Skin adhesive for pet operation and preparation method thereof
The combination of self-healing composite gelatin formed through Schiff base reaction and bioactive ingredients and other ingredients solves the shortcomings of traditional pet surgery skin adhesives in self-healing, rapid curing, high strength and biocompatibility, significantly improving the Healing efficiency and convenience of postoperative care for pet surgery wounds.
Patent Information
- Application Number
- CN202411053279.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional pet surgery skin adhesives have shortcomings in self-healing, rapid curing, high strength and ultra-strength, which are difficult to meet the needs of modern pet medical care. Especially when handling postoperative wounds of live pets, it is easy to cause the wound to crack again. Prolongs healing time and may cause infection.
Through Schiff base reaction, composite modified gelatin with self-healing function is formed, and mixed with the biological active ingredients uniformly to form a microneedle structure. Combined with polyethylene glycol, collagen fibers and α-cyanoacrylate and other components, it is prepared Pet surgical skin adhesive with fast curing, high strength, ultra toughness and good biocompatibility.
It significantly improves the healing efficiency of pet surgical wounds and the convenience of postoperative care, enhances bond strength and self-repair ability, reduces the risk of wound cracking again, and promotes wound healing and prevents infection.
Smart Images

Figure BDA0004975559850000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a pet surgical skin adhesive and a preparation method thereof. Background Art
[0002] With the continuous development of pet medical technology, the performance requirements for pet surgical skin adhesives are getting higher and higher. Although traditional pet surgical skin adhesives meet the basic wound closure needs to a certain extent, they are insufficient in self-repair, rapid curing, high strength and super toughness, and it is difficult to meet the needs of modern pet medical care. Especially when dealing with postoperative wounds of active pets, these deficiencies are more prominent. It is difficult for pets to rest completely after surgery, and frequent activities can easily cause the wound to crack again, which not only increases the pain of the pet, but also prolongs the healing time and may even cause complications such as infection.
[0003] Therefore, developing a pet surgical skin adhesive with excellent self-healing function, fast curing, high strength, super toughness and good biocompatibility is of great significance for improving the postoperative care effect and wound healing efficiency of pets. Summary of the invention
[0004] In view of the above shortcomings of the prior art, the present invention provides a method for preparing a pet surgical skin adhesive to solve the technical problem that the existing pet surgical skin adhesive is difficult to have self-repair function, rapid curing, high strength, super toughness and good biocompatibility, so as to simplify pet postoperative care operations and improve the healing efficiency of surgical wounds.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A method for preparing a pet surgical skin adhesive, the method comprising the following steps:
[0007] S1: Hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are reacted by Schiff base reaction to form a composite modified gelatin with self-repairing function in situ;
[0008] S2: uniformly mixing the composite modified gelatin with self-repairing function obtained in step S1 with the bioactive component, then injecting the mixture into the mold, centrifuging to allow the mixture to fill the pinholes, removing excess solution on the surface and drying to form a modified gelatin with a microneedle structure;
[0009] S3: Compounding the composite modified gelatin with self-repairing function in step S1 and the modified gelatin with microneedle structure in step S2 with polyethylene glycol, collagen fiber, α-cyanoacrylate and auxiliary agents to obtain the pet surgical skin adhesive.
[0010] In step S1 of the present invention, hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are combined by Schiff base reaction to form a composite modified gelatin with self-repairing function. The composite modified gelatin of the present invention has enhanced mechanical properties and bonding strength, and the self-repairing ability helps the adhesive to restore its integrity when slightly damaged, which is beneficial to simplifying the postoperative care operation of pets, because pets are active and it is difficult for them to follow the postoperative care guidelines like humans.
[0011] In step S2 of the present invention, the composite modified gelatin and the bioactive ingredients are uniformly mixed, and a modified gelatin with a microneedle structure is formed by mold forming, centrifugation and drying processes. The microneedle structure increases the surface area of the adhesive in contact with the skin, which can overcome the tissue contact between the surface layer of the skin and the inside of the wound, and improves the bonding efficiency and tightness; and the introduction of cellulose nanocrystals and the microneedle structure modified gelatin with self-repairing function further ensure the structural strength of the microneedle needle tip, so that the gelatin can still maintain a certain mechanical strength after absorbing water, thereby advantageously avoiding the problem of secondary cracking of the wound caused by the pet's activeness; in addition, as the gelatin dissolves after a certain period of contact with the skin, the bioactive ingredients can be quickly released inside the wound, which is beneficial to promote wound healing, reduce inflammation and prevent infection.
[0012] In step S3 of the present invention, the modified gelatin with self-repairing function and microneedle structure is compounded with other ingredients such as polyethylene glycol, collagen fiber, α-cyanoacrylate and adjuvants, and the obtained adhesive has the characteristics of rapid curing, high strength, super toughness and good biocompatibility. Specifically, the addition of α-cyanoacrylate enables the adhesive to cure quickly when it contacts the skin, shortening the operation time; and the composite modified gelatin with self-repairing function and the modified gelatin with microneedle structure work together with polyethylene glycol and collagen fiber to give the skin adhesive high strength and super toughness, which helps to resist external tension. The raw materials selected in steps S1 to S3 of the present invention have good biocompatibility, ensuring the safety and stability of the adhesive.
[0013] As a preferred technical solution, the hydrazine-modified gelatin is obtained by reacting hydrazine acid with gelatin.
[0014] As a preferred technical solution, the hydrazino acid is at least one of hydrazinoacetic acid, 2,2-hydrazonodi-acetic acid, 3-hydrazinopropionic acid, and 2-hydrazino-2-methyl-propionic acid.
[0015] As a preferred technical solution, the modification method of the aldehyde-modified gelatin is: gelatin and sodium periodate solution are evenly mixed, the mass ratio of sodium periodate to gelatin is 1:5-10, the reaction temperature is controlled at 40-50°C, the reaction time is 1-3h, and aldehyde-modified gelatin is obtained.
[0016] As a preferred technical solution, the modification method of the aldehyde-modified cellulose nanocrystals is: cellulose nanocrystals are evenly mixed with sodium periodate solution, the mass ratio of sodium periodate to cellulose nanocrystals is 1:2-5, the reaction temperature is controlled at 25-35°C, the reaction time is 0.5-1.5h, and aldehyde-modified cellulose nanocrystals are obtained.
[0018] As a preferred technical solution, in step S1, the reaction conditions of the Schiff base reaction include: under the conditions of a temperature of 25 to 40°C and a pH value of 7.5 to 8.5, the solvent is a mixture of water and ethanol, and the stirring reaction time is 4 to 6 hours. The molar ratio of the hydrazine-modified gelatin, the aldehyde-modified gelatin and the aldehyde-modified cellulose nanocrystals is 2 to 3: 1 to 1.5: 0.8 to 1.2.
[0019] As a preferred technical solution, the bioactive ingredient is at least one substance selected from the group consisting of corticosteroids, antibiotics, collagen, laminin, fibronectin, and vascular endothelial growth factor.
[0020] As a preferred technical solution, the α-cyanoacrylate is at least one of ethyl α-cyanoacrylate, methoxyethyl α-cyanoacrylate, n-butyl α-cyanoacrylate, n-octyl α-cyanoacrylate, and sec-octyl α-cyanoacrylate.
[0021] As a preferred technical solution, the auxiliary agent is at least one of a plasticizer, a stabilizer, and an antioxidant.
[0022] As a preferred technical solution, in step S3, the raw materials compounded for the pet surgical skin adhesive are, in parts by weight, 30 to 50 parts of composite modified gelatin with self-repairing function, 10 to 20 parts of modified gelatin with a microneedle structure, 5 to 15 parts of polyethylene glycol, 5 to 15 parts of collagen fibers, 1 to 5 parts of α-cyanoacrylate and 1 to 10 parts of auxiliary agents.
[0023] Another aspect of the present invention is to provide a pet surgical skin adhesive, wherein the skin adhesive is prepared by the above-mentioned preparation method of the pet surgical skin adhesive.
[0024] Beneficial effects of the present invention:
[0025] The preparation method of the pet surgical skin adhesive of the present invention, through the compounding of composite modified gelatin with self-repairing function, modified gelatin with microneedle structure, polyethylene glycol, collagen fiber, α-cyanoacrylate and auxiliary agents, makes the prepared pet surgical skin adhesive have excellent biocompatibility and adhesion effect, which not only realizes excellent self-repairing function, but also enhances mechanical properties and rapid curing performance, thereby significantly improving the healing efficiency of pet surgical wounds and the convenience of postoperative care. DETAILED DESCRIPTION
[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0027] Example 1
[0028] The preparation method of the pet surgical skin adhesive in this embodiment comprises the following steps:
[0029] S1: Hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are reacted by Schiff base reaction to form a composite modified gelatin with self-repairing function in situ; the molar ratio of the hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals is 3:1.5:1.2. The reaction conditions of the Schiff base reaction include: at a temperature of 30°C and a pH value of 8, the solvent is a mixture of water and ethanol (volume ratio of 1:1), and the stirring reaction time is 4 hours.
[0030] S2: Evenly mix 70 parts by weight of the composite modified gelatin with self-repairing function obtained in step S1 with 0.5 parts by weight of antibiotics, 18 parts by weight of collagen, 11 parts by weight of fibronectin, and 0.5 parts by weight of vascular endothelial growth factor, and then inject the mixed solution into the mold, centrifuge it to allow the mixed solution to fill the pinholes, remove excess solution on the surface and dry it to form a modified gelatin with a microneedle structure.
[0031] S3: Compounding the composite modified gelatin with self-repairing function in step S1 and the modified gelatin with microneedle structure in step S2 with polyethylene glycol, collagen fiber, ethyl α-cyanoacrylate and an auxiliary agent to obtain the pet surgical skin adhesive. The raw materials compounded in the pet surgical skin adhesive are, by weight, 30 parts of composite modified gelatin with self-repairing function, 10 parts of modified gelatin with microneedle structure, 5 parts of polyethylene glycol, 5 parts of collagen fiber, 1 part of ethyl α-cyanoacrylate and 2 parts of an auxiliary agent.
[0032] The hydrazine-modified gelatin is obtained by reacting hydrazine acid with gelatin. Specifically, 20 g of gelatin is dissolved in 250 mL of deionized water to form a uniform solution; then 0.2 mmol of hydrazine acetic acid and 0.5 g of N-hydroxysuccinimide are added to react; during the reaction, the pH value is controlled to be 4.5 and the temperature is 45°C; after reacting for 6 hours, the pH value is adjusted to 7.0 to stop the reaction.
[0033] The modification method of the aldehyde-modified gelatin is as follows: gelatin and sodium periodate solution are uniformly mixed, the mass ratio of sodium periodate to gelatin is 1:5, the reaction temperature is controlled to be 40° C., and the reaction time is 2 hours to obtain the aldehyde-modified gelatin.
[0034] The modification method of the aldehyde-modified cellulose nanocrystals is as follows: cellulose nanocrystals are uniformly mixed with sodium periodate solution, wherein the mass ratio of sodium periodate to cellulose nanocrystals is 1:2, the reaction temperature is controlled to be 25° C., and the reaction time is 1.5 hours, to obtain aldehyde-modified cellulose nanocrystals.
[0035] The auxiliary agent consists of epoxidized soybean oil and vitamin E in a mass ratio of 3:2.
[0036] Example 2
[0037] The preparation method of the pet surgical skin adhesive in this embodiment comprises the following steps:
[0038] S1: Hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are reacted by Schiff base reaction to form a composite modified gelatin with self-repairing function in situ; the molar ratio of the hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals is 2.5:1.2:1. The reaction conditions of the Schiff base reaction include: at a temperature of 40°C and a pH value of 8.5, the solvent is a mixture of water and ethanol (volume ratio of 1:1), and the stirring reaction time is 4 hours.
[0039] S2: Evenly mix 75 parts by weight of the composite modified gelatin with self-repairing function obtained in step S1 with 0.4 parts by weight of antibiotics, 15 parts by weight of collagen, 9 parts by weight of fibronectin, and 0.6 parts by weight of vascular endothelial growth factor, then inject the mixed solution into the mold, centrifuge to allow the mixed solution to fill the pinholes, remove excess solution on the surface and dry to form a modified gelatin with a microneedle structure.
[0040] S3: Compound the composite modified gelatin with self-repairing function in step S1 and the modified gelatin with microneedle structure in step S2 with polyethylene glycol, collagen fiber, α-butyl cyanoacrylate and auxiliary agent to obtain the pet surgical skin adhesive. The raw materials compounded in the pet surgical skin adhesive are, by weight, 40 parts of composite modified gelatin with self-repairing function, 15 parts of modified gelatin with microneedle structure, 10 parts of polyethylene glycol, 8 parts of collagen fiber, 3 parts of α-butyl cyanoacrylate and 5 parts of auxiliary agent.
[0041] The hydrazine-modified gelatin is obtained by reacting hydrazine acid with gelatin. Specifically, 20 g of gelatin is dissolved in 250 mL of deionized water to form a uniform solution; then 0.2 mmol of 2,2-hydrazonodiacetic acid and 0.5 g of N-hydroxysuccinimide are added to react; during the reaction, the pH value is controlled to be 5 and the temperature is 45°C; after reacting for 8 hours, the pH value is adjusted to 7.0 to stop the reaction.
[0042] The modification method of the aldehyde-modified gelatin is as follows: gelatin and sodium periodate solution are uniformly mixed, the mass ratio of sodium periodate to gelatin is 1:8, the reaction temperature is controlled to be 50° C., and the reaction time is 3 hours to obtain the aldehyde-modified gelatin.
[0043] The modification method of the aldehyde-modified cellulose nanocrystals is as follows: cellulose nanocrystals are uniformly mixed with sodium periodate solution, wherein the mass ratio of sodium periodate to cellulose nanocrystals is 1:4, the reaction temperature is controlled at 30°C, and the reaction time is 1h, to obtain aldehyde-modified cellulose nanocrystals.
[0044] The auxiliary agent consists of epoxidized soybean oil and vitamin E in a mass ratio of 3:2.
[0045] Example 3
[0046] The preparation method of the pet surgical skin adhesive in this embodiment comprises the following steps:
[0047] S1: Hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are reacted in situ to form a composite modified gelatin with self-repairing function through Schiff base reaction; the molar ratio of hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals is 2:1:0.8. The reaction conditions of the Schiff base reaction include: at a temperature of 25°C and a pH value of 8.5, the solvent is a mixture of water and ethanol (volume ratio of 1:1), and the stirring reaction time is 6 hours.
[0048] S2: Evenly mix 72 parts by weight of the composite modified gelatin with self-repairing function obtained in step S1 with 0.6 parts by weight of antibiotics, 16 parts by weight of collagen, 11 parts by weight of fibronectin, and 0.4 parts by weight of vascular endothelial growth factor, and then inject the mixed solution into the mold, centrifuge it to allow the mixed solution to fill the pinholes, remove excess solution on the surface and dry it to form a modified gelatin with a microneedle structure.
[0049] S3: Compounding the composite modified gelatin with self-repairing function in step S1 and the modified gelatin with microneedle structure in step S2 with polyethylene glycol, collagen fiber, α-octyl cyanoacrylate and auxiliary agent to obtain the pet surgical skin adhesive. The raw materials compounded in the pet surgical skin adhesive are, by weight, 50 parts of composite modified gelatin with self-repairing function, 20 parts of modified gelatin with microneedle structure, 15 parts of polyethylene glycol, 12 parts of collagen fiber, 5 parts of α-octyl cyanoacrylate and 7 parts of auxiliary agent.
[0050] The hydrazine-modified gelatin is obtained by reacting hydrazine acid with gelatin. Specifically, 20 g of gelatin is dissolved in 250 mL of deionized water to form a uniform solution; then 0.2 mmol of 3-hydrazine propionic acid and 0.5 g of N-hydroxysuccinimide are added to react; during the reaction, the pH value is controlled to be 4 and the temperature is 40°C; after reacting for 4 hours, the pH value is adjusted to 7.0 to stop the reaction.
[0051] The modification method of the aldehyde-modified gelatin is as follows: gelatin and sodium periodate solution are uniformly mixed, the mass ratio of sodium periodate to gelatin is 1:10, the reaction temperature is controlled to be 50° C., and the reaction time is 3 hours to obtain the aldehyde-modified gelatin.
[0052] The modification method of the aldehyde-modified cellulose nanocrystals is as follows: cellulose nanocrystals are uniformly mixed with sodium periodate solution, wherein the mass ratio of sodium periodate to cellulose nanocrystals is 1:5, the reaction temperature is controlled at 35° C., and the reaction time is 1.5 hours to obtain aldehyde-modified cellulose nanocrystals.
[0053] The auxiliary agent consists of epoxidized soybean oil and vitamin E in a mass ratio of 3:2.
[0054] Comparative Example 1
[0055] The raw material composition and preparation steps of the preparation method of the pet surgical skin adhesive in this comparative example are basically the same as those in Example 1, except that, in the preparation method of the adhesive in this comparative example, the gelatin modification treatment operation of step S1 is omitted, and unmodified gelatin is directly used to replace the composite modified gelatin with self-repairing function in step S1.
[0056] Comparative Example 2
[0057] The raw material composition and preparation steps of the comparative example pet surgical skin adhesive are basically the same as those of Example 1, except that, in the comparative example adhesive preparation method, step S2 of preparing modified gelatin with a microneedle structure is omitted, that is, the composite modified gelatin with self-repairing function obtained in step S1 is evenly mixed with antibiotics, collagen, fibronectin and vascular endothelial growth factor, but not injected into the mold and dried to form the modified gelatin with a microneedle structure.
[0058] The pet surgical skin adhesive samples prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance tests, and the performance results are shown in Table 1:
[0059] The biocompatibility test method is tested with reference to ISO 10993-10 "Biological evaluation of medical devices - Part 10: Test methods for irritation and sensitization". It assesses whether the adhesive sample will cause skin irritation or allergic reaction.
[0060] The adhesion test method is based on ASTM F2255 "Standard Test Method for Shear Bond Strength of Medical Adhesives" and is evaluated by the bonding strength (MPa).
[0061] The self-healing function test method simulates the damage and self-healing process that the adhesive may encounter in actual use by periodically stretching and releasing the adhesive sample (under the conditions of temperature of 25°C and humidity of 50%, after each stretching, it is placed for 2 hours and 10 cycles are tested). The self-healing ability of the adhesive is evaluated by measuring the recovery rate (%) of the bonding strength.
[0062] The toughness test method is tested with reference to ASTM D1018 "Standard Test Method for Izod Beam Impact Testing of Polymer Materials". Use an Izod beam impact tester to impact the adhesive sample, record the energy absorbed when the sample breaks, expressed in J / m, and evaluate the impact absorption capacity of the adhesive.
[0063] The curing performance test method measures the time from when the adhesive contacts the simulated skin sample to when the preset bonding strength (4.5MPa) is reached. Table 1
[0064] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.
Claims
1. A method for preparing a pet surgical skin adhesive, characterized in that: The preparation method comprises the following steps: S1: Hydrazine-modified gelatin, aldehyde-modified gelatin and aldehyde-modified cellulose nanocrystals are reacted by Schiff base reaction to form a composite modified gelatin with self-repairing function in situ; S2: uniformly mixing the composite modified gelatin with self-repairing function obtained in step S1 with the bioactive component, then injecting the mixture into the mold, centrifuging to allow the mixture to fill the pinholes, removing excess solution on the surface and drying to form a modified gelatin with a microneedle structure; S3: Compounding the composite modified gelatin with self-repairing function in step S1 and the modified gelatin with microneedle structure in step S2 with polyethylene glycol, collagen fiber, α-cyanoacrylate and auxiliary agents to obtain the pet surgical skin adhesive.
2. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The hydrazine-modified gelatin is obtained by reacting hydrazine acid with gelatin.
3. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The hydrazino acid is at least one of hydrazinoacetic acid, 2,2-hydrazonodi-acetic acid, 3-hydrazinopropionic acid, and 2-hydrazino-2-methyl-propionic acid.
4. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The modification method of the aldehyde-modified gelatin is as follows: gelatin and sodium periodate solution are uniformly mixed, the mass ratio of sodium periodate to gelatin is 1:5-10, the reaction temperature is controlled at 40-50°C, the reaction time is 1-3h, and the aldehyde-modified gelatin is obtained.
5. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The modification method of the aldehyde-modified cellulose nanocrystals is as follows: cellulose nanocrystals are uniformly mixed with a sodium periodate solution, wherein the mass ratio of the sodium periodate to the cellulose nanocrystals is 1:2-5, the reaction temperature is controlled at 25-35°C, and the reaction time is 0.5-1.5h, to obtain the aldehyde-modified cellulose nanocrystals.
6. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: In step S1, the reaction conditions of the Schiff base reaction include: under the conditions of a temperature of 25 to 40° C., a pH value of 7.5 to 8.5, a solvent of a mixture of water and ethanol, and a stirring reaction time of 4 to 6 hours.
7. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The bioactive component is at least one of corticosteroids, antibiotics, collagen, laminin, fibronectin, and vascular endothelial growth factor.
8. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The α-cyanoacrylate is at least one of ethyl α-cyanoacrylate, methoxyethyl α-cyanoacrylate, n-butyl α-cyanoacrylate, n-octyl α-cyanoacrylate, and sec-octyl α-cyanoacrylate.
9. The method for preparing the pet surgical skin adhesive according to claim 1, characterized in that: The auxiliary agent is at least one of a plasticizer, a stabilizer and an antioxidant.
10. A pet surgical skin adhesive, characterized in that: The skin adhesive is prepared by the method for preparing the pet surgical skin adhesive according to any one of claims 1 to 9.