Optimized reverse release process of low-viscosity low-gram-weight die cutting assembly
By optimizing the hardness of the back glue and protective film, glue ratio and adjustment of die-cutting tools, the problem of C2/C4 angle of copper foil surface in the existing reverse release process is solved, and more efficient reverse release is achieved and heat dissipation effect avoids the risk of copper foil wrinkles and screen breakage.
Patent Information
- Application Number
- CN202411118480.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
AI Technical Summary
During the existing reverse release process, when the roller pressure of the cage assembly is changed for optimization, the C2/C4 angle reverse release phenomenon occurs on the copper foil surface, which cannot meet the batch control of reverse release, resulting in poor heat dissipation effect and Risk of broken screen.
By optimizing the hardness of the back glue and protective film on the copper foil surface, adjusting the glue ratio and the cut mark depth of the die-cutting tool, the grid film model and production pressure of the protective film are improved, and the adhesion between the copper foil and the protective film is ensured. and solid viscosity, control the amount of glue and the depth of the cut, and achieve more efficient reverse release.
It effectively avoids copper foil wrinkles, improves the accuracy of die-cutting, reduces the release risk caused by back glue, improves the release effect of product end angles, and ensures efficient heat dissipation performance.
Smart Images

Figure CN118977293A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of die-cutting reverse release, and in particular to an optimized reverse release process for a low-viscosity and low-grammage die-cutting component. Background Art
[0002] With the development of electronic technology and various social needs, mobile electronic products and high-end electronic products are increasingly widely used in various industries and households. With the popularization of 5G products, the performance of device function modules has been improved, the integration has increased, and the power consumption has increased significantly. Better thermal conductive devices are needed to meet the heat transfer requirements of high heat flux density. Heat dissipation has become a core factor restricting the development of high-end electronic devices. During the operation of the whole machine, the heat of the screen is transferred and dissipated through copper foil, steel sheet and graphite sheet. During the assembly process, due to the adhesive on the surface of the product, a protective film needs to be applied for protection. Therefore, there is a risk of the adhesive backing being reversed during the film tearing process, which can easily cause the copper foil to wrinkle. The screen will break during the assembly process and the heat dissipation effect will deteriorate.
[0003] In the existing reverse release process, the reverse release is optimized by changing the roller pressure of the mesh box assembly. After the protective film is assembled, the C2 / C4 angle reverse release phenomenon occurs on the copper foil surface, which cannot meet the batch control of the reverse release. Therefore, it does not meet the existing needs. In this regard, we propose an optimized reverse release process for low-viscosity and low-grammage die-cut components. Summary of the invention
[0004] The purpose of the present invention is to provide an optimized reverse release process for low-viscosity and low-grammage die-cut components, so as to solve the problems in the existing reverse release process proposed in the above background technology, in which the reverse release is optimized by changing the roller pressure of the mesh box assembly, and after the protective film is assembled, the C2 / C4 angle reverse release phenomenon occurs on the copper foil surface, and the batch control of the reverse release cannot be met.
[0005] To achieve the above object, the present invention provides the following technical solution: an optimized reverse release process for a low-viscosity and low-weight die-cut component, comprising the following steps: S1: Optimize the degree of wrinkles of the copper foil, specifically, provide a backing adhesive on the surface of the copper foil, and provide a protective film on the surface of the backing adhesive, so that the protective film is adjusted first during the die-cutting and reverse release process of the product, specifically, the hardness of the composite material constituting the protective film is increased, the degree of wrinkles caused by the protective film to the copper foil during reverse release is reduced, and the adhesion and solid adhesion between the copper foil and the protective film are changed; S2: Optimizing the glue ratio, and processing the glue on both sides of the back adhesive at the same time, specifically, the glue is formed by filtering, proportioning and stirring in sequence, and in the process of proportioning the glue ingredients, the proportion of the ingredients for preparing the glue is adjusted to achieve the effect of optimizing the viscosity of the glue and improving the peeling force, and the glue is stirred by a high-speed stirrer, and the stirring rate of the high-speed stirrer is not less than 18000rpm; S3: Adjust the depth of the knife mark. Specifically, when the protective film is used to assemble and protect the adhesive backing, the whole needs to be die-cut. The die-cutting tool perpendicular to the protective film is selected for die-cutting. Before die-cutting the copper foil and the protective film, the thickness of the pad knife foam used for bottom support during die-cutting is increased, and the sharpness of the die-cutting tool, that is, the tool life, is adjusted. The depth of the product knife mark is controlled during the die-cutting process, and the flow and interference of glue during the assembly process are reduced by maintaining the amount of overflow glue; S4: Adjust the mesh film model on the surface of the protective film to increase the dyne value of the product surface, reduce the product delamination caused by the presence of silicone after bonding, avoid the failure of the dyne pen caused by the transfer of silicone from the protective film, and adjust the weight of the incoming protective film; S5: Test the production pressure of the protective film. Specifically, the product is re-prepared after adjusting the production parameters. The prepared protective film assembly box needs to be verified. The anti-release verification effect of the protective film is carried out at different pressure values in the pressure range of 30KG to 75KG. When the protective film is between 30KG and 33KG in this pressure value range, the anti-release effect is significantly improved. Then the pressure range of 30KG to 33KG is applied to the production of the protective film, and the yield rate of the protective film is counted in real time during the anti-release process.
[0006] Preferably, the adhesive backing is arranged between the copper foil and the protective film, the copper foil and the protective film are connected by the adhesive backing, glue is filled between the two sides of the adhesive backing and the copper foil and the protective film, and the adhesive backing is bonded and fixed to the copper foil and the protective film.
[0007] Preferably, the glue ingredients in step S1 are prepared by mixing high-viscosity glue and low-viscosity glue, and the mixing ratio of the high-viscosity glue and the low-viscosity glue is adjusted from 4:6 to 2:8.
[0008] Preferably, in step S3, the thickness of the knife pad foam is adjusted from 10 mm to 15 mm, and the tool life is adjusted from 100K to 50K.
[0009] Preferably, in step S3, the amount of glue overflow does not exceed 0.2 mm, the depth of the knife mark does not exceed 0.009 mm, and the single cutting cycle of the die-cutting tool is 0.3S.
[0010] Preferably, a release agent is coated on a side of the protective film close to the back adhesive, and a lamination process is performed between the protective film and the release agent. The release agent is composed of polyethylene particles, and the melt index of the polyethylene particles is 7.
[0011] Preferably, the protective film is composed of a first base layer, a second base layer and two release layers, the first base layer and the second base layer are arranged between the two release layers, the first base layer is located on the upper end surface of the second base layer, the first base layer, the second base layer and the two release layers are all adhesively installed, and the first base layer, the second base layer and the two release layers are hot-pressed as a whole.
[0012] Preferably, a grid film is fixedly provided on a side of the protective film away from the back adhesive, and the grid film and the protective film are bonded together by heat pressing.
[0013] Preferably, the model of the grid membrane is adjusted from 10w to 2G-50C01, and a waterproof membrane is provided on the surface of the grid membrane.
[0014] Preferably, in step S4, the gram weight of the protective film material is adjusted from 6 to 10 gf / in to 8 to 12 gf / in.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention can effectively maintain the anti-release effect of the protective film and avoid wrinkles of the copper foil caused by the release of the backing glue by adjusting the ratio of glue, the thickness of the knife pad foam, the life of the die-cutting tool and the model of the protective film in sequence, and can control the amount of glue overflow, improve the accuracy of die-cutting, and avoid the release phenomenon of the product end corners. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A schematic diagram of the peeling force of the product of the present invention; Figure 2 It is a comparative schematic diagram before and after the glue ratio of the present invention is changed; Figure 3 It is a schematic diagram of the knife mark size of the die-cutting tool of the present invention; Figure 4 It is a schematic diagram of the force of the die-cutting tool of the present invention during cutting; Figure 5 It is a schematic diagram of the thin-size die-cutting tool after cutting of the present invention; Figure 6 It is a schematic diagram of the thick-size die-cutting tool after cutting of the present invention; Figure 7 It is a schematic diagram of the depth of the cutter marks of the die-cutting tool of the present invention; Figure 8 It is a comparative schematic diagram of the protective film of the present invention before and after the model is changed; Fig. 9This is a schematic diagram of adjusting the incoming weight of the protective film of the present invention; Fig.10 This is a schematic diagram of the end angle reverse separation of the product of the present invention; Fig.11 Schematic diagram of the reverse release of the protective film of the present invention at different pressure values; Fig.12 It is a schematic diagram of the reverse separation verification of the product of the present invention; Fig.13 It is a schematic diagram of reverse release verification of the end angle of the product of the present invention; Fig.14 The figure is a schematic diagram of the overall reverse separation optimization process of the present invention; Fig.15 It is a schematic flow diagram of the process operation steps of the present invention. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0018] See also Figures 1 to 15 , an embodiment provided by the present invention: an optimized reverse release process for a low-viscosity and low-weight die-cut component, comprising the following steps: S1: Optimize the degree of wrinkles of the copper foil, specifically, provide a backing adhesive on the surface of the copper foil, and provide a protective film on the surface of the backing adhesive, so that the protective film is adjusted first during the die-cutting and reverse release process of the product, specifically, the hardness of the composite material constituting the protective film is increased, the degree of wrinkles caused by the protective film to the copper foil during reverse release is reduced, and the adhesion and solid adhesion between the copper foil and the protective film are changed; S2: Optimizing the glue ratio, and processing the glue on both sides of the back adhesive at the same time, specifically, the glue is formed by filtering, proportioning and stirring in sequence, and in the process of proportioning the glue ingredients, the proportion of the ingredients for preparing the glue is adjusted to achieve the effect of optimizing the viscosity of the glue and improving the peeling force, and the glue is stirred by a high-speed stirrer, and the stirring rate of the high-speed stirrer is not less than 18000rpm; S3: Adjust the depth of the knife mark. Specifically, when the protective film is used to assemble and protect the adhesive backing, the whole needs to be die-cut. The die-cutting tool perpendicular to the protective film is selected for die-cutting. Before die-cutting the copper foil and the protective film, the thickness of the pad knife foam used for bottom support during die-cutting is increased, and the sharpness of the die-cutting tool, that is, the tool life, is adjusted. The depth of the product knife mark is controlled during the die-cutting process, and the flow and interference of glue during the assembly process are reduced by maintaining the amount of overflow glue; S4: Adjust the mesh film model on the surface of the protective film to increase the dyne value of the product surface, reduce the product delamination caused by the presence of silicone after bonding, avoid the failure of the dyne pen caused by the transfer of silicone from the protective film, and adjust the weight of the incoming protective film; S5: Test the production pressure of the protective film. Specifically, the product is re-prepared after adjusting the production parameters. The prepared protective film assembly box needs to be verified. The anti-release verification effect of the protective film is carried out at different pressure values in the pressure range of 30KG to 75KG. When the protective film is between 30KG and 33KG in this pressure value range, the anti-release effect is significantly improved. Then the pressure range of 30KG to 33KG is applied to the production of the protective film, and the yield rate of the protective film is counted in real time during the anti-release process.
[0019] See also Figure 1 and Figure 2 The adhesive backing is arranged between the copper foil and the protective film, the copper foil and the protective film are connected by the adhesive backing, the two sides of the adhesive backing and the space between the copper foil and the protective film are filled with glue, the adhesive backing and the copper foil and the protective film are bonded and fixed, the ingredients of the glue in step S1 are formed by mixing high-viscosity glue and low-viscosity glue, the mixing ratio of high-viscosity glue and low-viscosity glue is adjusted from 4:6 to 2:8, and changing the glue ratio can improve the situation where the product has low peeling force and initial adhesion.
[0020] See also Figure 3 and Figure 6 In step S3, the thickness of the knife pad foam is adjusted from 10mm to 15mm, the tool life is adjusted from 100K to 50K, the glue overflow does not exceed 0.2mm, the knife mark depth does not exceed 0.009mm, and the single cutting cycle of the die-cutting tool is 0.3S. By adjusting the glue overflow and knife mark depth at the copper foil position, the flow and interference of glue during the assembly process are reduced.
[0021] See also Figure 5 , a release agent is coated on the side of the protective film close to the adhesive backing, and a coating process is performed between the protective film and the release agent. The release agent is composed of polyethylene particles, and the melt index of the polyethylene particles is 7. A grid film is fixed on the side of the protective film away from the adhesive backing. The grid film and the protective film are laminated by hot pressing. The model of the grid film is adjusted from 10w to 2G-50C01. A waterproof film is provided on the surface of the grid film. By changing the model of the protective film, the problem of the failure of the dyne pen caused by the transfer of silicon from the protective film can be avoided; The protective film consists of a first base layer, a second base layer and two release layers. The first base layer and the second base layer are arranged between the two release layers. The first base layer is located on the upper end surface of the second base layer. The first base layer, the second base layer and the two release layers are all bonded and installed. The first base layer, the second base layer and the two release layers are hot-pressed as a whole.
[0022] See also Figure 8 and Fig. 9 In step S4, the gram weight of the incoming protective film is adjusted from 6-10 gf / in to 8-12 gf / in. By adjusting the gram weight of the incoming protective film, the effect of the release of the protective film on the back adhesive is reduced.
[0023] Instructions attached Fig.11 In order to verify the anti-release effect of the protective film in the pressure range of 30KG to 75KG, the yield rate of the anti-release of the protective film can be controlled at a higher level by verifying the protective film in turn under different pressure values.
[0024] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. An optimized reverse release process for low-viscosity and low-weight die-cut components, characterized in that: The steps include: S1: Optimize the degree of wrinkles of the copper foil, specifically, provide a backing adhesive on the surface of the copper foil, and provide a protective film on the surface of the backing adhesive, so that the protective film is adjusted first during the die-cutting and reverse release process of the product, specifically, the hardness of the composite material constituting the protective film is increased, the degree of wrinkles caused by the protective film to the copper foil during reverse release is reduced, and the adhesion and solid adhesion between the copper foil and the protective film are changed; S2: Optimizing the glue ratio, and processing the glue on both sides of the back adhesive at the same time, specifically, the glue is formed by filtering, proportioning and stirring in sequence, and in the process of proportioning the glue ingredients, the proportion of the ingredients for preparing the glue is adjusted to achieve the effect of optimizing the viscosity of the glue and improving the peeling force, and the glue is stirred by a high-speed stirrer, and the stirring rate of the high-speed stirrer is not less than 18000rpm; S3: Adjust the depth of the knife mark. Specifically, when the protective film is used to assemble and protect the adhesive backing, the whole needs to be die-cut. The die-cutting tool perpendicular to the protective film is selected for die-cutting. Before die-cutting the copper foil and the protective film, the thickness of the pad knife foam used for bottom support during die-cutting is increased, and the sharpness of the die-cutting tool, that is, the tool life, is adjusted. The depth of the product knife mark is controlled during the die-cutting process, and the flow and interference of glue during the assembly process are reduced by maintaining the amount of overflow glue; S4: Adjust the mesh film model on the surface of the protective film to increase the dyne value of the product surface, reduce the product delamination caused by the presence of silicone after bonding, avoid the failure of the dyne pen caused by the transfer of silicone from the protective film, and adjust the weight of the incoming protective film; S5: Test the production pressure of the protective film. Specifically, the product is re-prepared after adjusting the production parameters. The prepared protective film assembly box needs to be verified. The anti-release verification effect of the protective film is carried out at different pressure values in the pressure range of 30KG to 75KG. When the protective film is between 30KG and 33KG in this pressure value range, the anti-release effect is significantly improved. Then the pressure range of 30KG to 33KG is applied to the production of the protective film, and the yield rate of the protective film is counted in real time during the anti-release process.
2. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 1, characterized in that: The adhesive backing is arranged between the copper foil and the protective film, the copper foil and the protective film are connected by the adhesive backing, glue is filled between the two sides of the adhesive backing and the copper foil and the protective film, and the adhesive backing is bonded and fixed to the copper foil and the protective film.
3. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 1, characterized in that: In step S1, the glue ingredients are prepared by mixing high-viscosity glue and low-viscosity glue, and the mixing ratio of the high-viscosity glue and the low-viscosity glue is adjusted from 4:6 to 2:
8.
4. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 1, characterized in that: In step S3, the thickness of the knife pad foam is adjusted from 10 mm to 15 mm, and the tool life is adjusted from 100K to 50K.
5. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 1, characterized in that: In step S3, the amount of glue overflow does not exceed 0.2 mm, the depth of the knife mark does not exceed 0.009 mm, and the single cutting cycle of the die-cutting tool is 0.3S.
6. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 2, characterized in that: A release agent is coated on the side of the protective film close to the back adhesive, and a lamination process is performed between the protective film and the release agent. The release agent is composed of polyethylene particles, and the melting index of the polyethylene particles is 7.
7. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 2, characterized in that: The protective film is composed of a first base layer, a second base layer and two release layers, the first base layer and the second base layer are arranged between the two release layers, the first base layer is located on the upper end surface of the second base layer, the first base layer, the second base layer and the two release layers are all bonded and installed, and the first base layer, the second base layer and the two release layers are integrally hot-pressed.
8. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 2, characterized in that: A grid film is fixedly arranged on one side of the protective film away from the back adhesive, and the grid film and the protective film are bonded together by heat pressing.
9. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 8, characterized in that: The model of the grid membrane is adjusted from 10w to 2G-50C01, and a waterproof membrane is provided on the surface of the grid membrane.
10. The optimized reverse release process of a low-viscosity and low-weight die-cut component according to claim 1, characterized in that: In step S4, the gram weight of the protective film material is adjusted from 6-10 gf / in to 8-12 gf / in.