Polytetrafluoroethylene microporous membrane, hydrophilic modification method thereof and water treatment device
By introducing benzene ring and hydrophobic chain segments on the polytetrafluoroethylene microporous membrane and crosslinking under ultraviolet light, the problems of easy deformation and poor water resistance of the polytetrafluoroethylene microporous membrane are solved, and the modulus and water resistance are improved and reduce the cost of cross-linking reaction, achieving efficient water treatment effect.
Patent Information
- Application Number
- CN202411149742.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
The polytetrafluoroethylene microporous membrane is prone to deformation and the existing hydrophilic modification methods lead to poor water resistance, especially when treating high-concentration polluted wastewater, the material needs high water flattening resistance and high crosslinking reaction costs.
Alcohol solvents, hydrophilic modified materials and photoinitiators are used to prepare hydrophilic modified photosensitive solutions. The benzene ring and hydrophobic chain segment are introduced on PVA through acetal and ring-opening reactions, which improves the modulus and cross-linking degree and is in ultraviolet. Cross-linking is performed under light to form a hydrophilic polytetrafluoroethylene microporous film.
The modulus and water resistance of the PTFE microporous membrane are improved, the polar group content is reduced, the stability and durability of the material are enhanced, and the equipment investment and operating costs are reduced through low-energy ultraviolet light cross-linking.
Smart Images

Figure BDA0005003305840000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polytetrafluoroethylene materials, and in particular relates to a hydrophilic modification technology of a polytetrafluoroethylene microporous membrane. Background Art
[0002] Polytetrafluoroethylene (PTFE) has excellent resistance to strong acids and alkalis, and will not decompose even under high temperature conditions, so it has excellent stability. The microporous membrane made of PTFE can intercept tiny particles due to its special asymmetric polymer chain structure, and has a very high filtration effect due to its chemical corrosion resistance. The filter membrane can meet the filtration of corrosive liquids.
[0003] However, the material itself is chemically inert and has low surface energy, is extremely hydrophobic, and is difficult for water to penetrate. Therefore, it cannot be used directly for liquid water separation and requires hydrophilic modification.
[0004] There are many hydrophilic modification methods disclosed in the prior art. For example, the applicant's prior application, Chinese patent with publication number CN115245743A, discloses a polytetrafluoroethylene microporous membrane and its hydrophilic modification method. DMF solution, triethylamine and PU are added to a reaction container, and the PU solution is prepared by sufficient stirring. The PTFE membrane anchored with perfluoroalkylsulfonyl fluoride is transferred to the PU solution, and the solution is placed under vacuum at -0.06 to -0.1 MPa for 5 to 30 minutes and then allowed to stand for 2 to 10 hours. The PTFE microporous membrane is taken out and placed in an oven at 50 to 80°C for drying for 1 to 4 hours. In this process, the sulfonyl fluoride reacts with the primary and secondary amines of the PU to generate a topological structure, which is anchored on the polytetrafluoroethylene to introduce hydrophilic sulfonamide groups, ether bonds and amino structures. Since the fluorocarbon chain of the Rf-structure has a low surface energy and has good bonding with PTFE, sulfonyl fluoride reacts with the primary and secondary amino groups on the polyether urea structural material to undergo a sulfonylation reaction, and sulfonamide groups, ether bonds and amino structures are introduced into PTFE to enhance the acid and alkali tolerance of the hydrophilic coating.
[0005] Another example is the Chinese patent application with publication number CN117771960 A, which discloses a method for hydrophilic modification of polytetrafluoroethylene membranes. The main steps of the hydrophilic modification method are: soaking the polytetrafluoroethylene membrane in an organic solvent until it is transparent, taking it out and soaking it in a hydrophilic PVA mixed solution, wherein the hydrophilic PVA mixed solution includes PVA and a hydrophilic component containing amino groups; placing the soaked polytetrafluoroethylene membrane in a crosslinking agent aqueous solution, heating the reaction and drying it to obtain a pre-modified polytetrafluoroethylene membrane; placing the pre-modified polytetrafluoroethylene membrane in a γ-glycidyloxypropyltrimethoxysilane aqueous solution, heating the reaction and drying it to obtain a hydrophilic modified polytetrafluoroethylene membrane. It constructs a micro-nano structure on the polytetrafluoroethylene membrane to enhance the hydrophilicity and durability of the modified polytetrafluoroethylene membrane.
[0006] However, since the PTFE microporous membrane is expanded, the modulus is low and it is easy to deform, and the prior art does not solve this problem well. In addition, since the PVA side chain contains a large number of polar hydroxyl groups, it has strong hydrophilicity, resulting in poor water resistance and easy swelling and dissolution in water. Summary of the invention
[0007] In view of the problems existing in the prior art, the present invention provides a polytetrafluoroethylene microporous membrane and its hydrophilic modification method and a water treatment device, which solve the problems of easy deformation of the PTFE microporous membrane and poor water resistance caused by excessively enhanced hydrophilicity, and reduce the cost of the cross-linking reaction.
[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0009] First, a method for hydrophilic modification of a polytetrafluoroethylene microporous membrane is provided, comprising the following steps:
[0010] Adding an alcohol solvent, a hydrophilic modification material and a photoinitiator into a light-proof reaction container to prepare a hydrophilic modification photosensitive solution, wherein the hydrophilic modification material comprises a PVA solution, aminobenzaldehyde, glacial acetic acid, alkylsulfonyl chloride and an epoxy material, wherein the glacial acetic acid causes the aldehyde group in the aminobenzaldehyde to react with the hydroxyl group of the PVA to undergo an acetal reaction and introduce an amino group and a benzene ring, the alkylsulfonyl chloride is used to introduce a hydrophobic segment into the PVA, and the epoxy group in the epoxy material reacts with the hydroxyl group of the PVA to undergo a ring-opening reaction, thereby introducing a photosensitive group into the PVA;
[0011] Placing the PTFE microporous membrane in the hydrophilic modified photosensitive solution in the reaction container so that the PTFE microporous membrane is evenly coated with a layer of material containing polar groups;
[0012] The PTFE microporous membrane coated with the polar group-containing material is taken out from the reaction container, and is subjected to ultraviolet crosslinking under ultraviolet light irradiation to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0013] Preferably, the PVA solution is prepared by stirring and dissolving polyvinyl alcohol and deionized water in a heated water bath; and / or the concentration of the PVA solution is 3-8%.
[0014] Preferably, the aminobenzaldehyde is: p-aminobenzaldehyde, o-phenylaminobenzaldehyde, m-phenylaminobenzaldehyde, p-acetylaminobenzaldehyde, 2,4-diaminobenzaldehyde, 2-amino-3,5-dibromobenzaldehyde, one or more thereof; and / or, the alkylsulfonyl chloride is: pentanesulfonyl chloride, octanesulfonyl chloride, undecanesulfonyl chloride, dodecanesulfonyl chloride, pentadecanesulfonyl chloride, heptadecanylsulfonyl chloride, octadecanesulfonyl chloride, one or more thereof.
[0015] Preferably, the preparation method of the hydrophilic modified material comprises the following steps:
[0016] Adding aminobenzaldehyde to the PVA solution;
[0017] Add glacial acetic acid and stir to make the aldehyde group in aminobenzaldehyde react with the hydroxyl group of PVA to introduce amino group and benzene ring;
[0018] After the acetalization reaction is completed, alkylsulfonyl chloride is added and stirred to introduce hydrophobic segments into PVA to obtain a PVA-AbA solution;
[0019] The PVA-AbA solution is transferred to a light-proof reaction container, and epoxy material is added to allow the epoxy group to undergo a ring-opening reaction with the hydroxyl group of PVA, thereby introducing a photosensitive group onto the PVA.
[0020] Preferably, the epoxy material is one or more of 4-vinylbenzyl glycidyl ether, allyl glycidyl ether, and glycidyl methacrylate.
[0021] Preferably, the PVA-AbA solution is transferred to a light-proof reaction container, an alcohol solvent and triethylamine are added, and the mixture is heated to a set temperature and stirred for a set time before adding the epoxy material and stirring for reaction.
[0022] Preferably, the alcohol solvent is one or at least two of methanol, ethanol, propanol and butanol.
[0023] Preferably, the PTFE microporous membrane is placed in the hydrophilic modified photosensitive solution in the reaction container, degassed for 30-60 minutes by means of an ultrasonic and vacuum-assisted system, and then allowed to stand for 1-6 hours, so that a layer of material containing polar groups is evenly coated on the PTFE.
[0024] Secondly, a polytetrafluoroethylene microporous membrane is provided, which is modified by the hydrophilic modification method.
[0025] In addition, a water treatment device is also provided, comprising the polytetrafluoroethylene microporous membrane.
[0026] The technical solution adopted by the present invention has the following beneficial effects:
[0027] Since the PTFE microporous membrane is expanded, it has a low modulus and is easily deformed, especially when treating high-concentration polluted wastewater, the material itself needs to have a high ability to resist water flattening. In response to this demand, the present invention adopts a technical solution of introducing a benzene ring, which is a rigid group. The introduction of the benzene ring improves the modulus of the PTFE microporous membrane material.
[0028] In order to introduce the benzene ring, a condensation reaction occurred between the aldehyde group of aminobenzaldehyde and the hydroxyl group of PVA to introduce the benzene ring and the amino group into the PVA skeleton.
[0029] Since PVA side chains contain a large number of polar hydroxyl groups and have strong hydrophilicity, they have poor water resistance and are prone to swelling and dissolution in water. Therefore, in addition to increasing the degree of cross-linking, it is also necessary to introduce hydrophobic segments into the cross-linked PVA skeleton macromolecules to reduce the content of polar groups, that is, to reduce the polarity of the polymer so that water cannot enter, or enters less. In response to this demand, the present invention adopts a technical solution of introducing long carbon chain hydrophobic segments.
[0030] The free amino group and alkylsulfonyl chloride undergo Hinsberg reaction to introduce long carbon chain hydrophobic segments on PVA. The introduction of long carbon chain hydrophobic segments further reduces the polarity of PVA, making it easier for PVA to bind to the PTFE surface.
[0031] Through the ring-opening reaction between the epoxy group of propylene / vinyl glycidyl ether and the hydroxyl group of PVA, photosensitive groups are introduced into PVA. After chemical modification of PVA, PVA is given photosensitivity, and the photosensitive groups are cross-linked under ultraviolet conditions, which improves the stability of PVA. In this way, low-energy ultraviolet light is used as the radiation source, and the equipment is easy to obtain, the investment cost is low, and the operation is simple.
[0032] The specific technical solutions and beneficial effects of the present invention will be described in detail in the following specific embodiments. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Those skilled in the art will appreciate that, in the absence of conflict, the features in the following embodiments and implementations may be combined with each other.
[0035] The embodiment of the present invention first provides a material for hydrophilic modification of polytetrafluoroethylene microporous membrane, including PVA solution, aminobenzaldehyde, glacial acetic acid, alkylsulfonyl chloride, and epoxy material.
[0036] Among them, glacial acetic acid causes the aldehyde group in aminobenzaldehyde to react with the hydroxyl group of PVA to undergo acetal reaction and introduce amino groups and benzene rings. Alkyl sulfonyl chloride is used to introduce hydrophobic segments into PVA. The epoxy group in the epoxy material undergoes a ring-opening reaction with the hydroxyl group of PVA to introduce photosensitive groups into PVA.
[0037] It is to be understood that glacial acetic acid may also be replaced by materials that can perform similar functions.
[0038] The preparation method of the above hydrophilic modified material comprises the following steps:
[0039] Adding aminobenzaldehyde to the PVA solution;
[0040] Add glacial acetic acid and stir to make the aldehyde group in aminobenzaldehyde react with the hydroxyl group of PVA to introduce amino group and benzene ring;
[0041] After the acetalization reaction is completed, alkylsulfonyl chloride is added and stirred to introduce hydrophobic segments into PVA to obtain a PVA-AbA solution;
[0042] The PVA-AbA solution is transferred to a light-proof reaction container, and epoxy material is added to allow the epoxy group to undergo a ring-opening reaction with the hydroxyl group of PVA, thereby introducing a photosensitive group onto the PVA.
[0043] The PVA solution is prepared by stirring and dissolving polyvinyl alcohol and deionized water in a heated water bath. The concentration of the PVA solution is 3-8%, preferably 5%, and the temperature of the heated water bath is 95°C.
[0044] Preferably, the aminobenzaldehyde is p-aminobenzaldehyde, o-phenylaminobenzaldehyde, m-phenylaminobenzaldehyde, p-acetylaminobenzaldehyde, 2,4-diaminobenzaldehyde and 2-amino-3,5-dibromobenzaldehyde, or one or more thereof. Moreover, the amount of the aminobenzaldehyde added is 5-15% by mass of the PVA solution, such as 8%, 10%, or 12%; the amount of the glacial acetic acid added is 1-5% by mass of the PVA solution, such as 2%, 3%, or 4%.
[0045] Preferably, the alkyl sulfonyl chloride is one or more of pentanesulfonyl chloride, octanesulfonyl chloride, undecanesulfonyl chloride, dodecanesulfonyl chloride, pentadecanesulfonyl chloride, heptadecanylsulfonyl chloride and octadecanesulfonyl chloride. After the acetalization reaction is completed, the alkyl sulfonyl chloride is added, and the added alkyl sulfonyl chloride accounts for 2-15% of the mass percentage of the PVA solution, such as 3%, 6%, 8%, 10%, 12%.
[0046] Preferably, the epoxy material is one or more of 4-vinylbenzyl glycidyl ether, allyl glycidyl ether, and glycidyl methacrylate.
[0047] In the preparation method of the above-mentioned hydrophilic modified material, the PVA-AbA solution is transferred to a light-proof reaction container, and an alcohol solvent is first added to prepare a 1-5% solution, wherein the alcohol solvent can be one or at least two of methanol, ethanol, propanol, and butanol, and at the same time, 0.5-3% of triethylamine by mass of the solution is added for catalysis, and after heating to a set temperature and stirring for a set time, 1-5% of the epoxy material by mass of the solution is added and stirred for reaction.
[0048] Preferably, after catalysis, the mixture is heated to 100° C. and stirred for 4-6 hours; after the epoxy material is added, the stirring time is 10-12 hours.
[0049] In addition, the embodiment of the present invention also provides a method for hydrophilic modification of a polytetrafluoroethylene microporous membrane, comprising the following steps:
[0050] An alcohol solvent, a hydrophilic modified material and a cationic photoinitiator are added to a light-proof reaction container to prepare a hydrophilic modified photosensitive solution; wherein the mass ratio of the alcohol solvent: the hydrophilic modified material: the cationic photoinitiator is 100:1-3:0.5-1, for example 100:2:0.8.
[0051] Placing the PTFE microporous membrane in the hydrophilic modified photosensitive solution in the reaction container so that the PTFE microporous membrane is evenly coated with a layer of material containing polar groups;
[0052] The PTFE microporous membrane coated with the polar group-containing material is taken out from the reaction container, and is subjected to ultraviolet crosslinking under ultraviolet light irradiation to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
[0053] Wherein, the alcohol solvent is one or at least two of methanol, ethanol, propanol and butanol.
[0054] The PTFE microporous membrane is placed in the hydrophilic modified photosensitive solution in the reaction container, and after degassing for 30-60 minutes with the help of ultrasound and vacuum auxiliary system, it is allowed to stand for 1-6 hours, so that a layer of material containing polar groups is evenly coated on the PTFE.
[0055] On the basis of the above, an embodiment of the present invention further provides a polytetrafluoroethylene microporous membrane, which is modified by the above hydrophilic modification method.
[0056] It can be understood that the polytetrafluoroethylene microporous membrane prepared by the above method can replace the conventional polytetrafluoroethylene microporous membrane and be used in various water treatment devices that originally used conventional polytetrafluoroethylene microporous membranes.
[0057] Since the PTFE microporous membrane is expanded, it has a low modulus and is easily deformed, especially when treating high-concentration polluted wastewater, the material itself needs to have a high ability to resist water flattening. The technical solution specifically adopted in this embodiment is to introduce a benzene ring, which is a rigid group. The introduction of the benzene ring increases the modulus of the PTFE microporous membrane material.
[0058] In order to introduce the benzene ring, a condensation reaction occurred between the aldehyde group of aminobenzaldehyde and the hydroxyl group of PVA to introduce the benzene ring and the amino group into the PVA skeleton.
[0059] In addition, since the PVA side chains contain a large number of polar hydroxyl groups and have strong hydrophilicity, they have poor water resistance and are prone to swelling and dissolution in water. Therefore, in addition to increasing the degree of cross-linking, it is also necessary to introduce hydrophobic segments into the cross-linked PVA skeleton macromolecules to reduce the content of polar groups, that is, to reduce the polarity of the polymer so that water cannot enter, or enters less. In response to this demand, the present invention adopts a technical solution of introducing long carbon chain hydrophobic segments.
[0060] The free amino group and alkylsulfonyl chloride undergo Hinsberg reaction to introduce long carbon chain hydrophobic segments on PVA. The introduction of long carbon chain hydrophobic segments further reduces the polarity of PVA, making it easier for PVA to bind to the PTFE surface.
[0061] Through the ring-opening reaction between the epoxy group of propylene / vinyl glycidyl ether and the hydroxyl group of PVA, photosensitive groups are introduced into PVA. After chemical modification of PVA, PVA is given photosensitivity, and the photosensitive groups are cross-linked under ultraviolet conditions, which improves the stability of PVA. In this way, low-energy ultraviolet light is used as the radiation source, and the equipment is easy to obtain, the investment cost is low, and the operation is simple.
[0062] The technical solution of the present invention is further described below in conjunction with specific examples.
[0063] Example 1:
[0064] 1) Take 5 g of polyvinyl alcohol 1799 (alcoholysis degree 98% to 99%) and 95 ml of deionized water, heat and stir in a 95°C water bath to completely dissolve to obtain a 5% solution;
[0065] 2) Add 2.0 g of p-aminobenzaldehyde and 1.0 g of glacial acetic acid to the dissolved 5% PVA solution and stir for 8 h to allow the aldehyde group to react with the hydroxyl group of PVA to undergo acetalization.
[0066] 3) After the reaction was completed, 1.1 g of dodecylsulfonyl chloride was added while stirring, and PVA-AbA was obtained after 3 hours.
[0067] 4) The PVA-AbA solution was transferred to a brown / light-opaque reaction vessel, and a certain amount of 100 mL of ethanol and 2.0 g of triethylamine were added. After heating to 100° C., 2.2 g of allyl glycidyl ether was added and stirred for 10 h to obtain the product PVA-AbA-Alsc-1.
[0068] 5) Clean the 0.4 micron PTFE microporous membrane with ethanol and dry it with hot air. Add 200 ml of methanol to a light-proof reaction vessel, and add the synthesized PVA-AbA-Alsc-1 and cationic photoinitiator. Place the cleaned PTFE microporous membrane in a reaction vessel, degas for 30-60 minutes with the help of ultrasound and vacuum-assisted systems, and then let it stand for 1-6 hours so that a layer of material containing polar groups is evenly coated on the PTFE. Take out the PTFE microporous membrane coated with PVA-AbA-Alsc from the reaction vessel, and after ultraviolet crosslinking for a period of time under ultraviolet light irradiation, a hydrophilic polytetrafluoroethylene microporous membrane is obtained.
[0069] Example 2:
[0070] 1) Take 5 g of polyvinyl alcohol 1799 (alcoholysis degree 98% to 99%) and 95 ml of deionized water, heat and stir in a 95°C water bath to completely dissolve to obtain a 5% solution;
[0071] 2) Add 1.0 g of p-aminobenzaldehyde and 1.0 g of glacial acetic acid to the dissolved 5% PVA solution and stir for 8 h to allow the aldehyde group to react with the hydroxyl group of PVA to undergo acetalization.
[0072] 3) After the reaction was completed, 0.7 g of dodecylsulfonyl chloride was added while stirring, and PVA-AbA was obtained after reacting for 3 h.
[0073] 4) The PVA-AbA solution was transferred to a brown / light-proof reaction vessel, and a certain amount of 100 ml of ethanol and 2.2 g of triethylamine were added. After heating to 100° C., 4.0 g of allyl glycidyl ether was added and stirred for 10 h to obtain the product PVA-AbA-Alsc-2.
[0074] 5) Clean the 0.4 micron PTFE microporous membrane with ethanol and dry it with hot air. Add 200 ml of methanol to a light-proof reaction vessel, and add the synthesized PVA-AbA-Alsc and cationic photoinitiator. Place the cleaned PTFE microporous membrane in a reaction vessel, degas for 30-60 minutes with the help of an ultrasonic and vacuum-assisted system, and then let it stand for 1-6 hours so that a layer of material containing polar groups is evenly coated on the PTFE. Take out the PTFE microporous membrane coated with PVA-AbA-Alsc from the reaction vessel, and after ultraviolet crosslinking for a period of time under ultraviolet light irradiation, a hydrophilic polytetrafluoroethylene microporous membrane is obtained. Example 3:
[0075] 1) Take 10 g of polyvinyl alcohol 1799 (alcoholysis degree 98% to 99%) and 90 ml of deionized water, heat and stir in a 95°C water bath to completely dissolve to obtain a 10% solution;
[0076] 2) Add 4.0 g of p-aminobenzaldehyde and 1.5 g of glacial acetic acid to the dissolved 5% PVA solution and stir for 8 h to allow the aldehyde group to react with the hydroxyl group of PVA to undergo acetalization.
[0077] 3) After the reaction was completed, 3.0 g of dodecylsulfonyl chloride was added while stirring, and PVA-AbA was obtained after 3 h.
[0078] 4) The PVA-AbA solution was transferred to a brown / light-proof reaction vessel, and a certain amount of 100 mL of ethanol and 2.2 g of triethylamine were added. After heating to 100° C., 4.0 g of allyl glycidyl ether was added and stirred for 10 h to obtain the product PVA-AbA-Alsc-3.
[0079] 5) Clean the 0.4 micron PTFE microporous membrane with ethanol and dry it with hot air. Add 200 ml of methanol to a light-proof reaction vessel, and add the synthesized PVA-AbA-Alsc and a cationic photoinitiator. Place the cleaned PTFE microporous membrane in a reaction vessel, degas for 30-60 minutes with the help of an ultrasonic and vacuum-assisted system, and then let it stand for 1-6 hours so that a layer of material containing polar groups is evenly coated on the PTFE. Take out the PTFE microporous membrane coated with PVA-AbA-Alsc from the reaction vessel, and after ultraviolet crosslinking for a period of time under ultraviolet light irradiation, a hydrophilic polytetrafluoroethylene microporous membrane is obtained.
[0080] Example 1-3, PVA-AbA-Alsc modified PTFE hydrophilicity test result table:
[0081]
[0082] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.
Claims
1. A method for hydrophilic modification of polytetrafluoroethylene microporous membrane, characterized in that: The steps include: Adding an alcohol solvent, a hydrophilic modification material and a photoinitiator into a light-proof reaction container to prepare a hydrophilic modification photosensitive solution, wherein the hydrophilic modification material includes a PVA solution, aminobenzaldehyde, glacial acetic acid, alkylsulfonyl chloride, and an epoxy material, wherein the glacial acetic acid causes the aldehyde group in the aminobenzaldehyde to react with the hydroxyl group of the PVA to undergo an acetal reaction and introduce an amino group and a benzene ring, the alkylsulfonyl chloride is used to introduce a hydrophobic segment into the PVA, and the epoxy group in the epoxy material reacts with the hydroxyl group of the PVA to undergo a ring-opening reaction to introduce a photosensitive group into the PVA; placing a PTFE microporous membrane in the hydrophilic modification photosensitive solution in the reaction container so that the PTFE microporous membrane is evenly coated with a layer of the material containing a polar group; The PTFE microporous membrane coated with the polar group-containing material is taken out from the reaction container, and is subjected to ultraviolet crosslinking under ultraviolet light irradiation to obtain a hydrophilic polytetrafluoroethylene microporous membrane.
2. The hydrophilic modification method of a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: The PVA solution is prepared by stirring and dissolving polyvinyl alcohol and deionized water in a heated water bath; and / or the concentration of the PVA solution is 3-8%.
3. The hydrophilic modification method of a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: The aminobenzaldehyde is: p-aminobenzaldehyde, o-phenylaminobenzaldehyde, m-phenylaminobenzaldehyde, p-acetylaminobenzaldehyde, 2,4-diaminobenzaldehyde, 2-amino-3,5-dibromobenzaldehyde, one or more thereof; and / or the alkylsulfonyl chloride is: pentanesulfonyl chloride, octanesulfonyl chloride, undecanesulfonyl chloride, dodecanesulfonyl chloride, pentadecanesulfonyl chloride, heptadecanylsulfonyl chloride, octadecanesulfonyl chloride, one or more thereof.
4. The hydrophilic modification method of a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: The preparation method of the hydrophilic modified material comprises the following steps: Adding aminobenzaldehyde to the PVA solution; Add glacial acetic acid and stir to allow the aldehyde group of aminobenzaldehyde to react with the hydroxyl group of PVA to form an acetal and introduce an amino group and a benzene ring; After the acetalization reaction is completed, alkylsulfonyl chloride is added and stirred to introduce hydrophobic segments into PVA to obtain a PVA-AbA solution; The PVA-AbA solution is transferred to a light-proof reaction container, and epoxy material is added to allow the epoxy group to undergo a ring-opening reaction with the hydroxyl group of PVA, thereby introducing a photosensitive group onto the PVA.
5. The hydrophilic modification method of a polytetrafluoroethylene microporous membrane according to claim 4, characterized in that: The epoxy material is one or more of 4-vinylbenzyl glycidyl ether, allyl glycidyl ether and glycidyl methacrylate.
6. The method for hydrophilic modification of a polytetrafluoroethylene microporous membrane according to claim 4, characterized in that: The PVA-AbA solution is transferred to a light-proof reaction container, and an alcohol solvent and triethylamine are added. After heating to a set temperature and stirring for a set time, the epoxy material is added and stirred for reaction.
7. The method for hydrophilic modification of a polytetrafluoroethylene microporous membrane according to claim 6, characterized in that: The alcohol solvent is one or at least two of methanol, ethanol, propanol and butanol.
8. The method for hydrophilic modification of a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: The PTFE microporous membrane is placed in the hydrophilic modified photosensitive solution in the reaction container, and after degassing for 30-60 minutes with the help of ultrasound and vacuum auxiliary system, it is allowed to stand for 1-6 hours, so that a layer of material containing polar groups is evenly coated on the PTFE.
9. A polytetrafluoroethylene microporous membrane, characterized in that: The hydrophilic modification method according to any one of claims 1 to 8 is used to obtain the hydrophilic modification product.
10. A water treatment device, characterized in that: The invention comprises the polytetrafluoroethylene microporous membrane as claimed in claim 9.