Preparation method and application of sulfur-loaded material, positive electrode material, positive electrode and lithium-sulfur battery

By using carbon and biomass sugars to prepare porous carbon sphere materials and combining them with metal salts and nitrogen sources to form a carbon sphere carrier loaded with single atoms, the polysulfide shuttle effect and redox reaction kinetics in lithium-sulfur batteries are solved. The problem of the electrochemical performance and cyclic stability significantly improves the electrochemical performance and cyclic stability.

CN118978131APending Publication Date: 2024-11-19HUAZHONG AGRI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411431610.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the charging and discharging process, lithium-sulfur batteries have poor electrochemical performance due to the shuttle effect of long-chain polysulfur ions and poor redox reaction kinetics, and the insulating properties and volume changes of sulfur affect their commercial development.

Method used

Using carbon and biomass sugars as carbon sources, porous carbon ball materials are prepared by spray drying, and stirred with metal salt and nitrogen sources to form a carbon ball carrier material with metal single atoms loaded, used for the positive electrode of lithium sulfur battery, and strengthened Electron transport capability and active sites to reduce polysulfide shuttle.

Benefits of technology

It improves the electrochemical performance of lithium-sulfur batteries, enhances the contact area between the electrode and the electrolyte, reduces the polarization of the battery, and significantly improves the cycle stability and charge and discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978131A_ABST
    Figure CN118978131A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium-sulfur batteries, in particular to a preparation method and application of a sulfur-loaded material, a positive electrode material, a positive electrode and a lithium-sulfur battery. The method comprises the following steps: drying and sintering mixed slurry containing a first carbon source and a second carbon source to obtain a dry material, mixing the dry material with a solution containing a metal source and a nitrogen source, drying and sintering to obtain the sulfur-loaded material, and sequentially preparing a positive electrode material, a positive electrode and a lithium-sulfur battery from the sulfur-loaded material. The preparation process is simple, good in repeatability, low in cost, environment-friendly, high in controllability and easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium-sulfur batteries, and in particular to a preparation method and application of a sulfur-carrying material, a positive electrode material, a positive electrode and a lithium-sulfur battery. Background Art

[0002] In the electrochemical energy storage system, metal sulfur-based secondary batteries (sodium sulfur batteries, potassium sulfur batteries, etc.) represented by lithium sulfur batteries have attracted much attention due to their high theoretical capacity, high energy density and low sulfur raw material cost. However, during the charging and discharging process, the shuttle effect of long-chain polysulfide ions and poor redox reaction kinetics have hindered the commercial development of lithium sulfur batteries. Taking lithium sulfur batteries as an example, the insulating properties of sulfur and its final discharge products (Li2S / Li2S2) lead to low utilization of active materials. The volume changes severely during the cycle (about 80%), resulting in poor cycle stability. In addition, the so-called shuttle effect caused by soluble polysulfides (LiPs) has always been considered its main bottleneck.

[0003] In order to solve the problems of poor conductivity, volume expansion, and polysulfide shuttling in lithium-sulfur batteries, the current methods are mainly to encapsulate the positive electrode sulfur in a porous carbon matrix material matrix that has good electronic and ionic conductivity and limits the diffusion of polysulfides, such as porous carbon, carbon nanotubes and other materials, or to introduce polar electrode materials that have mutual chemical forces with polysulfides, and reduce the shuttling of polysulfides through surface adsorption and other forces, such as heteroatom-doped carbon, oxides and other materials. However, the strategy of using porous materials for "physical confinement" or polar groups for "chemical adsorption" can only improve the electrochemical performance of lithium-sulfur batteries to a certain extent, and cannot fundamentally improve the conversion efficiency of lithium-sulfur battery reactions. Summary of the invention

[0004] In view of this, the present invention provides a sulfur-carrying material for a lithium-sulfur battery positive electrode, a preparation method and an application thereof, to solve one of the above technical problems.

[0005] In a first aspect, one of the purposes of the present invention is to provide a method for preparing a sulfur-carrying material. The sulfur-carrying material is used to load sulfur to make a positive electrode of a lithium-sulfur battery. The preparation method comprises: subjecting a mixed slurry containing a first carbon source and a second carbon source to a first drying and a first sintering in sequence to obtain a dry material; and mixing the dry material into a solution containing a metal source and a nitrogen source, and subjecting the mixed slurry to a second drying and a second sintering in sequence to obtain the sulfur-carrying material.

[0006] Optionally, the first carbon source is selected from conductive carbon black, and the second carbon source is selected from one of sugar alcohol, glucose and sucrose.

[0007] Optionally, the mass ratio of the first carbon source to the second carbon source in the mixed slurry is (4-7): (3-6). Optionally, the mass ratio of the first carbon source to the second carbon source in the mixed slurry is 3:7, 4:6, 5:5, 6:4 or 7:3.

[0008] Optionally, the first drying is spray drying. The conditions of the spray drying include: spray drying at 80-150°C, collecting the spray drying crude product; the slurry flow rate entering the spray system is 10-30mL / min, the atomization pressure is 5-15MPa, and the gas flow rate is ≤10L / min.

[0009] Optionally, the first sintering conditions include: a sintering temperature of 800-1200°C, and a sintering time of 3-5 hours. Specifically, the first sintering temperature is 1200°C, 1000°C, 800°C or 600°C.

[0010] Optionally, the metal source is selected from one of acetate, nitrate and chlorate containing metals Fe, Co, Ni, Zn and Cu. The nitrogen source is 1,10-phenanthroline and / or dimethylimidazole.

[0011] Optionally, the mass ratio of the metal source to the nitrogen source is 1:(1~3).

[0012] Optionally, the dry material is mixed into the solution containing the metal source and the nitrogen source in a mass ratio of 1:(0.1~0.5).

[0013] Optionally, the first sintering atmosphere is selected from one of nitrogen and argon, and the second sintering atmosphere is selected from one of nitrogen and argon.

[0014] Optionally, the second sintering conditions include: a sintering temperature of 500-1000° C. and a sintering time of 3-6 hours.

[0015] Optionally, the second drying conditions include: a drying temperature of 60-80° C. and a drying time of 8-12 hours.

[0016] Optionally, the preparation method further includes a stirring step before the second drying, wherein the stirring method is oil bath stirring or water bath stirring, and the stirring conditions include: stirring temperature of 50-80°C, stirring speed of 800-1200rpm, and stirring time of 3-8h.

[0017] In the second aspect, one of the purposes of the present invention is to provide a method for preparing a positive electrode material for a lithium-sulfur battery. The preparation method comprises: in a vacuum or inert gas protective atmosphere, sublimated sulfur is mixed with the sulfur-carrying material obtained in the first aspect by melt-filling sulfur to obtain a positive electrode material for a sulfur battery, wherein the temperature of the melt-filling sulfur is 155°C for 4 to 12 hours, wherein the mass proportion of the sulfur-carrying material in the positive electrode material of the lithium-sulfur battery is 5% to 50%. Optionally, the sulfur-carrying method adopts vacuum sulfur-carrying, and the mass proportion of the sulfur-carrying material in the obtained positive electrode material of the lithium-sulfur battery is 10% to 40%.

[0018] In the third aspect, one of the purposes of the present invention is to provide a method for preparing a positive electrode of a lithium-sulfur battery. The preparation method comprises: preparing a mixed slurry containing the positive electrode material obtained in the second aspect, a conductive agent, and a binder, using nitrogen methyl pyrrolidone (NMP) as a solvent, coating the mixed slurry on a current collector, and drying to obtain a positive electrode of a lithium-sulfur battery. Optionally, the proportion of positive electrode materials of a lithium-sulfur battery in the mixed slurry is 80-90%, the conductive agent is 5-10% of a conductive material, and the binder is 5-10%. Optionally, the conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, and graphene, and the binder is polyvinylidene fluoride (PVDF). Optionally, the slurry mixing method adopts a ball milling method, the ball milling time is 1~2h, and the positive electrode sulfur loading is 0.5~10mg / cm 2 .

[0019] In a fourth aspect, one of the purposes of the present invention is to provide a method for preparing a lithium-sulfur battery. The preparation method comprises: assembling the positive electrode and the metal negative electrode, the separator, the electrolyte and the shell obtained in the third aspect to obtain a lithium-sulfur battery. The metal negative electrode is metallic lithium. The separator is selected from a microporous polyolefin separator, a ceramic separator or a non-woven fabric separator. Optionally, the polyolefin separator is composed of one or more layers of polyethylene (PE) and polypropylene (PP). The electrolyte is composed of a lithium-containing electrolyte and a non-aqueous organic solvent. The electrolyte is lithium bistrifluoromethanesulfonyl imide (LiTFSI), the non-aqueous organic solvent is one or two of dioxolane and ethylene glycol dimethyl ether (DME), and the additive is 0~2wt% (mass percentage) of LiNO3.

[0020] In a fifth aspect, one of the objectives of the present invention is to provide the use of the sulfur-carrying material described in the first aspect in the preparation of a lithium-sulfur battery positive electrode material, a lithium-sulfur battery positive electrode and a lithium-sulfur battery.

[0021] Compared with the prior art, the present invention has at least the following technical effects: (1) The present invention uses carbon and biomass sugars as carbon sources and deionized water as a dispersion medium, and prepares a carbon ball precursor through spray drying, and prepares a porous carbon ball material through further heat treatment. The cost of the obtained material is lower than that of commercial carbon. At the same time, the spherical material increases the contact area between the electrode and the electrolyte, making it easier to be wetted. The tap density of the porous spherical carbon is also improved, which is conducive to the coating and preparation of high-surface-loaded positive electrodes. The carbon ball material is then stirred, dried and sintered with a metal salt and a nitrogen source to prepare a carbon ball carrier material loaded with metal single atoms. The preparation process is simple, reproducible, low-cost, environmentally friendly, highly controllable, and easy to industrialize. The preparation process of the sulfur-carrying material provided by the present invention is green, simple, low-cost, reproducible, highly controllable, and easy to industrialize.

[0022] (2) The sulfur-carrying material prepared by the present invention has a spherical structure and a high tap density, and the porous structure of the carbon sphere helps to increase the contact area between the active material and the electrolyte. As a carrier of the positive electrode material of a lithium-sulfur battery, it plays a role in "physical confinement" and "chemical adsorption" of polysulfides, reducing the "shuttle effect". In addition, by embedding metal single-atom active sites, the electron transport capacity and the number of active sites of the sulfur-carrying material are increased, which not only improves the conductivity of the carbon material, but also the catalytic properties of the single-atom metal can greatly improve the reaction kinetics of the lithium-sulfur battery, accelerate the electron transport in the electrochemical reaction process, reduce the shuttling of polysulfides, and reduce the polarization of the battery.

[0023] (3) The sulfur-carrying material provided by the present invention can be used as a positive electrode carrier of a lithium-sulfur battery. It can not only fix sulfur by physical confinement, but also improve the conversion reaction kinetics of the sulfur positive electrode. When it is used as a positive electrode material of a lithium-sulfur battery, it can exhibit excellent electrochemical performance.

[0024] (4) The sulfur-carrying material obtained by the present invention has a high specific surface area and pore structure, has a good adsorption effect on LiPs, can provide a channel for the transmission of electrolyte, promote ion diffusion, improve the battery specific capacity and cycle stability, and significantly reduce the migration resistance of lithium ions and electrons in the sulfur / carbon lithium sulfur battery positive electrode material; in addition, the single-atom catalyst can significantly activate and reduce the delithiation barrier of the final discharge product due to its high activity, thereby affecting the macroscopic reaction kinetics of the active sulfur redox process and improving the charge and discharge performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the X-ray diffraction pattern (XRD) of the sulfur-carrying material (Co-NC) obtained in Example 1 of the present invention.

[0026] Figure 2 This is a scanning electron microscope image (SEM) of the sulfur-carrying material (Co-NC) prepared in Example 1 of the present invention.

[0027] Figure 3 The 20nm and 10nm transmission electron microscope (TEM) images of the sulfur-carrying material (Co-NC) prepared in Example 1 of the present invention are shown.

[0028] Figure 4 This is the full X-ray photoelectron spectrum (XPS) of the sulfur-carrying material (Co-NC) prepared in Example 1 of the present invention.

[0029] Figure 5 The contact angle test graphs of lithium-sulfur battery positive electrode materials prepared using the sulfur-carrying material (Co-NC, left figure) obtained in Example 1 and the sulfur-carrying material (NC, right figure) obtained in Comparative Example 1 are respectively.

[0030] Figure 6 The electrochemical impedance test curves of lithium-sulfur batteries prepared with the sulfur-carrying material (Co-NC) prepared in Example 1 and the sulfur-carrying material (NC) prepared in Comparative Example 1 are shown.

[0031] Figure 7 The graphs are the cycle performances of lithium-sulfur batteries prepared with the sulfur-carrying material (Co-NC) prepared in Example 1, the sulfur-carrying material (NC) prepared in Comparative Example 1, and the sulfur-carrying material (double single atom) prepared in Comparative Example 2 at a current density of 0.2C (1C=1675mA / g).

[0032] Figure 8 These are different rate performance diagrams of lithium-sulfur batteries prepared using the sulfur-carrying material (Co-NC) prepared in Example 1, the sulfur-carrying material (NC) prepared in Comparative Example 1, and the sulfur-carrying material (double single atom) prepared in Comparative Example 2.

[0033] Fig. 9 The graphs are the cycle performances of lithium-sulfur batteries prepared with the sulfur-carrying material (Co-NC) prepared in Example 1 and the sulfur-carrying material (Ni-NC) prepared in Example 5 at a current density of 0.2C. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The reagents not described separately in detail in the present invention are all conventional reagents and can be obtained from commercial channels; the methods not described in detail are all conventional experimental methods and can be obtained from the prior art.

[0035] Example 1

[0036] 1. Preparation and testing of sulfur-carrying materials This embodiment provides a method for preparing a sulfur-carrying material, comprising the following steps: (1) 6 g of conductive carbon black (purchased from Power Source, purity 99%) and 4 g of glucose were dispersed in 100 g of deionized water, and stirred at 1200 rpm and 30° C. for 12 h to form a mixed slurry; (2) Take 100 mL of the mixed slurry and spray dry it at 100°C. The slurry flow rate entering the spray system is 20 mL / min, the atomization pressure is 10 MPa, and the gas flow rate is ≤10 L / min. Then dry it at 60°C for 12 hours to obtain sample I; (3) placing sample I in a tube furnace under an argon atmosphere at 1200° C. for a first sintering treatment for 4 h, and naturally cooling to room temperature to obtain sample II; (4) 0.0188 g of cobalt acetate tetrahydrate and 0.095 g of 1,10-phenanthroline were mixed and added to 10 mL of pure ethanol, and stirred for 1 h to obtain a uniform solution; the mass ratio between the metal source and the nitrogen source was 1:6; (5) 1 g of sample II was added to the uniform solution obtained in step (4), with the mass ratio of sample II to the uniform solution being 1:0.1. The mixture was stirred in an oil bath at 60°C for 4 h, dried at 80°C for 8 h, and then sintered at 600°C under argon for 4 h to obtain the sulfur-loaded material (Co-NC).

[0037] Figure 1 The XRD pattern of the sulfur-carrying material (Co-NC) obtained in this example is shown. Figure 1 In the figure, the diffraction peaks at 23° and 43° are carbon diffraction peaks, and there are no characteristic diffraction peaks of Co elemental substance, which correspond to the (002) and (100) crystal planes of carbon respectively. In addition, there are no diffraction peaks of Co and its compounds, which indicates that Co is dispersed in the mesoporous carbon in the form of atoms.

[0038] like Figure 2 As shown, the sulfur-loaded material (Co-NC) obtained in this example still maintains a spherical morphology.

[0039] like Figure 3 As shown, the sulfur-loaded material (Co-NC) obtained in this example does not show metal agglomeration, which further indicates that the Co metal is dispersed on the carbon spheres in the form of atoms.

[0040] Figure 4 The XPS graph of the sulfur-carrying material (Co-NC) obtained in this example is shown. Figure 4 The Co 2pXPS peak at 781 eV and the peak at 786.0 eV indicate that the Co element on Co-NC exists in ionic form.

[0041] 2. Preparation and testing of lithium-sulfur battery positive electrode materials, lithium-sulfur battery positive electrodes and lithium-sulfur batteries 30 mg of Co-NC and 120 mg of elemental sulfur powder were mixed and heat treated at 155°C for 12 h under vacuum to obtain the positive electrode material for lithium-sulfur batteries.

[0042] The prepared positive electrode material of lithium-sulfur battery, conductive carbon black and binder polyvinylidene fluoride were mixed evenly and fully ground, then mixed with dispersant N-methylpyrrolidone to make the sample viscous, coated on aluminum foil, dried, and the dried sample was cut into electrode sheets with a diameter of 10 mm. The electrode sheet was used as the positive electrode of lithium-sulfur battery, and the sulfur loading in the obtained positive electrode was 5 mg / cm 2 . 2032 button cells were used for the electrochemical performance test of the electrode material, with the positive electrode as the working electrode, the 14mm round lithium sheet as the counter electrode, and the Celgard 2400 polypropylene film (diameter 19mm, thickness 25μm) as the diaphragm. The electrolyte was a mixed solution of 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) (volume ratio 1:1) containing 1M lithium bistrifluoromethanesulfonyl imide (LiTFSI) electrolyte and 0.2M lithium nitrate (LiNO3) additives. After standing at room temperature for 8h, the electrochemical performance of the lithium-sulfur battery was tested. During the charge and discharge test, the potential range was 1.8~2.8V (vs. Li / Li + ).

[0043] like Figure 5 As shown in the figure, the electrolyte wettability of the positive electrode material (S / Co-NC) after the sulfur-loaded material (Co-NC) is significantly higher than that of the sulfur-loaded material (NC), which is conducive to the penetration of the electrolyte into the dense sulfur positive electrode to achieve good ion transport. This shows that the dense S / Co-NC overall positive electrode has unique characteristics such as compact structure, high density, high conductivity and good electrolyte permeability.

[0044] like Figure 6 As shown, the lithium-sulfur battery assembled with Co-NC as the positive electrode material has a smaller impedance, indicating that ions can migrate more easily in the positive electrode material.

[0045] like Figure 7 As shown, at a current density of 0.2C, the lithium-sulfur battery has an initial specific capacity of 805mAh / g. After 100 cycles, the capacity remains at 693mAh / g, with a capacity retention rate of up to 86%.

[0046] Embodiment 2~embodiment 4 Different sulfur-carrying materials, lithium-sulfur battery positive electrode materials, lithium-sulfur battery positive electrodes and lithium-sulfur batteries were obtained by referring to the preparation process of Example 1. Among them, Examples 2 to 4 differ only in the temperature of the first sintering. The first sintering temperature in the specific sulfur-carrying material preparation process, the initial specific capacity of the lithium-sulfur battery and the capacity retention rate (the percentage of the last cycle capacity to the first cycle capacity) are shown in Table 1. The capacity retention rate is calculated as the specific capacity after 0.2C cycle / 0.2C initial specific capacity.

[0047] Table 1

[0048] As can be seen from Table 1 above, at a current density of 0.2C, the lithium-sulfur battery of Sample II in Example 1 with a pretreatment temperature of 1200°C has an initial specific capacity of 805mAh / g, and the capacity retention rate can reach 89.8% after 50 cycles. It can be seen that when the first sintering temperature is 1200°C, the Co-NC catalyst has the best effect and the battery has the best stability.

[0049] Example 5

[0050] 1. Preparation of sulfur-carrying materials This embodiment provides a method for preparing a sulfur-carrying material, comprising the following steps: (1) Dispersing 5 g of conductive carbon black and 5 g of glucose in 120 g of deionized water, stirring at 1000 rpm and 25° C. for 15 h to form a mixed slurry; (2) Take 120 mL of the mixed slurry and spray dry it at 90°C. The slurry flow rate entering the spray system is 15 mL / min, the atomization pressure is 10 MPa, and the gas flow rate is ≤ 8 L / min. Then dry it at 80°C for 12 hours to obtain sample I; (3) Sample I was placed in a tube furnace under an argon atmosphere for a first sintering treatment at 1000°C for 6 hours, and then naturally cooled to room temperature to obtain sample II; (4) 0.0188 g of nickel acetate tetrahydrate and 0.095 g of 1,10-phenanthroline were mixed and added to 20 mL of pure ethanol, and stirred for 2 h to obtain a uniform solution; the mass ratio between the metal source and the nitrogen source was 1:6; (5) 1 g of sample II was added to the uniform solution obtained in step (4), with the mass ratio of sample II to the uniform solution being 1:0.1. The mixture was stirred in an oil bath at 60°C for 4 h, dried at 80°C for 8 h, and then sintered at 600°C under argon for 4 h to obtain the sulfur-loaded material (Ni-NC).

[0051] 2. Preparation and testing of lithium-sulfur battery positive electrode materials, lithium-sulfur battery positive electrodes and lithium-sulfur batteries 30 mg Ni-NC and 120 mg elemental sulfur powder were mixed and heat treated at 155 ° C for 12 h under vacuum to obtain a positive electrode material for a lithium-sulfur battery. The preparation process of the positive electrode and the lithium-sulfur battery is referred to Example 1, wherein the loading amount of the positive electrode sulfur is 5 mg / cm 2 .

[0052] The electrochemical performance of the lithium-sulfur battery was tested in the same manner as in Example 1.

[0053] like Fig. 9 As shown in the figure, at a current density of 0.2C, the lithium-sulfur battery has an initial specific capacity of 703mAh / g. After 60 cycles, the capacity remains at 602mAh / g, with a capacity retention rate of up to 85%. The overall cycle life curve is lower than that of the lithium-sulfur battery assembled by Co-NC.

[0054] Comparative Example 1 In Comparative Example 1, a sulfur-carrying material was prepared by referring to the steps of Example 1, except that step (4) of Example 1 was replaced by not adding a metal source, and the sulfur-carrying material prepared was used to prepare a lithium-sulfur battery positive electrode material, a lithium-sulfur battery positive electrode and a lithium-sulfur battery in turn, and the performance of the lithium-sulfur battery was tested.

[0055] The cycle performance of the sulfur-carrying material (NC) obtained in Comparative Example 1 at 0.2C current is as follows: Figure 7 As shown, the performance of different rates is as follows Figure 8 By comparing the performance of the sulfur-carrying material and the lithium-sulfur battery obtained in Comparative Example 1 with that in Example 1, it is found that the introduction of metal single atoms significantly improves the performance and cycle life of the lithium-sulfur battery, especially the introduction of Co single atoms.

[0056] Comparative Example 2 The performance of lithium-sulfur batteries prepared by nitrogen-doped carbon-cobalt-nickel diatomic catalysts (Co-Ni-NC, Nanjing Xianfeng Nanomaterials Technology) was tested, with C content: 65-75wt% (XPS), N content: 10-20wt% (XPS), Co content: 2-3wt% (XPS), and Ni content: 2-3wt% (XPS).

[0057] like Figure 7 , 8 As shown, at a current density of 0.2C, the capacity of the lithium-sulfur battery remained at 556 mAh / g after 100 cycles, which is lower than the Co-NC assembled battery prepared in Example 1 (693 mAh / g). This shows that the sulfur-carrying material Co-NC prepared in Example 1 is more suitable for use as the positive electrode of a lithium-sulfur battery.

[0058] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a positive electrode material for a lithium-sulfur battery, the preparation method include: Under vacuum or inert gas protection atmosphere, sublimated sulfur and sulfur-carrying material are mixed by melt-filling sulfur to obtain a sulfur battery positive electrode material, wherein the temperature of the melt-filling sulfur is 155° C. and the temperature is kept for 4 to 12 hours, wherein the mass proportion of the sulfur-carrying material in the lithium-sulfur battery positive electrode material is 5% to 50%; The sulfur-carrying material is used to load sulfur to prepare a positive electrode of a lithium-sulfur battery. The preparation method of the sulfur-carrying material comprises: sequentially subjecting the mixed slurry containing the first carbon source and the second carbon source to a first drying and a first sintering to obtain a dry material; and The dry material is mixed into a solution containing a metal source and a nitrogen source, and the sulfur-carrying material is obtained by sequentially performing a second drying and a second sintering; Wherein, the first carbon source is selected from conductive carbon black, and the second carbon source is selected from one of sugar alcohol, glucose, and sucrose; the mass ratio of the first carbon source to the second carbon source in the mixed slurry is (4-7): (3-6); The first sintering conditions include: sintering temperature of 800-1200°C, sintering time of 3-5h; The second sintering conditions include: a sintering temperature of 500-1000° C. and a sintering time of 3-6 hours. 2 . The preparation method according to claim 1 , wherein the temperature of the first sintering is 1200° C., 1000° C., 800° C. or 600° C.

3. The preparation method according to claim 1, wherein the first drying is spray drying; Optionally, the spray drying conditions include: spray drying at 80-150°C, and collecting the spray-dried crude product; The slurry flow rate entering the spray system is 10~30mL / min, the atomization pressure is 5~15MPa, and the gas flow rate is ≤10L / min; Optionally, the metal source is selected from one of acetate, nitrate and chlorate containing metals Fe, Co, Ni, Zn and Cu; the nitrogen source is 1,10-phenanthroline and / or dimethylimidazole; Optionally, the mass ratio of the metal source to the nitrogen source is 1:(1-3); Optionally, the mass ratio of the dry material mixed into the solution containing the metal source and the nitrogen source is 1:(0.1-0.5); Optionally, the first sintering atmosphere is selected from one of nitrogen and argon, and the second sintering atmosphere is selected from one of nitrogen and argon; Optionally, the second drying conditions include: drying temperature of 60-80° C., drying time of 8-12 h; Optionally, the preparation method further includes a stirring step before the second drying, wherein the stirring method is oil bath stirring or water bath stirring, and the stirring conditions include: stirring temperature of 50-80°C, stirring speed of 800-1200rpm, and stirring time of 3-8h.

4. A method for preparing a positive electrode of a lithium-sulfur battery, the preparation method include: A mixed slurry containing the positive electrode material of a lithium-sulfur battery obtained by any preparation method according to any one of claims 1 to 3, a conductive agent, and a binder, with nitrogen methyl pyrrolidone as a solvent, is prepared, the mixed slurry is coated on a current collector, and dried to obtain a positive electrode of a lithium-sulfur battery.

5. A method for preparing a lithium-sulfur battery, the preparation method include: The lithium-sulfur battery positive electrode and metal negative electrode, a separator, an electrolyte and a shell obtained in claim 4 are assembled to obtain a lithium-sulfur battery.

6. Use of the sulfur-carrying material obtained by the preparation method according to any one of claims 1 to 3 in the preparation of lithium-sulfur battery positive electrode materials, lithium-sulfur battery positive electrodes and lithium-sulfur batteries.

Citation Information

Patent Citations

  • Active carbon material with spherical structure and preparation method and applications thereof

    CN107808955A

  • Preparation method of lithium-sulfur battery positive electrode

    CN108123102A

  • Cobalt-doped carbon nanotube composite diaphragm and preparation method thereof

    CN112290162A

  • Application of cobalt-nitrogen-doped carbon material in positive electrode of all-solid-state lithium-sulfur battery and preparation of cobalt-nitrogen-doped carbon material

    CN114023940A