Manufacturing process suitable for trunk guide of self-elevating platform ship
By adopting web construction method and optimizing welding process in the production of the self-lifting platform circumference well guide, the welding deformation and accuracy problems are solved, safety and efficiency are improved, and efficient guidance prefabrication and on-site construction are achieved.
Patent Information
- Application Number
- CN202411150494.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
During the production process of the jack-up platform, the welding quality and accuracy requirements are high, and it is easy to cause welding deformation, resulting in safety risks and difficult production, which is difficult to effectively solve the existing technology.
Prefabricated guidance is adopted using web as the tire construction method, select the appropriate tooling and welding sequence, predict and add the reverse deformation amount, cancel the angular deformation horse plate, use a fillet welding machine for efficient welding, and optimize the welding steps to meet the accuracy Require and improve safety.
The safety improvement and accuracy pass rate during the guided production process are achieved, the deformation and rework of welding heat input is reduced, the production cost is reduced, and the efficiency of on-site construction is improved.
Smart Images

Figure CN118977822A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of self-elevating platform ships, and in particular to a manufacturing process suitable for guiding a well enclosure of a self-elevating platform ship. Background Art
[0002] The jack-up platform ship has 4 enclosures, and each enclosure has 3 groups of guides. The guide is a guiding device for the pile leg during the lifting process. Due to its thick plate, dense structure, large welding volume, easy welding deformation, and high precision requirements, the control of weld quality, precision error and safety risks during its production process also faces new challenges. As a special area control part, the production of the enclosure area guide has high welding quality and precision requirements, and is difficult to produce. In the design stage, the requirements of all parties are taken into account, and the structural form, plate thickness, and welding form of the guide prefabrication are optimized to meet the design requirements while facilitating on-site production as much as possible. Therefore, formulating a process plan for the prefabrication of the guide structure becomes a prerequisite for safe and reliable operations and meeting precision and quality requirements. Therefore, it is very important to solve this problem. Summary of the invention
[0003] In view of this, the purpose of the present invention is to propose a manufacturing process suitable for the guide of the well of a self-elevating platform ship, so as to solve the problems raised in the above-mentioned background technology.
[0004] Based on the above purpose, the present invention provides a manufacturing process suitable for a guide for a self-elevating platform ship enclosure well, comprising the following steps: Step 1, selection of the tread: use the construction method of using the belly plate as the tread, i.e. lying construction, to prefabricate the guide; Step 2, selection of guide tooling: tooling is made according to the structural form, welding amount and prediction of welding deformation. Two long rows of FB250*30mm are installed on the panel. The long row is symmetrically welded on both sides, with a welding length of 50mm. The welding position is aligned with the small rib plate. A short row of FB250*20mm is installed between the two long rows. The double-sided symmetrical intermittent welding is 50mm long. A short row is added every other small rib plate, and the anti-angle deformation plate is removed. Step three, welding and installation of guide production: Step 1, welding between guide panel, web and large rib plate; Step 2, correction of welding deformation and increase of reverse angle deformation between panel and web; Step 3, welding and installation of small rib plates on the left and right sides; Step 4, inspection of straightness and verticality of panel and web according to the schematic diagram of guide production accuracy measurement points.
[0005] Preferably, the addition of the anti-deformation amount is performed by predictive guidance before step three: considering the deformation position and deformation amount, there are mainly two positions for adding the anti-deformation, the first is the sagging deformation when the panel and the web are welded; the second is the angular deformation when the narrow side of the panel exists; Preferably, when the face plate and the web are welded, a 2-3 mm vertical anti-deformation is placed in the middle of the face plate, and a 2 mm anti-angle deformation is placed on the narrow side of the face plate.
[0006] Preferably, an analysis is performed before the guide is made to determine the welding sequence: the tack welding position between the panel webs is selected, the tack welding is performed on the wide side of the panel, i.e., the large rib plate side, the web groove on the narrow side of the panel is welded first, the web groove on the wide side is carbon planed, and the wide side welding amount is large; in the large rib plate welding stage, the large rib plate is welded and then the formed web and panel are welded, at which time the large rib plate can play the role of reverse angle deformation reinforcement on the wide side of the panel.
[0007] Preferably, the first step of step 4 is specifically as follows: assemble the guide panel, the web and the left large rib plate, without installing the small rib plate, and add the anti-deformation when assembling the panel and the web; when assembling, position weld the panel and the web on one side of the large rib plate, i.e., the wide side of the panel; install the angle steel diagonal braces, the long row on the panel and the web, and the short row on the panel; first complete the welding of the large rib plate in sequence, turn over and weld 2 / 3 of the depth of the right side groove of the panel and the web in sequence from the middle to both sides, turn over 180° and carbon planer and complete the welding of 2 / 3 of the depth of the left side groove in sequence, and weld the left and right sides alternately in sequence until the welding of the panel and the web is completed.
[0008] Preferably, the second step of step four is specifically as follows: after the welds at the corner joints of the panel and the web are inspected and qualified, the long and short rows on the panel are removed, the deformation of the panel is corrected, and a 2mm reverse angle deformation is added to the narrow side of the panel, and then the small rib plate on the right is assembled.
[0009] Preferably, the third step of step 4 is specifically as follows: assemble and weld the small rib plate on the left side, first weld the flat fillet weld, then weld the vertical fillet weld, and weld two small rib plates in the middle to 2 / 3 of the groove depth; after the remaining small rib plates on the left side are welded to 2 / 3 of the groove depth, turn over 180°, and weld the small rib plates on the right side to 2 / 3 of the groove depth in the same order. Then turn over 180° to weld the remaining groove on the left side, and finally turn over 180° to weld the remaining groove on the right side.
[0010] Preferably, when welding the small ribs, the secondary auxiliary structures of the guide are welded incidentally to reduce the number of times the guide is turned over.
[0011] The beneficial effects of the present invention are as follows: the present invention adopts a construction method of lying down with the belly plate as the tire to prefabricate the guide, so that the tread surface is increased and the risk of tipping during the guide manufacturing process is reduced to zero; the deformation of the panel can be monitored in all directions; and the amount of anti-deformation can be added conveniently.
[0012] The selection of the guide manufacturing tooling of the present invention adopts the method of adding a short row of small rib plates for each other. Due to the double-sided alternating welding, the deformation caused by welding heat input is greatly reduced; the anti-angular deformation plate is eliminated, because the large rib plate is welded first, and the face plate and the web are formed and welded later; the use of short rows and anti-angular deformation plate tooling is greatly reduced; after the anti-angular deformation plate is eliminated, it is convenient to use a fillet welding machine instead of manual dioxygen welding for efficient welding.
[0013] Before the guide manufacturing and welding of the present invention, the addition of the guide manufacturing reverse deformation is predicted: when the panel and the web are welded, a 2-3mm vertical reverse deformation is placed in the middle of the panel, so that the one-time qualified rate of the straightness of the panel after the panel and the web are welded and formed is 100%; a 2mm reverse angle deformation is placed on the narrow side of the panel, so that the one-time qualified rate of the verticality of the panel is 90% after the small rib plate on the narrow side of the panel is welded.
[0014] The guide production of the present invention is analyzed before welding, and the positioning welding is carried out on the wide side of the panel, that is, the side of the large rib plate. The web groove on the narrow side of the panel is welded first, and the web groove on the wide side is carbon planed. The wide side welding amount is large, and the large rib plate is welded and then welded to form the web and panel. In this way, large angular deformation caused by the large narrow side welding amount of the panel is avoided. After the panel and the web are welded, the one-time pass rate of the verticality of the panel is 90%, and the amount of pyrotechnic correction and welding rework is reduced by 80%. The large rib plate is first welded and then formed into a whole with the long row and the short row, which increases the rigidity of the panel and reduces the angular deformation area of the panel by 80%.
[0015] The welding and assembling of the guide production of the present invention firstly performs welding between the guide panel, the web and the large rib plate, then performs welding deformation correction and reverse angle deformation addition on the panel and the web, then performs welding and assembling of the left and right small rib plates, and finally detects the straightness and verticality of the panel and the web according to the schematic diagram of guide production precision measurement points. In this way, the welding and assembling steps are optimized and the reverse deformation is added, so that the guide prefabrication meets the precision requirements, and at the same time, the safety of on-site construction is greatly improved, and finally cost reduction and efficiency improvement are achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 is a flow chart of a specific embodiment of the present invention; Figure 2 It is a schematic diagram of the selection of the manufacturing tooling guided by the specific embodiment of the present invention; Figure 3It is a schematic diagram of adding and releasing the vertical deformation amount in a specific implementation manner of the present invention; Figure 4 It is a schematic diagram of the addition and release of the reverse angle deformation of the narrow side of the panel according to a specific embodiment of the present invention; Figure 5 It is a schematic diagram of the selection of the tack welding position between the webs of the panels for the analysis of the manufacturing and welding sequence according to the specific implementation mode of the present invention; Figure 6 It is a schematic diagram of the welding stage of the large rib plate guided by the analysis of the welding sequence for the specific implementation method of the present invention; Figure 7 It is a schematic diagram of welding between the guide panel, web plate and large rib plate manufactured and welded according to a specific embodiment of the present invention; Figure 8 It is a schematic diagram of the welding of left and right small rib plates guided by a specific implementation method of the present invention. DETAILED DESCRIPTION
[0018] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0019] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0020] like Figure 1 As shown, this embodiment provides a manufacturing process suitable for a self-elevating platform ship enclosure guide, comprising the following steps: S1. Choice of tread surface: prefabricate the guide by using the belly plate as the tread, that is, lying construction; prefabricate the guide by using the belly plate as the tread, that is, lying construction, so that the tread surface is increased and the risk of tipping during the guide production process is reduced to zero; the deformation of the panel can be monitored in all directions; and it is convenient to add or release the anti-deformation amount.
[0021] S2, selection of guide tooling: Figure 2 As shown, The tooling is made according to the structural form, welding amount and the prediction of welding deformation. Two long rows of FB250*30mm are installed on the panel. The long row is symmetrically welded on both sides, with a welding length of 50mm. The welding position is aligned with the small rib plate. A short row of FB250*20mm is installed between the two long rows. The two-sided symmetrical intermittent welding is 50mm. A short row is added every other small rib plate, and the anti-angle deformation plate is cancelled. The short row is added every other small rib plate. Due to the double-sided alternating welding, the deformation caused by welding heat input is greatly reduced; the anti-angle deformation plate is cancelled, because the large rib plate is welded first, and the panel and the web are formed and welded later; the use of short rows and anti-angle deformation plate tooling is greatly reduced; after the anti-angle deformation plate is cancelled, it is convenient to use a fillet welder instead of manual dioxygen welding for efficient welding.
[0022] S3, perform prediction-guided production and add / drop reverse deformation: Considering the deformation position and deformation amount, there are two main locations for the addition of anti-deformation. The first is the sagging deformation caused by the welding of the panel and the web; the second is the angular deformation caused by the narrow side of the panel. Figure 3 As shown in the figure, when the panel and the web are welded, a 2~3mm vertical anti-deformation is placed in the middle of the panel. In this way, the straightness of the panel will be 100% qualified at one time after the panel and the web are welded. Figure 4 As shown in the figure, a 2mm reverse angle deformation is placed on the narrow side of the panel. In this way, after the small ribs on the narrow side of the panel are welded, the one-time pass rate of the verticality of the panel is 90%.
[0023] S4, guide production and welding sequence analysis: like Figure 5 As shown in the figure, the tack welding position between the panel webs is selected. The tack welding is done on the wide side of the panel, i.e. the side of the large rib plate. The web groove on the narrow side of the panel is welded first, and the web groove on the wide side is carbon planed. The wide side has a large amount of welding. Figure 6 As shown in the figure, during the welding stage of the large rib plate, the web plate and the face plate are welded after the large rib plate is welded. At this time, the large rib plate can play the role of strengthening the reverse angle deformation on the wide side of the face plate. This avoids large angle deformation caused by large welding of the narrow side of the face plate. After the face plate and the web plate are welded, the one-time pass rate of the verticality of the face plate is 90%, and the amount of pyrotechnic correction and welding rework is reduced by 80%. The large rib plate is welded first and then formed into a whole with the long and short rows, which increases the rigidity of the face plate and reduces the angle deformation area of the face plate by 80%.
[0024] S5, welding of guide production: S51, such as Figure 7As shown, the welding between the guide panel, web and large rib plate: assemble the guide panel, web and the large rib plate on the left, without installing the small rib plate, and add the anti-deformation when assembling the panel and web; when assembling, position weld the panel and web on one side of the large rib plate, i.e., the wide side of the panel; install the angle steel diagonal brace, the long row on the panel and web, and the short row on the panel; first complete the welding of the large rib plate in sequence, turn over and weld 2 / 3 of the depth of the right side groove of the panel and web in sequence from the middle to both sides, turn over 180° and complete the welding of 2 / 3 of the depth of the left side groove in sequence, and weld the left and right sides alternately in sequence until the welding of the panel and web is completed.
[0025] S52, correction of welding deformation of panel and web and addition of reverse angle deformation: after the welds of the corner joints of the panel and web are qualified through flaw detection, the long and short rows on the panel are removed, the deformation of the panel is corrected, and a reverse angle deformation of 2mm is added to the narrow side of the panel, and then the small rib plate on the right is assembled.
[0026] S53, such as Figure 8 As shown, the welding of the small ribs on the left and right sides: when welding the small ribs on the left, first weld the flat fillet weld, then weld the vertical fillet weld, and weld two small ribs in between to 2 / 3 of the groove depth; after the remaining small ribs on the left are welded to 2 / 3 of the groove depth, turn over 180°, and weld the small ribs on the right to 2 / 3 of the groove depth in the same order, then turn over 180° to weld the remaining groove on the left, and finally turn over 180° to weld the remaining groove on the right; when welding the small ribs, the secondary auxiliary structures of the guide are welded to reduce the number of times the guide is turned over.
[0027] S54, according to the guide manufacturing accuracy measurement point diagram, the straightness and verticality of the face plate and the web are tested.
[0028] By optimizing the welding steps and increasing the amount of reverse deformation, the guide prefabrication not only meets the precision requirements, but also greatly improves the safety of on-site construction, ultimately achieving cost reduction and efficiency improvement.
[0029] It should be understood by those skilled in the art that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments may also be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included in the scope of protection of the present invention.
Claims
1. A manufacturing process suitable for the guide of a self-elevating platform ship enclosure well, characterized in that: The following steps are included: Step 1, selection of the tread: use the construction method of using the belly plate as the tread, i.e. lying construction, to prefabricate the guide; Step 2, selection of guide tooling: tooling is made according to the structural form, welding amount and prediction of welding deformation. Two long rows of FB250*30mm are installed on the panel. The long row is symmetrically welded on both sides, with a welding length of 50mm. The welding position is aligned with the small rib plate. A short row of FB250*20mm is installed between the two long rows. The double-sided symmetrical intermittent welding is 50mm long. A short row is added every other small rib plate, and the anti-angle deformation plate is removed. Step three, welding and installation of guide production: Step 1, welding between guide panel, web and large rib plate; Step 2, correction of welding deformation and increase of reverse angle deformation between panel and web; Step 3, welding and installation of small rib plates on the left and right sides; Step 4, inspection of straightness and verticality of panel and web according to the schematic diagram of guide production accuracy measurement points.
2. According to claim 1, a manufacturing process suitable for the guide of the self-elevating platform ship enclosure well, characterized in that: Before step three, predictive guidance is performed to add and release the anti-deformation amount: considering the deformation position and deformation amount, there are mainly two locations for adding and releasing the anti-deformation. The first is the sagging deformation caused by the welding of the panel and the web; the second is the angular deformation caused by the narrow edge of the panel.
3. According to claim 2, a manufacturing process suitable for the guide of the self-elevating platform ship enclosure well, characterized in that: When welding the panel and the web, allow 2~3mm of vertical deformation in the middle of the panel and 2mm of angle deformation on the narrow side of the panel.
4. A manufacturing process suitable for the guide of a self-elevating platform ship enclosure according to claim 3, characterized in that: Before the guide is made and the welding sequence is determined, an analysis is performed: the tack welding position between the webs of the panels is selected, the tack welding is done on the wide side of the panel, i.e., the side of the large rib plate, the web groove on the narrow side of the panel is welded first, and the web groove on the wide side is carbon planed, and the wide side welding amount is large; in the large rib plate welding stage, the large rib plate is welded and then the formed web and panel are welded, at this time the large rib plate can play the role of reverse angle deformation reinforcement on the wide side of the panel.
5. A manufacturing process suitable for guiding the well of a self-elevating platform according to claim 4, characterized in that: The first step of step 4 is specifically as follows: assemble the guide panel, the web and the left large rib plate, the small rib plate is not installed, and the anti-deformation is added when the panel and the web are assembled; when assembling, the panel and the web are tack welded on one side of the large rib plate, i.e., the wide side of the panel; install the angle steel braces, the long rows on the panel and the web, and the short rows on the panel; first complete the welding of the large rib plate in sequence, turn over and weld 2 / 3 of the depth of the right side groove of the panel and the web in sequence from the middle to both sides, turn over 180° and carbon planer and complete the welding of 2 / 3 of the depth of the left side groove in sequence, and weld the left and right sides alternately in sequence until the welding of the panel and the web is completed.
6. A manufacturing process suitable for the guide of a self-elevating platform ship enclosure according to claim 5, characterized in that: The second step of step 4 is specifically as follows: after the welds at the corner joints of the panel and the web are inspected and qualified, the long and short rows on the panel are removed, the deformation of the panel is corrected, and a 2mm reverse angle deformation is added to the narrow side of the panel, and then the small rib plate on the right is assembled.
7. A manufacturing process suitable for guiding the well of a self-elevating platform according to claim 6, characterized in that: The third step of step 4 is specifically as follows: assemble and weld the small rib plate on the left side, first weld the flat fillet weld, then weld the vertical fillet weld, and weld two small rib plates in the middle to 2 / 3 of the groove depth; after the remaining small rib plates on the left side are welded to 2 / 3 of the groove depth, turn over 180°, and weld the small rib plates on the right side to 2 / 3 of the groove depth in the same order. Then turn over 180° to weld the remaining groove on the left side, and finally turn over 180° to weld the remaining groove on the right side.
8. A manufacturing process suitable for guiding the well of a self-elevating platform according to claim 7, characterized in that: When welding small ribs, the secondary auxiliary structures of the guide are welded incidentally to reduce the number of times the guide is turned over.
Citation Information
Cited By
Assembling method for cross-shaped lifting foundation sheet body of self-elevating platform
CN120587739A