Preparation method of heterogeneous electro-Fenton system cathode catalytic material Fe3O4 (at) NOPC and application of heterogeneous electro-Fenton system cathode catalytic material Fe3O4 (at) NOPC in degradation of endocrine disrupter

By using Fe3O4@NOPC catalyst in heterogeneous electric Fenton system, the problems of limited pH application scope and iron sludge deposition in the prior art are solved, and efficient degradation of endocrine disturbances is achieved, especially without iron added In the case of the source, a degradation rate of 70% was achieved, which significantly improved the degradation efficiency and stability.

CN118976494APending Publication Date: 2024-11-19GUIZHOU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410640656.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing electrofenton system has problems with limited pH application scope and iron sludge deposition when degrading endocrine disturbances, making it difficult to effectively degrade contaminants such as phthalate.

Method used

Fe3O4@NOPC catalyst is used, which uses wine lees biomass charcoal as the base material and embeds Fe3O4 nanoparticles to form a porous structure and adjusts the Fe+ doping ratio. It is used to build a heterogeneous electric Fenton system to achieve endocrine interference Efficient degradation.

Benefits of technology

Without adding iron sources, Fe3O4@NOPC catalyst can efficiently degrade endocrine disruptors within a wide pH range, reaching a 70% degradation rate, and avoiding the generation of iron sludge, significantly improving degradation efficiency and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976494A_ABST
    Figure CN118976494A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a heterogeneous electro-Fenton system cathode catalytic material Fe3O4 (at) NOPC and application of the heterogeneous electro-Fenton system cathode catalytic material Fe3O4 (at) NOPC in degradation of endocrine disrupter, and the preparation method comprises the following steps: (1) weighing biomass porous carbon, adding deionized water, and carrying out ultrasonic treatment to obtain a solution A; (2) weighing FeCl3. 6H2O and FeSO4. 7H2O, and dissolving the FeCl3. 6H2O and the FeSO4. 7H2O in deionized water to obtain a solution B; (3) transferring the solution A into the solution B, adjusting the pH value by using a 5M NaOH solution, continuously stirring in a water bath kettle, repeatedly centrifuging the stirred solution, cleaning by using deionized water, and drying in a drying oven; and (4) finally putting the dried solid into a tubular furnace, introducing nitrogen into the tubular furnace, heating at a heating rate of 5 DEG C / min, and calcining to obtain the Fe3O4 (at) NOPC. The embedded Fe3O4 not only can provide iron ions for an electro-Fenton reaction, but also can form abundant functional groups and active sites on the surface of the biomass charcoal, so that the degradation efficiency is improved, and the degradation effect is good. And no iron sludge is generated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental functional materials and provides an application method of a Fe3O4@NOPC catalyst used in a heterogeneous electro-Fenton system to degrade endocrine disruptors. Background Art

[0002] Phthalates (PAEs) are endocrine disruptors, colorless, non-volatile and water-soluble synthetic organic compounds. PAEs can improve the strength, hardness, plasticity and durability of materials, so they are often widely used in various industrial production such as plastics, pesticides, cosmetics, etc. According to statistics from information processing services, the global annual consumption of PAEs exceeded 3.5 million tons in 2021. Because PAEs are non-polar molecules and are not covalently bound to the polymer molecules in plastics, they can easily migrate out of the product and be released directly or indirectly into various environments. For example, PAEs have been detected in soil, sediments, rivers, seawater and the atmosphere.

[0003] Dimethyl phthalate (DMP) is one of the most widely used phthalates in plastics and is also the most water-soluble of PAEs. Its hydrolysis half-life is more than 3 years and it is quite stable in aqueous solution. Therefore, DMP was selected as the target pollutant for research.

[0004] In recent years, renewable and low-cost biomass has been used as a carbon precursor, among which nitrogen-containing biomass has been endowed as an ideal precursor for nitrogen-rich porous carbon with excellent properties. Biomass carbon has a high degree of graphitization, porous structure and rich functional group characteristics, which effectively promotes electron transport and electrochemical action. A large amount of wine lees is produced in China every year. Wine lees itself is produced in the process of brewing. Its raw materials are mainly crops such as sorghum, with high starch and cellulose content, and a large amount of nutrients. The biomass carbon produced has a high specific surface area and good pore structure, and is rich in heteroatom doping. Therefore, wine lees is an ideal biomass carbon precursor.

[0005] As a traditional and efficient advanced oxidation technology, electro-Fenton technology can quickly degrade organic pollutants in sewage, but there are still many unresolved problems in the traditional electro-Fenton system, such as strict pH application range and iron sludge deposition. Therefore, it is hoped that these problems can be solved by constructing a heterogeneous electro-Fenton system. Summary of the invention

[0006] Purpose of the invention: In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a composite electrocatalyst that can degrade endocrine disruptors, has stable materials, and does not produce sludge or iron sludge. The method has a simple synthesis process, and the formed electrocatalyst has a rich pore structure and a large specific surface area. At the same time, it has good stability and is an application method of the Fe3O4@NOPC catalyst for degrading endocrine disruptors in a heterogeneous electro-Fenton system.

[0007] Technical solution: A method for preparing Fe3O4@NOPC, a cathode catalytic material of a heterogeneous electro-Fenton system, and its application in degrading endocrine disruptors, characterized in that it comprises the following steps:

[0008] (1) Weigh 200 mg of biomass porous carbon, add 50 ml of deionized water and ultrasonicate for 30 min to obtain solution A;

[0009] (2) Weigh FeCl3·6H2O and FeSO4·7H2O and dissolve them in 50 mL of deionized water to obtain solution B;

[0010] (3) Solution A was transferred into solution B and the pH was adjusted with 5 M NaOH solution. The mixture was kept in a water bath at 50° C. and stirred continuously. The stirred solution was repeatedly centrifuged, washed with deionized water, and then dried in an oven.

[0011] (4) Finally, the dried solid was placed in a tubular furnace, nitrogen was introduced into the tubular furnace for 30 min, and then the temperature was increased at a heating rate of 5 °C / min. After calcination, Fe3O4@NOPC was obtained.

[0012] Specifically, the preparation steps of biomass porous carbon (NOPC) in step (1) include:

[0013] ① Put the collected lees as a precursor into a blast drying oven and set the temperature to 90°C for drying;

[0014] ② After drying, use a cryogenic grinder to grind it into powder, then weigh KHCO3 and lees powder (mass ratio is 2:1) and grind and mix them evenly in an agate mortar, finally put them into an alumina crucible and put them into a tubular furnace for calcination.

[0015] The steps of tubular furnace calcination include:

[0016] i. After nitrogen was introduced into the tube furnace for 30 min, heating was started at a heating rate of 5°C / min;

[0017] ii. After the temperature is raised to 800°C, maintain the temperature for 2 hours, and continuously introduce nitrogen during the entire calcination and carbonization process.

[0018] iii After the tube furnace is cooled to room temperature, the biomass charcoal is taken out and ground evenly, and then the biomass charcoal is soaked in a 2 mol / L HCl solution for acid washing for 12 hours. Repeated centrifugation and washing with deionized water until the pH of the supernatant is neutral; finally, it is dried in a forced air drying oven at 80°C for 12 hours to obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

[0019] Specifically, in step (2), the amount of FeCl3·6H2O is 2 mmol, and the amount of FeSO4·7H2O is 1 mmol.

[0020] Specifically, in step (3), solution A and solution B are mixed and adjusted to pH=12, the temperature of the water bath is 50° C. and stirred for 6 hours, and then dried in an oven at a temperature of 80° C.

[0021] Specifically, in step (4), the Fe3O4@NOPC is prepared by adding FeCl3·6H2O and FeSO4·7H2O to solution A in a ratio of 2:1.

[0022] Specifically, after the temperature in step (4) is raised to 450° C., the temperature is maintained for 4 hours, and nitrogen is continuously introduced during the entire calcination process.

[0023] Beneficial effects:

[0024] The advantages of the present invention are:

[0025] The present invention uses distiller's grains waste as a biomass carbon source, carbonizes it at high temperature to make it into a biomass carbon base material, and then uses a simple hydrothermal and thermal reduction method to embed the prepared Fe3O4 nanoparticles into the distiller's grains biochar to adjust the Fe 3+ and Fe 2+ Fe3O4@NOPC is prepared by doping ratio, and the overall structure is porous. The pore structure of the material is a mesoporous structure, which can promote the transport of reactants and active substances.

[0026] (2) The Fe3O4 embedded in this method can not only provide iron ions for the electro-Fenton reaction, but also form abundant functional groups and active sites on the biochar surface, thus improving the degradation efficiency. In the absence of an external iron source, about 70% of the pollutants can be degraded within 5 h (-0.7 V, pH = 3 and 10 mg / L DMP, Fe3O4@NOPC(2) cathode), and no iron sludge is produced.

[0027] (3) After using EPR and limited experimental conditions to explore the degradation mechanism, it was found that in addition to the attack of ·OH on DMP, there were also partial electro-oxidation and adsorption effects during the entire degradation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a flow chart of the present invention;

[0029] Figure 2 The scanning electron microscope images of Fe3O4@NOPC (Y=1, 0.5 and 2) prepared by the present invention, the elemental mapping, TEM image and surface spectrum of Fe3O4@NOPC (2)

[0030] Figure 3 The Raman spectrum of Fe3O4@NOPC(Y) prepared by the present invention and the N2 adsorption-desorption isotherm and pore size distribution curve of Fe3O4@NOPC(2) (embedded);

[0031] Figure 4 is the Fourier transform infrared spectrum of Fe3O4@NOPC(2) prepared by the present invention;

[0032] Figure 5 The XPS full spectrum, C 1s spectrum, Fe 2p spectrum, N 1s spectrum, O 1s fine spectrum and XRD spectrum of Fe3O4@NOPC(2) prepared by the present invention are shown;

[0033] Figure 6 It is an electrochemical impedance spectroscopy (EIS) diagram of Fe3O4@NOPC(Y) prepared by the present invention;

[0034] Figure 7 This is a graph showing the degradation efficiency of Fe3O4@NOPC(Y) prepared by the present invention on dimethyl phthalate;

[0035] Figure 8 The TOC mineralization rate and iron ion leaching rate of Fe3O4@NOPC(Y) prepared by the present invention under different conditions. DETAILED DESCRIPTION

[0036] The specific implementation of the present invention will be further described below in conjunction with the accompanying drawings.

[0037] It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as there is no conflict between them.

[0038] The reagents used in the present invention, potassium bicarbonate, anhydrous sodium sulfate, ferrous sulfate heptahydrate, ferric chloride hexahydrate, sodium hydroxide and anhydrous ethanol are all purchased from Sinopharm Group; dimethyl phthalate is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; potassium titanium oxalate is purchased from Shanghai McLean Biochemical Technology Co., Ltd.; acetone, sulfuric acid and 37% hydrochloric acid are purchased from Chongqing Chuandong Chemical (Group) Co., Ltd.; 30% H2O2 is purchased from Chengdu Jinshan Chemical Reagent Co., Ltd.; acetonitrile is purchased from Anhui Tiandi High Purity Solvent Co., Ltd.; Nafion membrane solution and Nafion 117 membrane are purchased from Dupont Company of the United States; and carbon cloth is purchased from Shanghai Hesen Electric Co., Ltd.

[0039] The Fe3O4@NOPC preparation method provided by the present invention is characterized by comprising the following steps:

[0040] S1. The collected vinasse is first placed in a forced air drying oven as a precursor and dried at 90°C; after drying, it is ground into powder using a cryogenic grinder, and then KHCO3 and vinasse powder (mass ratio is 2:1) are weighed and ground and mixed evenly in an agate mortar, and finally loaded into an alumina crucible and placed in a tubular furnace for calcination.

[0041] According to the present invention, nitrogen is first introduced into the tubular furnace for 30 minutes and then heating is started at a heating rate of 5°C / min; after the temperature rises to 800°C, the temperature is kept constant for 2 hours, and nitrogen is continuously introduced during the entire calcination and carbonization process. After the tubular furnace is cooled to room temperature, the biomass charcoal is taken out and ground evenly, and then the biomass charcoal is soaked in a 2mol / L HCl solution for acid washing for 12 hours. Repeat centrifugation and washing with deionized water until the pH of the supernatant is neutral; finally, it is dried in a blast drying oven at 80°C for 12 hours to finally obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

[0042] S2. Transfer solution A into solution B to form a mixed solution.

[0043] First, 200 mg of the NOPC was weighed, and 50 mL of deionized water was added, followed by ultrasonication for 30 min to obtain solution A; 2 mmol of FeCl3·6H2O and 1 mmol of FeSO4·7H2O were weighed and dissolved in 50 mL of deionized water to obtain solution B.

[0044] According to the present invention, the pH of the mixed solution is adjusted to 12 using a 5M NaOH solution, and the mixture is stirred continuously for 6 hours at 50°C in a water bath. The stirred solution is centrifuged repeatedly and washed with deionized water and then placed in an oven at 80°C for drying. Finally, the dried solid is placed in a tubular furnace, and nitrogen is introduced into the tubular furnace for 30 minutes before heating at a heating rate of 5°C / min. After the temperature reaches 450°C, the temperature is maintained at a constant level for 4 hours, and nitrogen is continuously introduced during the entire calcination process. After calcination, the Fe3O4@NOPC(2) catalytic material is obtained (the numbers in brackets represent the ratio of the amount of FeCl3·6H2O to FeSO4·7H2O added to solution A).

[0045] The following examples will further illustrate the present invention.

[0046] Example 1

[0047] The collected lees were first placed in a forced air drying oven as a precursor and dried at 90°C; after drying, they were ground into powder using a freeze grinder, and then KHCO3 and lees powder (mass ratio of 2:1) were weighed and ground and mixed evenly in an agate mortar, and finally loaded into an alumina crucible and placed in a tubular furnace for calcination.

[0048] First, nitrogen was introduced into the tubular furnace for 30 minutes and then heating was started at a heating rate of 5°C / min; after the temperature rose to 800°C, the temperature was kept constant for 2 hours, and nitrogen was continuously introduced during the entire calcination and carbonization process. After the tubular furnace was cooled to room temperature, the biochar was taken out and ground evenly, and then the biochar was soaked in a 2mol / L HCl solution for acid washing for 12 hours. Repeated centrifugation and washing with deionized water until the pH of the supernatant was neutral; finally, it was dried in a blast drying oven at 80°C for 12 hours to obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

[0049] Weigh 200 mg of the NOPC, add 50 mL of deionized water and ultrasonicate for 30 min to obtain solution A; weigh 2 mmol of FeCl3·6H2O and 1 mmol of FeSO4·7H2O and dissolve them in 50 mL of deionized water to obtain solution B.

[0050] Solution A was transferred into solution B and the pH was adjusted to 12 using 5M NaOH solution. The mixture was stirred for 6 h at 50 °C in a water bath. The stirred solution was centrifuged repeatedly and washed with deionized water and then dried in an oven at 80 °C. The dried solid was finally placed in a tube furnace. After nitrogen was introduced into the tube furnace for 30 min, it was heated at a heating rate of 5 °C / min. After the temperature reached 450 °C, the temperature was kept constant for 4 h, and nitrogen was continuously introduced during the entire calcination process. After calcination, the Fe3O4@NOPC(2) catalytic material was obtained (the numbers in brackets represent the ratio of the amount of FeCl3·6H2O to FeSO4·7H2O added to solution A).

[0051] Application Example 1

[0052] In a single-chamber electrolytic cell with a volume of 150 mL, a three-electrode reaction system was used: a platinum sheet electrode (2 cm × 2 cm) was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and a platinum sheet clip and a carbon cloth (2 cm × 2 cm) modified with the Fe3O4@NOPC (2) catalytic material prepared in Example 1 formed a working electrode, forming a three-electrode system for electro-Fenton degradation performance test, wherein the pollutants were degraded under different conditions (pH, voltage, loading amount), and 10 mg / LDMP was completely dissolved in the solution. After the degradation electrolytic cell device was assembled, oxygen was continuously introduced into the solution for 30 min in advance, and the flow rate was controlled to 60 sccm to ensure that the dissolved oxygen in the solution reached saturation; during the test, the flow rate was adjusted to 30 sccm using a flow meter, and the speed of the stirrer was controlled to 450 rpm using a magnetic stirrer to ensure that the test process was not affected by the oxygen mass transfer rate. Samples were taken at predetermined time intervals, 2 mL each time, and filtered using a 0.22 μm filter membrane.

[0053] The reaction was tested using a constant voltage test with the test potential set at -0.7 V, and the test product was measured and analyzed using high performance liquid chromatography.

[0054] Example 2

[0055] In a single-chamber electrolytic cell with a volume of 150 mL, a three-electrode reaction system was used: a platinum sheet electrode (2 cm × 2 cm) was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and a platinum sheet clip and a carbon cloth (2 cm × 2 cm) modified with the Fe3O4@NOPC (2) catalytic material prepared in Example 1 formed a working electrode, forming a three-electrode system for electro-Fenton degradation performance test, wherein the pollutants were degraded under different conditions (pH, voltage, loading amount), and 10 mg / LDMP was completely dissolved in the solution. After the degradation electrolytic cell device was assembled, oxygen was continuously introduced into the solution for 30 min in advance, and the flow rate was controlled to 60 sccm to ensure that the dissolved oxygen in the solution reached saturation; during the test, the flow rate was adjusted to 30 sccm using a flow meter, and the speed of the stirrer was controlled to 450 rpm using a magnetic stirrer to ensure that the test process was not affected by the oxygen mass transfer rate. Samples were taken at predetermined time intervals, 2 mL each time, and filtered using a 0.22 μm filter membrane.

[0056] Experimental Example 2

[0057] The ability of Fe3O4@NOPC(2) heterogeneous electro-Fenton system to mineralize pollutants was further investigated, and TOC test was performed on the degraded DMP solution at a voltage of -0.7V and different pH environments. The reaction was tested with constant voltage, and samples were taken at predetermined time intervals, 2mL each time, and filtered using a 0.22μm filter membrane. The test was performed using a TOC meter and ICP-MS analysis.

[0058] Comparative Example 1

[0059] The collected lees were first placed in a forced air drying oven as a precursor and dried at 90°C; after drying, they were ground into powder using a freeze grinder, and then KHCO3 and lees powder (mass ratio of 2:1) were weighed and ground and mixed evenly in an agate mortar, and finally loaded into an alumina crucible and placed in a tubular furnace for calcination.

[0060] First, nitrogen was introduced into the tubular furnace for 30 minutes and then heating was started at a heating rate of 5°C / min; after the temperature reached 800°C, the temperature was kept constant for 2 hours, and nitrogen was continuously introduced during the entire calcination and carbonization process. After the tubular furnace was cooled to room temperature, the biochar was taken out and ground evenly, and then the biochar was soaked in a 2mol / L HCl solution for acid washing for 12 hours. Repeated centrifugation and washing with deionized water until the pH of the supernatant was neutral; finally, it was dried in a forced air drying oven at 80°C for 12 hours to obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

[0061] Weigh 200 mg of the NOPC, add 50 mL of deionized water and ultrasonicate for 30 min to obtain solution A; weigh 1 mmol of FeCl3·6H2O and 1 mmol of FeSO4·7H2O and dissolve them in 50 mL of deionized water to obtain solution B.

[0062] Solution A was transferred into solution B and the pH was adjusted to 12 using 5M NaOH solution. The mixture was stirred for 6 h at 50 °C in a water bath. The stirred solution was centrifuged repeatedly and washed with deionized water and then dried in an oven at 80 °C. The dried solid was finally placed in a tube furnace. After nitrogen was introduced into the tube furnace for 30 min, it was heated at a heating rate of 5 °C / min. After the temperature reached 450 °C, the temperature was kept constant for 4 h, and nitrogen was continuously introduced during the entire calcination process. After calcination, the Fe3O4@NOPC(1) catalytic material was obtained (the numbers in brackets represent the ratio of the amount of FeCl3·6H2O to FeSO4·7H2O added to solution A).

[0063] Application Comparative Example 1

[0064] In a single-chamber electrolytic cell with a volume of 150 mL, a three-electrode reaction system was used: a platinum sheet electrode (2 cm × 2 cm) was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and a platinum sheet clip and a carbon cloth (2 cm × 2 cm) modified with the Fe3O4@NOPC (2) catalytic material prepared in Example 2 formed a working electrode, forming a three-electrode system for electro-Fenton degradation performance test, wherein the electrolyte used a sodium sulfate solution with a pH of 3, and 10 mg / LDMP was completely dissolved in the solution. After the degradation electrolytic cell device was assembled, oxygen was continuously introduced into the solution for 30 min in advance, and the flow rate was controlled to 60 sccm to ensure that the dissolved oxygen in the solution reached saturation; during the test, the flow rate was adjusted to 30 sccm using a flow meter, and the speed of the stirrer was controlled to 450 rpm using a magnetic stirrer to ensure that the test process was not affected by the oxygen mass transfer rate. Samples were taken at predetermined time intervals, 2 mL each time, and filtered using a 0.22 μm filter membrane.

[0065] The reaction was tested using a constant voltage test with the test potential set at -0.7 V, and the test product was measured and analyzed using high performance liquid chromatography.

[0066] Comparative Example 2

[0067] The collected lees were first placed in a forced air drying oven as a precursor and dried at 90°C; after drying, they were ground into powder using a freeze grinder, and then KHCO3 and lees powder (mass ratio of 2:1) were weighed and ground and mixed evenly in an agate mortar, and finally loaded into an alumina crucible and placed in a tubular furnace for calcination.

[0068] First, nitrogen was introduced into the tubular furnace for 30 minutes and then heating was started at a heating rate of 5°C / min; after the temperature reached 800°C, the temperature was kept constant for 2 hours, and nitrogen was continuously introduced during the entire calcination and carbonization process. After the tubular furnace was cooled to room temperature, the biochar was taken out and ground evenly, and then the biochar was soaked in a 2mol / L HCl solution for acid washing for 12 hours. Repeated centrifugation and washing with deionized water until the pH of the supernatant was neutral; finally, it was dried in a forced air drying oven at 80°C for 12 hours to obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

[0069] Weigh 200 mg of the NOPC, add 50 mL of deionized water and ultrasonicate for 30 min to obtain solution A; weigh 0.5 mmol of FeCl3·6H2O and 1 mmol of FeSO4·7H2O and dissolve them in 50 mL of deionized water to obtain solution B.

[0070] Solution A was transferred into solution B and the pH was adjusted to 12 using 5M NaOH solution. The mixture was stirred for 6 hours at 50°C in a water bath. The stirred solution was centrifuged repeatedly and washed with deionized water and then dried in an oven at 80°C. Finally, the dried solid was placed in a tube furnace. After nitrogen was introduced into the tube furnace for 30 minutes, it was heated at a heating rate of 5°C / min. After the temperature reached 450°C, the temperature was kept constant for 4 hours, and nitrogen was continuously introduced during the entire calcination process. After calcination, Fe3O4@NOPC(0.5) catalytic material was obtained (the numbers in brackets represent the ratio of the amount of FeCl3·6H2O to FeSO4·7H2O added to solution A).

[0071] Application Comparative Example 2

[0072] In a single-chamber electrolytic cell with a volume of 150 mL, a three-electrode reaction system was used: a platinum sheet electrode (2 cm × 2 cm) was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and a platinum sheet clip and a carbon cloth (2 cm × 2 cm) modified with the Fe3O4@NOPC (2) catalytic material prepared in Example 3 formed a working electrode, forming a three-electrode system for electro-Fenton degradation performance test, wherein the electrolyte used a sodium sulfate solution with a pH of 3, and 10 mg / LDMP was completely dissolved in the solution. After the degradation electrolytic cell device was assembled, oxygen was continuously introduced into the solution for 30 min in advance, and the flow rate was controlled to 60 sccm to ensure that the dissolved oxygen in the solution reached saturation; during the test, the flow rate was adjusted to 30 sccm using a flow meter, and the speed of the stirring bar was controlled to 450 rpm using a magnetic stirrer to ensure that the test process was not affected by the oxygen mass transfer rate. Samples were taken at predetermined time intervals, 2 mL each time, and filtered using a 0.22 μm filter membrane.

[0073] The reaction was tested using constant voltage, and the test product was determined and analyzed using high performance liquid chromatography.

[0074] The structure and application analysis of the Fe3O4@NOPC(2) catalytic material prepared in the embodiment of the present invention:

[0075] See also Figure 2 , Figure 1 (ad) are scanning electron microscope images of Fe3O4@NOPC (Y = 1, 0.5 and 2) catalytic materials, (e) is the element mapping of Fe3O4@NOPC (2) catalytic materials, (f) is the TEM image of Fe3O4@NOPC (2) catalytic materials, and (g) is the surface spectrum of Fe3O4@NOPC (2) catalytic materials. It can be seen from the figure that Fe3O4@NOPC (Y) presents a porous structure as a whole, and there are many nanoparticles on the material uniformly embedded in the porous carbon surface. It is mainly composed of four elements, C, O, N and Fe, and is uniformly distributed in the material. The highest Fe doping content is 5.1wt%. The TEM image shows two types of crystal particle gaps, with lattice gap distances of 0.29nm and 0.48nm respectively. The above shows that iron oxide is successfully embedded in NOPC.

[0076] See also Figure 3 , Figure 2(a) is the Raman spectrum of Fe3O4@NOPC(Y) prepared by the present invention, and (b) is the N2 adsorption-desorption isotherm and pore size distribution curve (embedded) of Fe3O4@NOPC(2) prepared by Example 1 of the present invention. As can be seen from the figure, Fe3O4@NOPC(2) has more defects. The structural defects in the graphene lattice can serve as stable attachment points for capturing Fe species and promote the generation of metal center active sites. The pore structure of Fe3O4@NOPC(2) is a mesoporous structure. The specific surface area and pore volume are 437.9m 2 / g and 0.384cm 3 / g, and the pore diameter is mainly distributed in the range of 2-40nm.

[0077] See also Figure 4 , Figure 5 shows the Fourier transform infrared spectrum of Fe3O4@NOPC(2) prepared in Example 1 of the present invention. 563.16cm -1 The absorption peak at is due to the Fe-O stretching vibration on the surface of the iron oxide nanoparticles. The above peak observed in the spectrum indicates that the iron oxide has been successfully loaded on the biochar.

[0078] See also Figure 5 , Fe3O4@NOPC(2) mainly contains four elements: C, N, O, and Fe, which is consistent with the results of the elemental mapping spectrum. The figure shows that the Fe loaded on the surface of the material exists in a mixed valence state, and proves the existence of iron oxides; the diffraction characteristic peaks of Fe3O4 nanoparticles appear in all samples, which match well with the JCPDS card (19-0629) of the face-centered cubic lattice of Fe3O4 characteristic peaks. At the same time, all catalysts show strong interlayer (311) diffraction. XRD spectra prove that the iron oxide loaded on biochar is Fe3O4.

[0079] See also Figure 6 , electrochemical impedance spectroscopy (EIS) of Fe3O4@NOPC(Y). Figure 5 It can be seen that the charge transfer resistance of the catalytic materials prepared in Example 1, Comparative Example 2 and Comparative Example 3 of the present invention is relatively small, between 12-14Ω, indicating that these three catalytic materials can enable electrons to be transferred quickly during the reaction, so that Fe 3+ Rapid conversion to Fe 2+ , ensuring that the heterogeneous electro-Fenton reaction can continue; and in the low-frequency region of the Nyquist diagram, the slopes of the three straight lines are large, indicating that the diffusion resistance of the three is small, which is conducive to promoting the diffusion of substances (such as O2) in the electrochemical reaction.

[0080] See also Figure 7, Fe3O4@NOPC(Y) degradation efficiency diagram of pollutants. Different from the conventional electro-Fenton process, in the heterogeneous electro-Fenton reaction, there is no need to add Fe at the beginning of the reaction. 2+ , so it is necessary to load an appropriate proportion of Fe in the material 2+ with Fe 3+ , in order to 2+ While activating H2O2, it can also use the electrons transferred from the anode to the cathode to transfer Fe 3+ Reduction to Fe 2+ , to ensure that the reaction can proceed continuously. Therefore, three materials with different proportions of Fe3O4@NOPC(2), Fe3O4@NOPC(1) and Fe3O4@NOPC(0.5) were designed for degradation experiments. In sodium sulfate electrolyte with pH=3, platinum sheet was used as counter electrode and saturated calomel electrode was used as reference electrode, and 10mg / L DMP was degraded at a potential of -0.7V. From this, we can find that in the absence of an external iron source, under the conditions of Fe3O4@NOPC(2) loading, pH of 7, and voltage of -0.7V, the catalyst has the highest degradation efficiency for dimethyl phthalate.

[0081] See also Figure 8 The TOC mineralization rate and Fe ion leaching rate of Fe3O4@NOPC(Y) under different conditions are fully analyzed. It can be seen from the figure that Fe3O4@NOPC(2) has good pollutant removal ability and mineralization efficiency in a wide pH range. When the pH reaches 7, the TOC mineralization rate is as high as 50.5%, which corresponds to the degradation efficiency of pollutants. Moreover, under different conditions, the iron leaching rate is lower than the national water quality standard (0.1 mg / L).

[0082] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.

Claims

1. Heterogeneous electro-Fenton system cathode catalytic material Fe 3 O 4 @NOPC preparation method and its application in degrading endocrine disruptors, It is characterized in that The following steps are involved: (1) Weigh 200 mg of biomass porous carbon, add 50 ml of deionized water and ultrasonicate for 30 min to obtain solution A; (2) Weigh FeCl 3 6H 2 O and FeSO 4 7H 2 O was dissolved in 50 mL of deionized water to obtain solution B; (3) Solution A was transferred into solution B and the pH was adjusted with 5 M NaOH solution. The mixture was kept in a water bath at 50° C. and stirred continuously. The stirred solution was repeatedly centrifuged, washed with deionized water, and then dried in an oven. (4) Finally, the dried solid was placed in a tube furnace, nitrogen was introduced into the tube furnace for 30 min, and then the temperature was increased at a heating rate of 5 °C / min. After calcination, Fe 3 O 4 @NOPC.

2. The preparation method of the heterogeneous electro-Fenton system cathode catalytic material Fe3O4@NOPC according to claim 1 and its application in degrading endocrine disruptors, It is characterized in that Step (1) The preparation steps of the biomass porous carbon (NOPC) in step (1) include: ① Put the collected lees as a precursor into a blast drying oven and set the temperature to 90°C for drying; ② After drying, use a freeze grinder to grind it into powder, then weigh KHCO 3 The mixture was ground and mixed evenly with wine lees powder (mass ratio was 2:1) in an agate mortar, and finally loaded into an alumina crucible and placed in a tube furnace for calcination. The steps of tube furnace calcination include: i. After nitrogen was introduced into the tube furnace for 30 min, heating was started at a heating rate of 5°C / min; ii. After the temperature is raised to 800°C, maintain the temperature for 2 hours, and continuously introduce nitrogen during the entire calcination and carbonization process. iii After the tube furnace is cooled to room temperature, the biomass charcoal is taken out and ground evenly, and then the biomass charcoal is soaked in a 2 mol / L HCl solution for acid washing for 12 hours. Repeated centrifugation and washing with deionized water until the pH of the supernatant is neutral; finally, it is dried in a forced air drying oven at 80°C for 12 hours to obtain nitrogen-oxygen co-doped biomass porous carbon (NOPC).

3. The heterogeneous electro-Fenton system cathode catalytic material Fe according to claim 1 3 O 4 @NOPC preparation method and its application in degrading endocrine disruptors, It is characterized in that Step (2) FeCl 3 6H 2 O dosage is 2 mmol, FeSO 4 7H 2 The amount of O used is 1 mmol.

4. The heterogeneous electro-Fenton system cathode catalytic material Fe according to claim 1 3 O 4 @NOPC preparation method and its application in degrading endocrine disruptors, It is characterized in that In step (3), solution A and solution B are mixed and adjusted to pH = 12, the temperature of the water bath is 50° C. and stirred for 6 hours, and then dried in an oven at 80° C.

5. The heterogeneous electro-Fenton system cathode catalytic material Fe according to claim 1 3 O 4 @NOPC preparation method and its application in degrading endocrine disruptors, It is characterized in that Step (4) Fe 3 O 4 @NOPC is solution A with FeCl added 3 6H 2 O and FeSO 4 7H 2 The molar ratio of O substance is 2:

1.

6. The heterogeneous electro-Fenton system cathode catalytic material Fe according to claim 1 3 O 4 @NOPC preparation method and its application in degrading endocrine disruptors, It is characterized in that After the temperature in step (4) is raised to 450° C., the temperature is maintained for 4 hours, and nitrogen is continuously introduced during the entire calcination process.

Citation Information

Cited By

  • Carbon fiber loaded Fe3O4 composite material, preparation method and application thereof, and method for degrading organic pollutants by electro-Fenton oxidation

    CN120394010A

  • Preparation method of conductive biochar composite high-conductivity material

    CN121493962A