Adhesive composition, adhesive film for circuit connection, circuit connection structure, and method for producing same

By using thermoplastic resin, radical polymerizable compounds and conductive particles in circuit connection, combining cyclized polymerizable monomers and (poly)urethane acrylate compounds, electrode connection resistance under high temperature and high humidity conditions is solved. The problem of enlargement significantly improves the reliability of circuit connections.

CN118974194APending Publication Date: 2024-11-15RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031280.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-03-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing circuit connection, the structure using a radical curing adhesive is prone to increase the connection resistance between the electrodes under high temperature and high humidity conditions.

Method used

Using a binder composition containing a thermoplastic resin, a radical polymerizable compound, a radical polymerization initiator and conductive particles, the cyclized polymerizable monomer and (poly)carbamate (meth)acrylic acid in the circuit connection Ester compounds form polymers with high crosslinking density to improve heat and moisture resistance of the connection.

Benefits of technology

The connection resistance between the opposite electrodes is difficult to increase under high temperature and high humidity conditions, and the reliability of circuit connection is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974194A_ABST
    Figure CN118974194A_ABST
Patent Text Reader

Abstract

The adhesive film for circuit connection contains conductive particles and a resin component containing a thermoplastic resin, a radical polymerizable compound, and a radical polymerization initiator, and contains a cyclic polymerizable monomer as the radical polymerizable compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive composition, an adhesive film for circuit connection, a circuit connection structure and a manufacturing method thereof. Background Art

[0002] As a circuit connection material for semiconductor elements or liquid crystal display elements, it is known that a thermosetting resin using an epoxy resin showing high adhesiveness and high reliability is used (for example, reference patent document 1). As a component constituting the resin, epoxy resin, a curing agent such as a phenolic resin reactive with the epoxy resin, and a latent curing agent that promotes the reaction of the epoxy resin and the curing agent are generally used. The latent curing agent becomes an important factor in determining the curing temperature and the curing rate, and various compounds are used from the viewpoint of storage stability at room temperature and the curing rate when heated.

[0003] In recent years, attention has been paid to free radical curing adhesives that use acrylate derivatives and / or methacrylate derivatives (hereinafter collectively referred to as "(meth)acrylate derivatives") together with peroxides as free radical polymerization initiators. Since free radicals as reactive species are highly reactive, free radical curing can cure in a short time (for example, refer to Patent Documents 2 and 3).

[0004] Therefore, short-time curing adhesives are becoming more and more popular, which are advantageous for shortening production time. In addition, the use of chain transfer agents is being studied for the purpose of further improving the reactivity of radical curing adhesives (for example, see Patent Documents 4 and 5).

[0005] Previous technical literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 1-113480

[0008] Patent Document 2: Japanese Patent Application Publication No. 2002-203427

[0009] Patent Document 3: International Publication No. 98 / 044067 Pamphlet

[0010] Patent Document 4: Japanese Patent Application Publication No. 2003-221557

[0011] Patent Document 5: International Publication No. 2009 / 057376 Pamphlet Summary of the invention

[0012] Technical issues to be solved by the invention

[0013] An adhesive film having anisotropic conductivity and in which conductive particles are dispersed is used to connect circuit components. However, a circuit connection structure obtained by using a radical curing adhesive as an adhesive tends to have an increased connection resistance between electrodes facing each other after a high temperature and high humidity test.

[0014] Therefore, the object of the present invention is to provide an adhesive composition and an adhesive film for circuit connection that can obtain a circuit connection structure in which the connection resistance between electrodes facing each other is unlikely to increase even under high temperature and high humidity conditions, as well as a circuit connection structure and a method for manufacturing the same that can obtain a circuit connection structure in which the connection resistance between electrodes facing each other is unlikely to increase even under high temperature and high humidity conditions.

[0015] Means for solving technical problems

[0016] The contents of the present invention are as follows [1] to [8].

[0017] [1] An adhesive composition comprising a resin component containing a thermoplastic resin, a radical polymerizable compound and a radical polymerization initiator, and conductive particles, wherein the radical polymerizable compound contains a cyclopolymerizable monomer.

[0018] The adhesive composition described above can provide a circuit connection structure having a property that connection resistance between electrodes facing each other is unlikely to increase even under high temperature and high humidity conditions (hereinafter also referred to as “high temperature and high humidity connection reliability”).

[0019] [2] The adhesive composition according to [1] above, wherein:

[0020] The content of the cyclopolymerizable monomer is 3 to 50% by mass based on the total amount of the radical polymerizable compound.

[0021] [3] The adhesive composition according to [1] or [2] above, wherein

[0022] The (poly)urethane (meth)acrylate compound is further contained as a radical polymerizable compound, and the content of the (poly)urethane (meth)acrylate compound is 100 to 1000 parts by mass based on 100 parts by mass of the cyclopolymerizable monomer.

[0023] [4] An adhesive film for circuit connection, comprising a thermoplastic resin, a radical polymerizable compound, a radical polymerization initiator, and conductive particles, wherein the radical polymerizable compound contains a cyclopolymerizable monomer.

[0024] According to the above-mentioned adhesive film, a circuit connection structure having sufficient high-temperature and high-humidity connection reliability can be obtained.

[0025] [5] The adhesive film for circuit connection according to [4] above, wherein:

[0026] The content of the cyclopolymerizable monomer is 3 to 50% by mass based on the total amount of the radical polymerizable compound.

[0027] [6] The adhesive film for circuit connection according to [4] or [5] above, wherein:

[0028] The (poly)urethane (meth)acrylate compound is further contained as a radical polymerizable compound, and the content of the (poly)urethane (meth)acrylate compound is 100 to 1000 parts by mass based on 100 parts by mass of the cyclopolymerizable monomer.

[0029] [7] A circuit connection structure comprising:

[0030] A first circuit component having a first electrode;

[0031] a second circuit component having a second electrode; and

[0032] The connecting portion is disposed between the first circuit component and the second circuit component and electrically connects the first electrode and the second electrode to each other.

[0033] The connecting portion includes a cured product of the adhesive composition according to any one of [1] to [3] above.

[0034] The above-mentioned circuit connection structure can have sufficient high-temperature and high-humidity connection reliability.

[0035] [8] A method for manufacturing a circuit connection structure, comprising the following steps:

[0036] The first circuit component having a first electrode, the second circuit component having a second electrode, and the circuit connecting adhesive film described in any one of [4] to [6] are heated and pressurized in a state where the first electrode and the second electrode are arranged opposite to each other with the circuit connecting adhesive film interposed therebetween, thereby electrically connecting the first electrode and the second electrode.

[0037] According to the above method, a circuit connection structure having sufficient high-temperature and high-humidity connection reliability can be obtained.

[0038] Effects of the Invention

[0039] According to the present invention, there can be provided an adhesive composition and an adhesive film for circuit connection that can obtain a circuit connection structure in which the connection resistance between electrodes facing each other is unlikely to increase even under high temperature and high humidity conditions, as well as a circuit connection structure in which the connection resistance between electrodes facing each other is unlikely to increase even under high temperature and high humidity conditions and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic cross-sectional view showing one embodiment of a connection structure. DETAILED DESCRIPTION

[0041] In this specification, the numerical range represented by "~" indicates a range including the numerical values ​​recorded before and after "~" as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be replaced by the upper limit or lower limit of the numerical range of other stages. And, in the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. And, the upper limit and lower limit recorded separately can be combined arbitrarily. And, in this specification, "(meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. The same is true in other similar expressions such as "(meth)acryloyl". And, "(poly)" refers to both the case with the prefix of "poly" and the case without the prefix of "poly". And, "A or B" can include either A and B, or both. And, with respect to the materials exemplified below, unless otherwise specified, one can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the plurality of substances present in the composition unless otherwise specified.

[0042] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings as appropriate. However, the present invention is not limited to the following embodiments.

[0043] <Adhesive composition>

[0044] The adhesive composition of the present embodiment may include a resin component containing (A) a thermoplastic resin (hereinafter, also referred to as "component (A)"), (B) a radical polymerizable compound (hereinafter, also referred to as "component (B)"), and (C) a radical polymerization initiator (hereinafter, also referred to as "component (C)"), and (G) conductive particles (hereinafter, also referred to as "component (G)").

[0045] [(A) component: thermoplastic resin]

[0046] As component A, polyvinyl butyral resin, polyvinyl formal resin, polyamide resin, polyester resin, phenol resin, epoxy resin, phenoxy resin, polystyrene resin, xylene resin, polyurethane resin, polyester urethane resin, etc. can be used. These can be used alone or in combination of two or more.

[0047] From the viewpoint of film forming properties, the weight average molecular weight of the thermoplastic resin may be 1.0×10 4 From the perspective of miscibility, it can be 1.0×10 4 More than and less than 1.0×10 6 .

[0048] The weight average molecular weight of the thermoplastic resin refers to a value measured by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene under the following conditions.

[0049] [GPC conditions]

[0050] Equipment used: Hitachi L-6000 model [Hitachi, Ltd.], chromatographic columns: Gelpackg GL-R420 + Gelpackg GL-R430 + Gelpackg GL-R440 (3 in total) [manufactured by Hitachi Chemical Company, Ltd.], eluent: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1.75 ml / min, detector: L-3300RI [Hitachi, Ltd.]

[0051] As the component (A), a material having a Tg (glass transition temperature) of 40° C. or higher and a weight average molecular weight of 1.0×10 4 The above hydroxyl group-containing resin (eg, phenoxy resin) may be modified with an epoxy group-containing elastomer.

[0052] In the present specification, a thermoplastic resin having a radical polymerizable functional group is blended as (B) a radical polymerizable compound.

[0053] The phenoxy resin can be obtained by reacting a difunctional phenol with an epihalohydrin to a high molecular weight or by subjecting a difunctional epoxy resin to an addition polymerization reaction with a difunctional phenol.

[0054] Furthermore, as the component (A), a polyester urethane resin can be used.

[0055] From the viewpoint of further improving the effect of suppressing peeling, the content of component (A) in the adhesive composition may be 5% by mass or more, or 30% by mass or more, or 80% by mass or less, or 60% by mass or less, or 5 to 80% by mass, or 30 to 60% by mass, based on the resin component of the adhesive composition (e.g., components other than the conductive particles and the filler).

[0056] [Component (B): Radically polymerizable compound]

[0057] As component (B), a compound having a free radical polymerizable functional group can be used. As the free radical polymerizable functional group, vinyl, acryloyl, methacryloyl, etc. can be mentioned. Among them, compounds having acryloyl and / or methacryloyl are more preferred. Component (B) can be used alone or in combination of two or more.

[0058] The adhesive composition of the present embodiment may contain a cyclopolymerizable monomer (hereinafter, also referred to as "component (B1)") as component (B).

[0059] As the component (B1), a monomer containing a diene structure can be used. Examples of the monomer containing a diene structure include a monomer containing a 1,5-diene structure which may contain a heteroatom and a monomer containing a 1,6-diene structure which may contain a heteroatom. The component (B1) can be used alone or in combination of two or more.

[0060] As the component (B1), a monomer containing an acrylic diene structure represented by the following general formula (1) can be used.

[0061]

[0062] [In formula (1), R 1 represents a hydrogen atom or an organic group having 1 to 30 carbon atoms, R 2 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a phenyl group, a carboxyl group, an ester group or a cyano group, X and Y each independently represent a methylene group which may have an alkyl group having 1 to 4 carbon atoms, an imino group, a carbonyl group, an oxygen atom or a sulfur atom, Z represents a direct bond, a methylene group which may have an alkyl group having 1 to 4 carbon atoms, an imino group, a carbonyl group, an oxygen atom or a sulfur atom, and at least one of X, Y and Z is an oxygen atom, a sulfur atom or an imino group (wherein, in XYZ, hetero atoms are not adjacent).]

[0063] In R 1 In the case of an organic group having 1 to 30 carbon atoms, examples of the organic group include chain saturated hydrocarbon groups having 1 to 30 carbon atoms, chain unsaturated hydrocarbon groups having 2 to 30 carbon atoms, alicyclic hydrocarbon groups having 3 to 30 carbon atoms, aromatic hydrocarbon groups having 6 to 30 carbon atoms, and cyclic ether groups having 2 to 30 carbon atoms. In these organic groups, a part or all of the hydrogen atoms may be substituted with at least one substituent selected from the group consisting of an alkoxy group having 1 to 30 carbon atoms, a hydroxyl group, and a halogen atom. Examples of the halogen atom include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. R 1 It may be methyl, ethyl, isopropyl, phenoxyethyl, cyclohexyl, isobornyl, benzyl or tetrahydrofurfuryl, or it may be methyl or cyclohexyl.

[0064] In R2 In the case of an ester group, examples of the ester group include -COOR 3 (Where R 3 represents an organic group having 1 to 30 carbon atoms). 3 can be the same as the above R 1 Same group.

[0065] The adhesive composition of the present embodiment includes a monomer containing the above-mentioned acrylic diene structure as the (B) component, and it is easy to obtain a circuit connection structure having the characteristic that the connection resistance between the electrodes facing each other is difficult to increase even under high temperature and high humidity conditions. The present inventors speculate as follows about the reason why this effect can be obtained. It is believed that in the free radical polymerization reaction body containing the monomer containing the above-mentioned acrylic diene structure, a non-cyclization reaction and a cyclization reaction are carried out by heating when the circuit components are connected to each other. It is speculated that through these reactions, a polymer with a high crosslinking density, a polymer containing a ring structure in the main chain of the polymer, and a polymer containing a crosslinking structure and a ring structure are formed, thereby achieving the suppression of interface peeling caused by the reduction of shrinkage stress during connection and the imparting of heat resistance and moisture resistance to the cured product constituting the connection portion, and as a result, the above-mentioned effect is obtained.

[0066] The component (B1) may be a 1,6-diene structure-containing monomer represented by the following general formulae (1a) to (1c). In this case, the shrinkage stress generated during connection can be reduced and interfacial peeling can be further suppressed, thereby further improving the high temperature and high humidity resistant connection reliability.

[0067]

[0068] [In formula (1a), R 1 The meaning is the same as above.]

[0069]

[0070] [In formula (1b), R 1 The meaning is the same as above.]

[0071]

[0072] [In formula (1c), R 1 Same meaning as above, 2 R 1 Can be the same or different.]

[0073] When the adhesive composition of this embodiment contains the monomer containing the above-mentioned 1,6-diene structure, it is easier to obtain a circuit connection structure with excellent high-temperature and high-humidity connection reliability. This effect is believed to be due to the formation of a THF ring structure in the polymer, which can further relax the shrinkage stress during connection.

[0074] Examples of the monomer containing a 1,6-diene structure represented by the general formula (1a) include α-allyloxymethacrylic acid, methyl α-allyloxymethacrylate, ethyl α-allyloxymethacrylate, propyl α-allyloxymethacrylate, isopropyl α-allyloxymethacrylate, butyl α-allyloxymethacrylate, tert-butyl α-allyloxymethacrylate, phenoxyethyl α-allyloxymethacrylate, cyclohexyl α-allyloxymethacrylate, dicyclopentadienyl α-allyloxymethacrylate, isobornyl α-allyloxymethacrylate, adamantyl α-allyloxymethacrylate, benzyl α-allyloxymethacrylate, and allyloxymethacrylates such as tetrahydrofurfuryl α-allyloxymethacrylate.

[0075] Examples of the monomer containing a 1,6-diene structure represented by the general formula (1b) include α-methoxymethylacrylic acid, methyl α-methoxymethylacrylate, ethyl α-methoxymethylacrylate, propyl α-methoxymethylacrylate, isopropyl α-methoxymethylacrylate, butyl α-methoxymethylacrylate, tert-butyl α-methoxymethylacrylate, phenoxyethyl α-methoxymethylacrylate, cyclohexyl α-methoxymethylacrylate, dicyclopentadienyl α-methoxymethylacrylate, isobornyl α-methoxymethylacrylate, adamantyl α-methoxymethylacrylate, benzyl α-methoxymethylacrylate, tetrahydrofurfuryl α-methoxymethylacrylate and the like.

[0076] Examples of the 1,6-diene structure-containing monomer represented by the general formula (1c) include ether forms of α-hydroxymethylacrylate monomers such as bis(α-hydroxymethylacrylate) ether, bis(methyl α-hydroxymethylacrylate) ether, bis(ethyl α-hydroxymethylacrylate) ether, bis(propyl α-hydroxymethylacrylate) ether, bis(isopropyl α-hydroxymethylacrylate) ether, bis(butyl α-hydroxymethylacrylate) ether, bis(tert-butyl α-hydroxymethylacrylate) ether, bis(phenoxyethyl α-hydroxymethylacrylate) ether, bis(cyclohexyl α-hydroxymethylacrylate) ether, bis(dicyclopentadienyl α-hydroxymethylacrylate) ether, bis(isobornyl α-hydroxymethylacrylate) ether, bis(adamantyl α-hydroxymethylacrylate) ether, bis(benzyl α-hydroxymethylacrylate) ether, and bis(tetrahydrofurfuryl α-hydroxymethylacrylate) ether.

[0077] For example, the above monomer can be prepared by the method described in Japanese Patent Application Laid-Open No. 10-226669 and Japanese Patent Application Laid-Open No. 2012-184402. In addition, commercially available products such as "FX-AO-MA" (manufactured by Nippon Shokubai Co., Ltd., product name) can be used.

[0078] As the 1,5-diene structure-containing monomer which may contain a hetero atom, for example, monomers containing a 1,5-diene structure represented by the following general formulae (1d) to (1e) can be used.

[0079]

[0080] [In formula (1d), R 1 The meaning is the same as above.]

[0081]

[0082] [In formula (1e), R 1 The meaning is the same as above.]

[0083] From the viewpoint of reducing the shrinkage stress generated during connection and further suppressing interface peeling, the content of the component (B1) in the adhesive composition may be 3% by mass or more, or 7% by mass or more, or 50% by mass or less, or 45% by mass or less, or 3 to 50% by mass, 7 to 45% by mass, 10 to 40% by mass, or 13 to 37% by mass, based on the total mass of the component (B).

[0084] Furthermore, from the viewpoint of reducing the shrinkage stress generated during connection and further suppressing interface delamination, the content of the component (B1) in the adhesive composition may be 1% by mass or more, or 4% by mass or more, or 35% by mass or less, or 30% by mass or less, or 1% to 35% by mass, 4% to 30% by mass, 7% to 25% by mass, or 10% to 20% by mass, based on the total mass of the resin components of the adhesive composition (for example, components other than the conductive particles and the filler).

[0085] The adhesive composition of the present embodiment may contain the component (B1) and a radically polymerizable compound other than the above-mentioned (B1) (hereinafter, also referred to as "component (B2)").

[0086] As the component (B2), polymers such as polyurethane, polystyrene, polyethylene, polyvinyl butyral, polyvinyl formal, polyimide, polyamide, polyester, polyvinyl chloride, polyphenyl oxide, urea resin, melamine resin, phenol resin, xylene resin, epoxy resin, polyisocyanate resin, phenoxy resin, etc. can also be used. In addition, the polymer used as the component (B2) has at least one free radical polymerizable functional group in the molecule.

[0087] When a polymer is contained as the component (B2), it is preferred because it is easy to handle and has excellent stress relaxation during curing. When the polymer has a functional group such as a hydroxyl group, the adhesiveness is improved, which is more preferred.

[0088] The weight average molecular weight of the above polymer can be 1.0×10 4 From the perspective of mixing, it can also be 1.0×10 4 Above and 1.0×10 6 The weight average molecular weight here was measured by gel permeation chromatography (GPC) under the conditions described in the Examples using a calibration curve based on standard polystyrene.

[0089] As the component (B2), a (poly)urethane (meth)acrylate compound can be used from the viewpoint of achieving a balance between crosslinking density and cure shrinkage when used together with the component (B1) and further reducing connection resistance to improve high-temperature and high-humidity connection reliability.

[0090] From the viewpoint of the balance between crosslink density and cure shrinkage, the content of the (poly)urethane (meth)acrylate compound may be 40 to 95 mass %, 50 to 90 mass %, or 55 to 85 mass % based on the total mass of the component (B).

[0091] Furthermore, from the viewpoint of achieving a balance between crosslinking density and cure shrinkage and further reducing connection resistance, the content of the (poly)urethane (meth)acrylate compound may be 100 to 1000 parts by mass, 130 to 800 parts by mass, or 150 to 650 parts by mass based on 100 parts by mass of the component (B1).

[0092] As the component (B2), ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, 2-hydroxy-1,3-di(meth)acryloxypropane, 2,2-bis[4-((meth)acryloxymethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloxypolyethoxy)phenyl]propane, dicyclopentenyl(meth)acrylate, tricyclodecyl(meth)acrylate, tri((meth)acryloxyethyl)isocyanurate, urethane(meth)acrylate, dimethyloltricyclodecyl di(meth)acrylate, isocyanuric acid EO (ethylene oxide)-modified diacrylate, 2-methacryloxyethyl phosphate, and the like can be used.

[0093] Furthermore, as the component (B2), a compound having at least one partial structure selected from the group consisting of a dicyclopentane skeleton, a tricyclodecane skeleton, and a triazine ring can be used.

[0094] The component (B2) may include a (meth)acrylate compound (a (meth)acrylate compound having a phosphate structure) represented by the following formula (2). In this case, since the bonding strength with the surface of an inorganic substance (metal, etc.) is improved, it is suitable for bonding electrodes (for example, circuit electrodes).

[0095]

[0096] In formula (2), n represents an integer of 1 to 3, and R represents a hydrogen atom or a methyl group.

[0097] For example, a (meth)acrylate compound represented by formula (2) is obtained by reacting phosphoric anhydride with 2-hydroxyethyl (meth)acrylate. Specific examples of the (meth)acrylate compound represented by formula (1) include mono(2-(meth)acryloyloxyethyl)phosphate, di(2-(meth)acryloyloxyethyl)phosphate, and the like.

[0098] From the perspective of easily obtaining the cross-linking density required for reducing connection resistance and improving connection reliability, for example, the content of the (meth)acrylate compound represented by formula (2) can be 1 to 10 mass %, 2 to 5 mass % or 2.5 to 4 mass %, based on the total mass of component (B).

[0099] From the perspective of easily obtaining the cross-linking density required for reducing connection resistance and improving high-temperature and high-humidity resistant connection reliability, the content of component (B) in the adhesive film for circuit connection may be 5% by mass or more, 20% by mass or more, or 40% by mass or more, or may be 90% by mass or less, 75% by mass or less, or 60% by mass or less, or may be 5 to 90% by mass, 20 to 75% by mass, or 40 to 60% by mass, based on the total mass of the resin components of the adhesive composition (for example, components other than conductive particles and fillers).

[0100] [Component (C): Radical Polymerization Initiator]

[0101] As the (C) component, a compound that generates free radicals can be used, for example, a compound that generates free radicals by thermal decomposition such as a peroxide compound and an azo compound. The free radical polymerization initiator is appropriately selected according to the target connection temperature, connection time, etc. The (C) component can be used alone or in combination of two or more.

[0102] Examples of the radical polymerization initiator include diacyl peroxides, peroxydicarbonates, peroxyesters, peroxyketals, dialkyl peroxides, and hydroperoxides.

[0103] Examples of the diacyl peroxides include 2,4-dichlorobenzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, distearic acid peroxide, succinyl peroxide, benzoyl peroxytoluene, and benzoyl peroxide.

[0104] Examples of the peroxydicarbonates include di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, bis(4-tert-butylcyclohexyl)peroxydicarbonate, di-2-ethoxymethoxyperoxydicarbonate, di(2-ethylhexylperoxy)dicarbonate, dimethoxybutyl peroxydicarbonate, and di(3-methyl-3-methoxybutylperoxy)dicarbonate.

[0105] Examples of the peroxyesters include 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, tert-hexyl peroxyneodecanoate, tert-butyl peroxypivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexylperoxy)hexane, 1-cyclohexyl-1-methylethyl peroxy-2-ethylhexanoate, tert-hexyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, Butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, 1,1-bis(tert-butylperoxy)cyclohexane, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxy-3,5,5-trimethylethylhexanoic acid, tert-butyl peroxylaurate, 2,5-dimethyl-2,5-di(m-tolueneperoxy)hexane, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-hexyl peroxybenzoate, tert-butyl peroxyacetate, etc.

[0106] Examples of the peroxyketals include 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-hexylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-(tert-butylperoxy)cyclododecane, and 2,2-bis(tert-butylperoxy)decane.

[0107] Examples of the dialkyl peroxides include α,α′-bis(tert-butylperoxy)diisopropylbenzene, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and tert-butylperoxyisopropylbenzene.

[0108] Examples of the hydroperoxides include diisopropylbenzene hydroperoxide and cumene hydroperoxide.

[0109] These radical polymerization initiators may be used in combination with a decomposition accelerator, an inhibitor, etc. Furthermore, it is preferable to encapsulate these radical polymerization initiators with polyurethane-based or polyester-based polymers, etc., because the storage life can be prolonged.

[0110] From the viewpoint of the pot life of the adhesive composition, the content of the component (C) in the adhesive composition may be 0.1% by mass or more, 0.5% by mass or more, or 1% by mass or more, or 20% by mass or less, 10% by mass or less, or 5% by mass or less, or 0.1-20% by mass, 0.5-10% by mass, or 1-5% by mass, based on the total mass of the resin components of the adhesive composition (for example, components other than the conductive particles and the filler).

[0111] [Component (G): conductive particles]

[0112] As the (G) component, metal particles such as Au, Ag, Ni, Cu, solder, conductive carbon particles composed of conductive carbon, etc. can be used. In addition, the (G) component can be a component in which the surface of transition metals such as Ni is coated with precious metals such as Au. From the viewpoint of obtaining a sufficient shelf life, the surface layer can be set to Au, Ag, platinum group precious metals, or Au. In addition, the (G) component can be a conductive layer formed on the surface of non-conductive particles by coating the surface of non-conductive particles such as glass, ceramics, plastics, etc. with the above-mentioned conductive material, and the outermost layer is composed of precious metals. In the case of using such particles or hot-melt metal particles, they have deformability by heating and pressurizing, so that the contact area with the electrode can be increased during connection to improve reliability.

[0113] The (G) component may be the above-mentioned metal particles, conductive carbon particles, coated conductive particles, and insulating coated conductive particles, wherein the insulating coated conductive particles have an insulating layer containing an insulating material such as a resin and coating the surface of the particles. If the (G) component is an insulating coated conductive particle, even if the content of the (G) component is high, since the surface of the particle is coated with the resin, it is possible to suppress the occurrence of a short circuit caused by contact between the (G) components, and it is also possible to improve the insulation between adjacent electrode circuits.

[0114] (G) As the component, the above-mentioned various conductive particles can be used alone or in combination of two or more.

[0115] The maximum particle size of the (G) component needs to be smaller than the minimum spacing between the electrodes (the shortest distance between adjacent electrodes). From the perspective of excellent dispersibility and conductivity, the maximum particle size of the (G) component can be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the perspective of excellent dispersibility and conductivity, the maximum particle size of the (G) component can be 50 μm or less, 30 μm or less, or 20 μm or less. From these perspectives, the maximum particle size of the (G) component can be 1.0 to 50 μm, 2.0 to 30 μm, or 2.5 to 20 μm. In this specification, for any 300 (pcs) conductive particles, the particle size is measured by observation using a scanning electron microscope (SEM), and the maximum value obtained is used as the maximum particle size of the (G) component. In addition, in the case where the (G) component is not spherical with protrusions, the particle size of the (G) component is taken as the diameter of the circle circumscribed with the conductive particles in the SEM image.

[0116] From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (G) component can be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (G) component can be 50 μm or less, 30 μm or less, or 20 μm or less. From these viewpoints, the average particle size of the (G) component can be 1.0 to 50 μm, 2.0 to 30 μm, or 2.5 to 20 μm. In this specification, for any 300 (pcs) conductive particles, the particle size is measured by observation using a scanning electron microscope (SEM), and the average value of the obtained particle size is taken as the average particle size.

[0117] From the perspective of easily obtaining a stable connection resistance, the content of the component (G) in the adhesive composition may be in the range of 0.1 to 30 parts by volume relative to 100 parts by volume of the resin component (e.g., components other than the conductive particles and the filler) of the adhesive composition. From the perspective of preventing short circuits of adjacent circuits caused by excessive conductive particles, the content of the component (G) may also be 0.1 to 10 parts by volume.

[0118] Furthermore, from the perspective of easily obtaining stable connection resistance, the content of component (G) may be 0.5 to 60 mass %, 3 to 45 mass % or 6 to 30 mass % based on the total mass of the resin components of the adhesive composition (for example, components excluding conductive particles and fillers).

[0119] [Other ingredients]

[0120] The adhesive composition of the present embodiment may also contain other components in addition to the above-mentioned components. As other components, for example, thiol compounds (hereinafter, also referred to as (D) components), coupling agents (hereinafter, also referred to as (E) components), fillers (hereinafter, also referred to as (F) components), etc. can be cited. These components can be used alone or in combination of two or more.

[0121] The thiol compound of the component (D) may be a thiol compound having one thiol group (monofunctional thiol compound) or a thiol compound having a plurality of thiol groups (polyfunctional thiol compound).

[0122] The thiol group contained in the component (D) may be a primary thiol group, a secondary thiol group, or a tertiary thiol group.

[0123] Examples of the monofunctional thiol compound include 2-mercaptobenzothiazole, 2-methyl-4,5-dihydrofuran-3-thiol, 3-mercapto-1-hexanol, mercaptomethylbutanol, 3-mercapto-2-methylpentanol, 3-mercapto-3-methylbutanol, 4-ethoxy-2-methyl-2-butanethiol, hexanethiol, isobutyl mercaptan, 1,1-dimethylheptylthiol, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3-mercaptopropionate, and stearyl-3-mercaptopropionate.

[0124] Examples of the polyfunctional thiol compound include pentaerythritol tetrakis(3-mercaptobutyrate), ethanedithiol, 1,3-propanethiol, 1,4-butanethiol, trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, and tetraethylene glycol bis(3-mercaptopropionate).

[0125] From the viewpoint of suppressing the peeling at the interface between the cured adhesive composition and the circuit component and suppressing the increase in the connection resistance of the circuit connection structure, the content of the component (D) may be 0.05% by mass or more, 0.5% by mass or more, 1.0% by mass or more, or 1.5% by mass or more, based on the total mass of the resin component (e.g., components other than the conductive particles and the filler) of the adhesive composition. In addition, from the viewpoint of suppressing the peeling at the interface between the cured adhesive composition and the circuit component and suppressing the increase in the connection resistance of the circuit connection structure, the content of the component (D) may be 5.0% by mass or less, 3.0% by mass or less, 2.5% by mass or less, or 2.0% by mass or less, based on the total mass of the resin component (e.g., components other than the conductive particles and the filler) of the adhesive composition.

[0126] As the coupling agent of the component (E), a compound having at least one of a vinyl group, an acrylic group (acryloyl group), an amino group, an epoxy group, or an isocyanate group can be used from the viewpoint of improving the adhesiveness. The coupling agent may be a silane coupling agent, for example, vinyl trimethoxysilane, vinyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane, 3-glycidyloxypropyl methyl diethoxysilane, 3-(methyl)acryloxypropyl methyl dimethoxysilane, 3-(methyl)acryloxypropyl trimethoxysilane, 3-(methyl)acryloxypropyl methyl diethoxysilane, 3-(methyl)acryloxypropyl triethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, 3-ureidopropyl triethoxysilane, 3-mercaptopropyl trimethoxysilane, 3-isocyanate propyl triethoxysilane silane and condensates thereof. They may be used alone or in combination of two or more.

[0127] The content of component (E) may be greater than 0.5 mass %, greater than 1 mass %, or greater than 2 mass %, or less than 15 mass %, less than 10 mass %, or less than 5 mass %, based on the total mass of the resin components of the adhesive composition (for example, components other than the conductive particles and the filler).

[0128] As the filler material of component (F), for example, non-conductive fillers (for example, non-conductive particles) can be mentioned. The filler material can be any of an inorganic filler and an organic filler. As an inorganic filler, for example, metal oxide particles such as silica particles, alumina particles, silica-alumina particles, titanium dioxide particles, zirconium oxide particles; inorganic particles such as nitride particles can be mentioned. As an organic filler, for example, organic particles such as silicone particles, methacrylate-butadiene-styrene particles, acrylic-silicone particles, polyamide particles, polyimide particles can be mentioned. These particles can have a uniform structure or a core-shell structure. The maximum diameter of the filler can be smaller than the minimum particle size of the conductive particles.

[0129] The content of component (F) may be 4 to 60% by volume, 5 to 50% by volume, or 6 to 30% by volume based on the total volume of the adhesive composition. In addition, from the perspective of improving connection reliability, the content of the filler may be 3 to 60% by mass, 4 to 40% by mass, or 5 to 20% by mass based on the total mass of the resin components (e.g., components other than the conductive particles and the filler) of the adhesive composition.

[0130] In addition, the adhesive composition of the present embodiment may contain other additives such as a softener, an accelerator, an anti-aging agent, a colorant, a flame retardant, a thixotropic agent, a polymerization inhibitor, etc. Examples of the polymerization inhibitor include hydroquinone and methyl ether hydroquinones.

[0131] <Adhesive film for circuit connection>

[0132] The circuit-connecting adhesive film of the present embodiment may include a resin component containing (A) a thermoplastic resin, (B) a radical polymerizable compound, and (C) a radical polymerization initiator, and (G) conductive particles, and may have the same structure as the adhesive composition of the present embodiment described above.

[0133] In addition, regarding the content of each component, "based on the total amount of the adhesive composition" should be understood as "based on the total amount of the adhesive film", and "based on the total mass of the resin components of the adhesive composition (for example, components other than conductive particles and fillers)" should be understood as "based on the total mass of the resin components of the adhesive film (for example, components other than conductive particles and fillers)".

[0134] When the adhesive film of the present embodiment contains conductive particles, the particle density of the conductive particles in the adhesive film for circuit connection may be 100 particles / mm from the viewpoint of obtaining stable connection resistance. 2 Above, 1000 pieces / mm 2 Above or 3000 pcs / mm 2 From the viewpoint of ensuring insulation between adjacent electrodes, the particle density of the conductive particles in the circuit-connecting adhesive film may be 100,000 particles / mm 2 Below, 50000 pieces / mm 2 Below or 30000 pcs / mm 2 From these viewpoints, the particle density of the conductive particles in the circuit-connecting adhesive film may be 100 to 100,000 particles / mm. 2 1000~50000pcs / mm 2 or 3000~30000pcs / mm 2 .

[0135] The thickness of the circuit-connecting adhesive film may be, for example, 3 μm or more or 10 μm or more, or 30 μm or less or 20 μm or less.

[0136] The circuit-connecting adhesive film of the present embodiment can be preferably used as the following circuit-connecting adhesive film, which is used to connect a first circuit component having a first electrode (for example, a first circuit component having a first circuit electrode formed on the main surface of a first substrate) and a second circuit component having a second electrode (for example, a second circuit component having a second circuit electrode formed on the main surface of a second substrate) in a state in which the first electrode and the second electrode (the first circuit electrode and the second circuit electrode) are arranged opposite to each other.

[0137] For example, from the viewpoint of easily obtaining stable connection resistance, the circuit-connecting adhesive film may have a multilayer structure of two or more layers.

[0138] The adhesive film for circuit connection may be an adhesive film for circuit connection that does not contain conductive particles.

[0139] The circuit connection adhesive film of the present embodiment can be prepared by the following method. Specifically, first, component (A), component (B), component (C), component (D), component (E), and other components added as needed are added to a solvent (organic solvent), and dissolved or dispersed by stirring, mixing, kneading, etc., thereby preparing a varnish composition (varnish-like adhesive composition). Thereafter, the varnish composition is applied to a substrate subjected to a demolding treatment using a blade coater, a roller coater, an applicator, a comma coater, a die coater, etc., and the solvent is volatilized by heating, thereby forming a circuit connection adhesive film on the substrate.

[0140] As the solvent for preparing the varnish composition, a solvent having the characteristic of being able to uniformly dissolve or disperse each component can be used. As such a solvent, for example, toluene, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, propyl acetate, butyl acetate, etc. can be cited. These solvents can be used alone or in combination of two or more. For example, stirring, mixing and mixing when preparing the varnish composition can be performed using a stirrer, a grinder, a three-roller machine, a ball mill, a bead mill, a homogenizing disperser.

[0141] The substrate is not particularly limited as long as it is a material with heat resistance that can withstand the heating conditions for volatilizing the solvent. For example, a substrate (for example, a film) formed of stretched polypropylene (OPP), polyethylene terephthalate (PET), polyethylene naphthalate, polyethylene isophthalate, polybutylene terephthalate, polyolefin, polyacetate, polycarbonate, polyphenylene sulfide, polyamide, polyimide, cellulose, ethylene / vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, synthetic rubber, liquid crystal polymer, etc. can be used.

[0142] The heating conditions for volatilizing the solvent from the varnish composition applied on the substrate can be set to conditions that sufficiently volatilize the solvent. The heating conditions can be, for example, 40° C. to 120° C. and 0.1 minute to 10 minutes.

[0143] The circuit connection adhesive film of this embodiment may not remove part of the solvent but may remain. For example, the content of the solvent in the circuit connection adhesive film of this embodiment may be 10% by mass or less, or 5% by mass or less, based on the total mass of the adhesive film.

[0144] <Circuit connection structure and method for manufacturing the same>

[0145] Next, the circuit connection structure and its manufacturing method are described.

[0146] The circuit connection structure of the present embodiment comprises: a first circuit component having a first electrode; a second circuit component having a second electrode; and a connecting portion, which is arranged between the first circuit component and the second circuit component and electrically connects the first electrode and the second electrode to each other, and the connecting portion comprises a cured product of the adhesive composition of the present embodiment or the adhesive film for circuit connection of the present embodiment.

[0147] The manufacturing method of the circuit connection structure of the present embodiment includes the following steps: heating and pressurizing a first circuit component having a first electrode, a second circuit component having a second electrode, and an adhesive film for circuit connection of the present embodiment in a state where the first electrode and the second electrode are arranged opposite to each other with the adhesive film for circuit connection therebetween, thereby electrically connecting the first electrode and the second electrode.

[0148] Figure 1 This is a schematic cross-sectional view showing one embodiment of a circuit connection structure. Figure 1 The circuit connection structure 1 shown comprises: a first circuit component 20 having a first circuit substrate 21 and a first circuit electrode (first connection terminal) 22 formed on its main surface 21a; a second circuit component 30 having a second circuit substrate 31 and a second circuit electrode (second connection terminal) 32 formed on its main surface 31a; and a connection portion 10 sandwiched between the first circuit component 20 and the second circuit component 30 to bond them together. The second circuit component 30 is arranged opposite to the first circuit component 20 so that the second circuit electrode 32 is opposite to the first circuit electrode 22.

[0149] The connection portion 10 is formed by sandwiching the circuit connection adhesive film of the present embodiment between the first circuit component 20 and the second circuit component 30 and applying pressure in this state, and includes a cured product of the circuit connection adhesive film. In addition, in the present embodiment, an example of forming the connection portion 10 using a circuit connection adhesive film containing conductive particles is shown, and the connection portion 10 is composed of an insulating layer 11 and conductive particles 7 dispersed in the insulating layer 11. The insulating layer 11 is derived from components other than the conductive particles in the adhesive film, and includes a cured product formed by free radical polymerization of a radical polymerizable compound.

[0150] The first circuit electrodes 22 and the second circuit electrodes 32 facing each other are electrically connected via the conductive particles 7. On the other hand, the first circuit electrodes 22 and the second circuit electrodes 32 formed on the same circuit board are insulated from each other.

[0151] Examples of the first circuit board 21 and the second circuit board 31 include chip components such as semiconductor chips, resistor chips, capacitor chips, and substrates such as printed circuit boards. Generally, a large number of connection terminals are provided on circuit components, but a single connection terminal may be provided depending on circumstances.

[0152] More specifically, a substrate of an inorganic material such as a semiconductor, glass, or ceramic, a plastic substrate, or a glass / epoxy substrate is used. Examples of the plastic substrate include polyimide films, polycarbonate films, and polyester films. The first circuit electrode and the second circuit electrode are formed of a metal such as copper. In order to obtain a better electrical connection, it is preferred that the surface of at least one of the first circuit electrode and the second circuit electrode is made of a metal selected from gold, silver, tin, and the platinum group. The surface layer is selected from any one of gold, silver, the platinum group, or tin, and they may also be used in combination. Furthermore, a multilayer structure may be formed by combining a plurality of metals, such as copper / nickel / gold.

[0153] Furthermore, one of the first circuit component 20 and the second circuit component 30 may be a liquid crystal display panel having a glass substrate or a plastic substrate as a circuit substrate and having connection terminals formed of ITO or the like. Furthermore, one of the first circuit component 20 and the second circuit component 30 may be a flexible printed circuit board (FPC), a tape carrier package (TCP) or a chip on film (COF) having a polyimide film as a circuit substrate, or a semiconductor silicon chip having a semiconductor substrate as a circuit substrate. These various circuit components are appropriately combined as needed to form a circuit connection structure.

[0154] Furthermore, in order to eliminate the influence of volatile components due to heating during connection on the connection, it is preferable to perform a pre-heating treatment on the substrate provided with the circuit electrodes before the connection step using the circuit connection adhesive film.

[0155] For example, the circuit connection structure 1 is formed by overlapping the first circuit component 20, the circuit connection adhesive film and the second circuit component 30 in order in such a manner that the first connection terminal 22 and the second connection terminal 32 are opposite to each other, and pressurizing or further heating is performed in this state. The pressure is not particularly limited as long as it is within the range that does not damage the adherend, but is generally preferably 0.1 to 10 MPa. The heating temperature is not particularly limited, but is preferably 100 to 200° C. It is preferred that these pressurization and heating are performed within the range of 0.5 seconds to 100 seconds, and the bonding can be achieved even if heated at 130 to 180° C. and 3 MPa for 10 seconds.

[0156] Example

[0157] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the Examples.

[0158] <Synthesis of polyurethane acrylate (UA1)>

[0159] Into a reaction vessel equipped with a stirrer, a thermometer, a reflux cooling tube with a calcium chloride drying tube, and a nitrogen inlet tube, 2500 parts by mass (2.50 mol) of poly (1,6-hexanediol carbonate) (product name: Duranol T5652, manufactured by Asahi Kasei Corporation, number average molecular weight 1000) and 666 parts by mass (3.00 mol) of isophorone diisocyanate (manufactured by Sigma-Aldrich Co. LLC) were uniformly added dropwise over 3 hours. Then, after nitrogen was fully introduced into the reaction vessel, the reaction vessel was heated to 70-75° C. to react. Next, 0.53 parts by mass (4.3 mmol) of hydroquinone monomethyl ether (manufactured by Sigma-Aldrich Co. LLC) and 5.53 parts by mass (8.8 mmol) of dibutyltin dilaurate (manufactured by Sigma-Aldrich Co. LLC) were added to the reaction container, and 238 parts by mass (2.05 mol) of 2-hydroxyethyl acrylate (manufactured by Sigma-Aldrich Co. LLC) was added, and the mixture was reacted at 70° C. for 6 hours under an air atmosphere. Thus, polyurethane acrylate (UA1) was obtained. The weight average molecular weight of polyurethane acrylate (UA1) was 15,000. In addition, the weight average molecular weight was determined by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene under the following conditions.

[0160] (Measurement conditions)

[0161] Device: GPC-8020 manufactured by TOSOH CORPORATION

[0162] Detector: RI-8020 manufactured by TOSOH CORPORATION

[0163] Chromatographic column: Gelpack GLA160S+GLA150S manufactured by Hitachi Chemical Company, Ltd.

[0164] Sample concentration: 120mg / 3mL

[0165] Solvent: Tetrahydrofuran

[0166] Injection volume: 60μL

[0167] Pressure: 2.94×10 6 Pa(30kgf / cm 2 )

[0168] Flow rate: 1.00mL / min

[0169] <Production of Conductive Particles>

[0170] A layer made of nickel was formed on the surface of the polystyrene particles so as to have a thickness of 0.2 μm, thereby obtaining conductive particles having an average particle diameter of 4 μm, a maximum particle diameter of 4.5 μm, and a specific gravity of 2.5.

[0171] (Example 1 to Example 4, Comparative Example 1 to Comparative Example 4)

[0172] [Manufacturing of adhesive film]

[0173] The following components were mixed in the blending amounts (parts by mass) shown in Table 1 to prepare varnish compositions.

[0174] (Thermoplastic resin)

[0175] A1: A 40 mass % solution prepared by dissolving 40 g of bisphenol A type phenoxy resin (product name: PKHC, manufactured by UNION CARBIDE JAPAN LIMITED) in 60 g of methyl ethyl ketone (the blending amount in the table indicates the blending amount of bisphenol A type phenoxy resin)

[0176] (Radical polymerizable compound)

[0177] B1-1: Cyclopolymerizable monomer (product name: FX-AO-MA, manufactured by Nippon Shokubai Co., Ltd.)

[0178] B2-1: Polyurethane acrylate (UA1) synthesized as above

[0179] B2-2: 2-methacryloyloxyethyl acid phosphate (product name: LIGHT ESTER P-2M, manufactured by KYOEISHA CHEMICAL Co., LTD.)

[0180] B2-3: diacrylate having a tricyclodecane skeleton (dicyclopentadiene type diacrylate) (product name: DCP-A, manufactured by KYOEISHA CHEMICAL CO., LTD.)

[0181] B2-4: Isoborneol acrylate (product name: IBXA, manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD)

[0182] (Free Radical Polymerization Initiator)

[0183] C1: Benzoyl peroxide (product name: NYPER BMT-K40, manufactured by NOF CORPORATION)

[0184] (Thiol Compounds)

[0185] D1: Pentaerythritol tetrakis(3-mercaptobutyrate) (product name: CURRANTS MT PE-1 ("CURRANTS MT" is a registered trademark), manufactured by SHOWA DENKO KK), viscosity (@25°C): 1 Pa·s, molecular weight: 544.8

[0186] (Coupling agent)

[0187] E1: 3-methacryloxypropyltrimethoxysilane (product name: KBM503, manufactured by Shin-Etsu Chemical Co., Ltd.)

[0188] (Filling material)

[0189] F1: Silica fine particles (product name: R104, manufactured by NIPPON AEROSIL CO., LTD., average particle size (primary particle size): 12 nm)

[0190] (Conductive particles)

[0191] G1: Conductive particles made as above

[0192] The varnish composition obtained above was applied onto a PET film having a thickness of 50 μm using a coating device, and then hot air drying was performed at 70° C. for 3 minutes to form an adhesive film having a thickness (thickness after drying) of 10 μm on the PET film.

[0193] [Fabrication of Circuit Connection Structure]

[0194] The prepared adhesive film was interposed between COF (manufactured by FLEXSEED) with a pitch of 25 μm and a thin film electrode (height: ) was used, and a glass substrate with a thin film electrode (manufactured by GEOMATEC Co., Ltd.) was used to heat and pressurize at 180°C and 4.5 MPa for 4 seconds, and connected with a width of 1 mm to produce a circuit connection structure (connection structure).

[0195] [Evaluation of Circuit Connection Structure]

[0196] The obtained circuit-connected structures were evaluated as follows.

[0197] (Connecting resistor)

[0198] The obtained circuit connection structure was measured by a multimeter for the connection resistance between the opposing electrodes immediately after connection and after the high temperature and high humidity test. The high temperature and high humidity test was performed by placing it in a constant temperature and humidity chamber at 85°C and 85%RH for 100 hours. The connection resistance value was calculated as the average value of the resistance between the opposing electrodes at 16 locations.

[0199] [Table 1]

[0200]

[0201] As shown in Table 1, in Examples 1 to 4 using an adhesive film containing a cyclopolymerizable monomer, a circuit connection structure capable of maintaining a sufficiently low connection resistance between opposing electrodes was obtained even after a high temperature and high humidity test.

[0202] Explanation of symbols

[0203] 1-circuit connection structure, 7-conductive particles, 10-connecting portion, 11-insulating layer, 20-first circuit component, 21-first circuit substrate, 22-first circuit electrode (first connecting terminal), 30-second circuit component, 31-second circuit substrate, 32-second circuit electrode (second connecting terminal).

Claims

1. An adhesive composition comprising a thermoplastic resin, a free radical polymerizable compound, a free radical polymerization initiator and conductive particles, The radical polymerizable compound includes a cyclopolymerizable monomer.

2. The adhesive composition according to claim 1, wherein The content of the cyclopolymerizable monomer is 3 to 50% by mass based on the total amount of the radical polymerizable compound.

3. The adhesive composition according to claim 1 or 2, wherein: As the radical polymerizable compound, a (poly)urethane (meth)acrylate compound is further contained. The content of the (poly)urethane (meth)acrylate compound is 100 to 1000 parts by mass based on 100 parts by mass of the cyclopolymerizable monomer.

4. An adhesive film for circuit connection, comprising a thermoplastic resin, a free radical polymerizable compound, a free radical polymerization initiator and conductive particles, The radical polymerizable compound includes a cyclopolymerizable monomer.

5. The circuit connection adhesive film according to claim 4, wherein: The content of the cyclopolymerizable monomer is 3 to 50% by mass based on the total amount of the radical polymerizable compound.

6. The adhesive film for circuit connection according to claim 4 or 5, wherein: As the radical polymerizable compound, a (poly)urethane (meth)acrylate compound is further contained. The content of the (poly)urethane (meth)acrylate compound is 100 to 1000 parts by mass based on 100 parts by mass of the cyclopolymerizable monomer.

7. A circuit connection structure, comprising: A first circuit component having a first electrode; a second circuit component having a second electrode; and a connecting portion disposed between the first circuit component and the second circuit component and electrically connecting the first electrode and the second electrode to each other, The connecting portion comprises a cured product of the adhesive composition according to any one of claims 1 to 3.

8. A method for manufacturing a circuit connection structure, comprising the following steps: A first circuit component having a first electrode, a second circuit component having a second electrode, and an adhesive film for circuit connection according to any one of claims 4 to 6 are heated and pressurized in a state in which the first electrode and the second electrode are arranged opposite to each other with the adhesive film for circuit connection therebetween, thereby electrically connecting the first electrode and the second electrode.