic Compounds and Pigment Volume Concentration The density, solid volume percentage (solid volume %) and theoretical volatile organic compound (VOC) content of the composition were calculated according to ASTM D5201-05a (2020).

[0323] The pigment volume concentration (PVC) of the composition was determined by calculation according to the following formula: PVC = ((Vp + Vf) / (Vp + Vf + Vb)) * 100. Where Vp is the volume of the pigment, Vf is the volume of the filler (including glass spheres), and Vb is the volume of the binder.

[0324] Determination of viscosity

[0325] The viscosity of the adhesive and paint compositions was determined according to ISO 2884-1:2006 (ASTM D4287) using a cone and plate viscometer set at a temperature of 23°C and 50% RH and provided at 10,000 s -1 The viscosity measurement range is 0 to 10P.

[0326] Stormer viscosity (KU) was measured according to ASTM D 562 using a Stormer viscometer at 23°C.

[0327] Cathodic disbonding test

[0328] Cathodic disbonding test was carried out according to ASTM G8. The test duration was 30 days. The composition was applied at a wet film thickness corresponding to 2 x 150 μm dry film thickness (DFT) to a surface having dimensions of 150 x 75 x 3 mm and a cleanliness level of Sa 2 1 The coatings were cured for 7 days under ambient conditions before the cathodic disbonding test.

[0329] Adhesion testing of coatings applied to wet substrates

[0330] Pull-off adhesion testing was performed according to ISO 4624:2016. The composition was applied to a wet, sandblasted carbon steel panel of dimensions 150x75x3mm at a wet film thickness corresponding to 2x150μm dry film thickness (DFT). The wet panel was prepared by soaking the sandblasted carbon steel panel in water, letting the water drip off and applying the coating immediately thereafter. Based on the mass difference between the dry and wet panels and the surface of the panel, the residual water on the wet panel was 40 to 45 g / m 2 Before immersion in water, the steel plate has Sa2 1 The coatings were cured for 7 days at ambient conditions prior to pull-off adhesion testing.

[0331] Example

[0332] The following materials were used:

[0333] Table 1

[0334]

[0335]

[0336] Table 2: Examples of the present invention (wt%)

[0337]

[0338]

[0339] Table 3: Comparative Examples

[0340]

[0341]

[0342] Table 4: Primer composition properties

[0343]

[0344] In Table 4 above, the theoretical physical parameters of the coating compositions can be compared as well as the measured viscosities. The results show that CE1 without glass spheres has a higher VOC and density than E1-E4. CE3-CE5 have a viscosity greater than 2000 mPas 1 h after mixing of components A and B, meaning that these compositions have a shorter pot life than the other compositions. These compositions lack glycol ethers (CE3), silanes (CE4) or contain low levels of silanes (CE5). Therefore, the pot lives of CE3-CE5 demonstrate that low levels of silanes or the use of n-butanol instead of glycol ethers give higher viscosities more quickly.

[0345] The test results of the cathodic disbonding test and the adhesion test are shown in Table 5. The results of the cathodic disbonding test were rated on a scale of 1-3 based on the following criteria:

[0346] 1: No bubbles, peeling up to 3mm - good

[0347] 2: No bubbles, peeling 3 to 8 mm - acceptable

[0348] 3: Bubbles and / or peeling higher than 8mm - Failure

[0349] The results of the pull-off adhesion test on wet and damp substrates were rated on a scale of 1-3 based on the following criteria:

[0350] 1: Cohesive failure in the first or second coating

[0351] 2: Partial (0%-50%) adhesion failure between substrate and first coating, the rest is cohesive failure

[0352] 3: Greater than 50% adhesion failure between substrate and first coating

[0353] Options 2 and 3 were considered "failed" in the adhesion test.

[0354] Table 5 - Cathodic Disbonding Test and Adhesion Test on Wet Substrate

[0355]

[0356] Good adhesion between the substrate and the primer coating is important for the performance of the anticorrosion primer. Therefore, if the composition fails the adhesion test, it is considered unsuitable for use as a high performance anticorrosion primer.

[0357] Adhesion test results indicate that silane and glycol ether solvents are essential for adhesion to wet substrates. Example 3 shows that a xylene-free formulation can be used.

[0358] When the amount of glass spheres was too high (CE2), the formulation failed in the cathodic disbonding test. Since CE2 failed the G8 test, it was not tested further on a wet substrate. Similarly, since CE3 failed the wet substrate test, it was not an interesting composition for this type of primer coating and did not undergo cathodic disbonding.

[0359] The primer compositions of the present invention (Examples 1-4) can be applied on wet or damp surfaces. The compositions can also be applied on rusted and flash rusted substrates.

Claims

1. A primer coating composition comprising: (i) Epoxy resin; (ii) 2.0 to 15 wt % of silane; (iii) a curing agent, such as an amine-based curing agent; (iv) glycol ether solvents; and (v) 1.0 to 9.0 wt% of microspheres.

2. The primer coating composition according to claim 1, wherein the microspheres have a D90 diameter of 30 to 150 μm, more preferably 50 to 90 μm and even more preferably 50 to 80 μm as measured by ISO 13320:2009 using a Malvern Mastersizer 2000.

3. The primer coating composition according to any one of the preceding claims, further comprising a reactive diluent.

4. A primer coating composition according to any one of the preceding claims, wherein The epoxy resin is a liquid.

5. A primer coating composition according to any one of the preceding claims, wherein The epoxy resin is based on bisphenol, preferably based on bisphenol A.

6. A primer coating composition according to any one of the preceding claims, wherein The glycol ether solvent has formula (I): R-[O-R’] x -OH (I) Wherein, x is 1 to 3; R is C1-C 16 Aliphatic groups; and R' is C1-C 16 Aliphatic group.

7. A primer coating composition according to any one of the preceding claims, wherein The glycol ether solvent has formula (II): RO-R'-OH (II) wherein R is a C1-C8 linear or branched alkyl group; and R' is ethylene or propylene, preferably propylene glycol n-butyl ether.

8. A primer coating composition according to any one of the preceding claims, wherein The microspheres include glass spheres.

9. A primer coating composition according to any one of the preceding claims, wherein The silane is epoxy silane.

10. A primer coating composition according to any one of the preceding claims, wherein The curing agent includes N-benzylated polyalkyleneamines or phenalkamines, especially phenalkamines based on 1,3-bis(aminomethyl)benzene and ethylenediamine.

11. A primer coating composition according to any one of the preceding claims, wherein: The viscosity of the composition immediately upon formation at 23°C is 200-1000 mPas.

12. A primer coating composition according to any one of the preceding claims, wherein: The glycol ether solvent is present in an amount of 1.0 to 10 wt % of the composition.

13. A primer coating composition according to any one of the preceding claims, wherein: The pot life at 23°C is at least 30 minutes.

14. A primer coating composition according to any one of the preceding claims, having a VOC of 220 g / L or less.

15. A primer coating composition according to any one of the preceding claims, comprising: (i) 10 to 40 wt % of an epoxy resin; (ii) 2.5 wt % to 10 wt % of silane; (iii) a curing agent; (iv) 2.0 to 10 wt % of a glycol ether solvent; (v) 2.0 to 9.0 wt % of microspheres; (vi) 0 to 10 wt % (e.g., 2.0 to 10 wt %) of a hydrocarbon resin; and (vii) 0 to 15 wt % (eg, 2.0 to 15 wt %) of a reactive diluent.

16. A kit suitable for preparing a primer coating composition according to claims 1 to 15, comprising component (A) and component (B), wherein component (A) comprises: (i) Epoxy resin; (ii) silane; (iv) glycol ether solvents; and (v) microspheres; And the component (B) comprises at least one curing agent.

17. A metal substrate having applied thereon the primer coating composition according to any one of claims 1 to 15.

18. Use of a primer coating composition according to any one of claims 1 to 15 for application to wet and / or rusted substrates.

19. A method for applying paint to a wet metal substrate, comprising: 1) Blending component A and component B; wherein component (A) comprises an epoxy resin; and Component (B) comprises a curing agent; and wherein at least one of component (A) or component (B) comprises a silane, a glycol ether solvent, and microspheres, such that when component (A) and component (B) are mixed, the resulting composition comprises 2.0 to 15 wt % of the silane and 1.0 to 9.0 wt % of the microspheres; 2) applying the composition to a wet substrate, and 3) Allow the composition to form a film and cure.

Citation Information

Patent Citations

  • Heavy-duty anti-corrosion epoxy primer for low-grade substrate processing and preparation method of heavy duty anti corrosion epoxy primer

    CN104946075A

  • coatings

    CN109689724A

  • Two-component curable composition for metal surface treatment, method for mounting membrane on metal surface and surface structure

    CN113773726A

  • Organotin antifouling coatings with novolac and Bisphenol-A epoxy resins