Lithium cobalt oxide sintering process

Through the two sintering process and aluminum hydroxide doping method, the problems of grain growth and uneven element distribution of lithium cobalt oxide materials during high-temperature sintering are solved, and the uniformity and electrochemical properties of the material are improved. It is suitable for lithium Ion battery.

CN118978188APending Publication Date: 2024-11-19安徽巡鹰新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411352470.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the high-temperature sintering of lithium cobalt oxide materials, grain growth leads to degradation of material unevenness and electrochemical properties, and the uneven distribution of cobalt and lithium elements affects the uniformity and performance of the material.

Method used

The first sintering temperature is controlled at 800-850℃ to remove moisture and lithium carbonate decomposition products, and then pulverize and mix with titanium dioxide, and then perform secondary sintering, and the temperature is controlled at 900-1100℃ to optimize the crystal structure; Meanwhile, nano-grade aluminum hydroxide doping is used to inhibit the growth of lithium cobalt oxide particles.

Benefits of technology

The obtained lithium cobalt oxide material particles are smooth, have excellent cycle stability and conductivity. They are suitable for lithium-ion batteries and have better rate discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062714400000061
    Figure BDA0005062714400000061
Patent Text Reader

Abstract

The invention discloses a lithium cobalt oxide sintering process, and belongs to the technical field of lithium cobalt oxide materials, and the lithium cobalt oxide sintering process comprises the following steps: step 1, uniformly mixing cobaltosic oxide, lithium carbonate and aluminum hydroxide to obtain a primary mixed material; step 2, sintering, crushing and drying the primary mixed material to obtain a primary sintered material; step 3, uniformly mixing the primary sintered material with titanium dioxide to obtain a secondary mixed material; and step 4, sintering, crushing and drying the secondary mixed material to obtain the composite material. By selecting the raw material components and regulating and controlling the sintering temperature, the finally obtained lithium cobalt oxide particles are smooth, are stable in circulation and excellent in conductivity, and can be better applied to the field of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium cobalt oxide materials, and in particular relates to a lithium cobalt oxide sintering process. Background Art

[0002] Lithium cobalt oxide (LiCoO2) positive electrode material has the advantages of high energy density, high operating voltage, high tap density, high safety, and long cycle life. Lithium cobalt oxide is currently the most widely used positive electrode material in commercial lithium-ion batteries. High-rate lithium cobalt oxide is mostly used in high-power electronic devices such as electronic models (aircraft models, car models, etc.) and wireless electric toys. It is one of the most promising key materials.

[0003] During the production process of lithium cobalt oxide materials, especially during high-temperature sintering, lithium cobalt oxide particles are prone to grain growth, resulting in larger grain size, which not only affects the uniformity of the material, but may also reduce the electrochemical properties of the material, such as capacity retention and cycle stability. At the same time, during the sintering process, due to uneven temperature distribution or differences in reaction kinetics, the distribution of cobalt and lithium elements in the lithium cobalt oxide material may be uneven, thereby affecting the uniformity and electrochemical properties of the lithium cobalt oxide material. Therefore, in order to overcome the above shortcomings and improve the quality and performance of lithium cobalt oxide materials, optimizing and improving the sintering process of lithium cobalt oxide and the quality of finished products are technical issues that need to be solved urgently. Summary of the invention

[0004] The object of the present invention is to provide a lithium cobalt oxide sintering process to solve one of the problems mentioned in the background technology.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A lithium cobalt oxide sintering process comprises the following steps:

[0007] Step 1, mixing cobalt tetroxide, lithium carbonate and aluminum hydroxide evenly to obtain a primary mixed material;

[0008] Step 2, sintering, crushing and drying the primary mixed material to obtain a primary sintered material;

[0009] Step 3, uniformly mixing the primary sintered material with titanium dioxide to obtain a secondary mixed material;

[0010] Step 4: sintering, crushing and drying the secondary mixed material.

[0011] As a further embodiment of the present invention, in step 1, the mass ratio of cobalt tetroxide, lithium carbonate and aluminum hydroxide is 16.5-17:6-7:0.032-0.035.

[0012] As a further solution of the present invention, the particle size of the cobalt oxide is 3-5 μm.

[0013] As a further embodiment of the present invention, the particle size of the aluminum hydroxide is 20-30 nm.

[0014] As a further solution of the present invention, the amount of titanium dioxide used in step 3 is 0.14%-0.15% of the mass of the primary sintering material.

[0015] As a further solution of the present invention, in step 2, the sintering temperature is 800-850° C. and the sintering time is 10-14 hours.

[0016] As a further solution of the present invention, in step 2, the particles are crushed to a particle size of 3-6 μm.

[0017] As a further solution of the present invention, in step 4, the sintering temperature is 900-1100° C., and the sintering time is 8-12 hours.

[0018] As a further solution of the present invention, in step 4, the particles are crushed to a particle size of 3-6 μm.

[0019] Beneficial effects of the present invention:

[0020] The present invention controls the temperature during the sintering process of lithium cobalt oxide, and finally obtains the lithium cobalt oxide material with good comprehensive performance. The present invention adopts a two-time sintering method, wherein the temperature of the first sintering is controlled at 800-850°C, at which temperature, water in the raw material and carbon dioxide generated by the decomposition of lithium carbonate can escape, and a partial sintering reaction can be performed; then, the second sintering is performed after crushing and secondary mixing, the temperature of the second sintering is controlled at 900-1100°C, and the reaction temperature is controlled at above 900°C. Due to the high sintering temperature, after exceeding 900°C, the crystals can grow rapidly and the structural defects can be improved. The finally obtained lithium cobalt oxide particles are smooth, and have excellent cycle stability and conductive properties, and can be better applied in the field of lithium ion batteries.

[0021] Furthermore, the present invention uses cobalt tetraoxide, lithium carbonate and nano-scale aluminum hydroxide to mix once to obtain a primary mixed material. 3+ and Co 3+ The valence state of Al is +3, and 3+ The ionic radius of Co 3+ Similar to the above, doping aluminum hydroxide into the raw materials can replace some of the cobalt sites, thereby inhibiting the growth of lithium cobalt oxide particles, reducing the particle size of lithium cobalt oxide, improving cycle stability and enhancing conductivity. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] This embodiment provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0025] Step 1, 16.5 kg of cobalt tetroxide (particle size of 3 μm), 6 kg of lithium carbonate and 0.032 kg of aluminum hydroxide (particle size of 20 nm) are mixed uniformly to obtain a primary mixed material;

[0026] Step 2, sintering the primary mixed material at a sintering temperature of 800° C. for 14 h, crushing the material to a particle size of 3.5 μm, and drying the material to obtain a primary sintered material;

[0027] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.14% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0028] Step 4: Sinter the secondary mixed material at a sintering temperature of 950° C. for 12 h, then crush it to a particle size of 3.5 μm, and dry it.

[0029] Example 2

[0030] This embodiment provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0031] Step 1, 16.8 kg of cobalt trioxide (particle size 3 μm), 6.5 kg of lithium carbonate and 0.033 kg of aluminum hydroxide (particle size 20 nm) are mixed uniformly to obtain a primary mixed material;

[0032] Step 2, sintering the primary mixed material at a sintering temperature of 800° C. for 10 h, crushing the material to a particle size of 3.5 μm, and drying the material to obtain a primary sintered material;

[0033] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.14% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0034] Step 4: Sinter the secondary mixed material at a sintering temperature of 950° C. for 12 h, then crush it to a particle size of 3.5 μm, and dry it.

[0035] Example 3

[0036] This embodiment provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0037] Step 1, 17 kg of cobalt trioxide (particle size 3 μm), 7 kg of lithium carbonate and 0.035 kg of aluminum hydroxide (particle size 20 nm) are mixed uniformly to obtain a primary mixed material;

[0038] Step 2, sintering the primary mixed material at a sintering temperature of 850° C. for 12 h, crushing the material to a particle size of 5 μm, and drying the material to obtain a primary sintered material;

[0039] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.15% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0040] Step 4: sinter the secondary mixed material at a sintering temperature of 1000° C. for 10 h, then crush it to a particle size of 5 μm, and dry it.

[0041] Example 4

[0042] This embodiment provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0043] Step 1, 17 kg of cobalt tetroxide (particle size of 5 μm), 7 kg of lithium carbonate and 0.035 kg of aluminum hydroxide (particle size of 30 nm) are mixed uniformly to obtain a primary mixed material;

[0044] Step 2, sintering the primary mixed material at a sintering temperature of 850° C. for 12 h, crushing the material to a particle size of 5 μm, and drying the material to obtain a primary sintered material;

[0045] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.15% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0046] Step 4: sinter the secondary mixed material at a sintering temperature of 1100° C. for 8 h, then crush it to a particle size of 5 μm, and dry it.

[0047] Comparative Example 1

[0048] This comparative example provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0049] Step 1, 16.5 kg of cobalt tetroxide (particle size of 3 μm) and 6 kg of lithium carbonate are mixed evenly to obtain a primary mixed material;

[0050] Step 2, sintering the primary mixed material at a sintering temperature of 800° C. for 14 h, crushing the material to a particle size of 3.5 μm, and drying the material to obtain a primary sintered material;

[0051] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.14% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0052] Step 4: Sinter the secondary mixed material at a sintering temperature of 950° C. for 12 h, then crush it to a particle size of 3.5 μm, and dry it.

[0053] Comparative Example 2

[0054] This comparative example provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0055] Step 1, 16.5 kg of cobalt tetroxide (particle size of 3 μm), 6 kg of lithium carbonate and 0.032 kg of aluminum hydroxide (particle size of 20 nm) are mixed uniformly to obtain a primary mixed material;

[0056] Step 2, sintering the primary mixed material at a sintering temperature of 700° C. for 14 h, crushing the material to a particle size of 3.5 μm, and drying the material to obtain a primary sintered material;

[0057] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.14% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0058] Step 4: Sinter the secondary mixed material at a sintering temperature of 950° C. for 12 h, then crush it to a particle size of 3.5 μm, and dry it.

[0059] Comparative Example 3

[0060] This comparative example provides a lithium cobalt oxide sintering process, and the specific steps are as follows:

[0061] Step 1, 16.5 kg of cobalt tetroxide (particle size of 3 μm), 6 kg of lithium carbonate and 0.032 kg of aluminum hydroxide (particle size of 20 nm) are mixed uniformly to obtain a primary mixed material;

[0062] Step 2, sintering the primary mixed material at a sintering temperature of 900° C. for 14 h, crushing the material to a particle size of 3.5 μm, and drying the material to obtain a primary sintered material;

[0063] Step 3, uniformly mixing the primary sintered material with titanium dioxide, wherein the amount of titanium dioxide used is 0.14% of the mass of the primary sintered material, to obtain a secondary mixed material;

[0064] Step 4: Sinter the secondary mixed material at a sintering temperature of 850° C. for 12 h, then crush it to a particle size of 3.5 μm, and dry it.

[0065] The performance test of the lithium cobalt oxide obtained in Examples 1-4 and Comparative Examples 1-3 was performed: the obtained lithium cobalt oxide was used as the positive electrode active material, and graphite was used as the negative electrode to assemble a soft-pack battery, and the battery was tested for electrical performance using a battery performance tester. The charge and discharge cut-off voltage was 3-4.2V, the charge rate was 0.2C, and the first 1C discharge specific capacity was measured, and the capacity retention rate at different discharge rates of 20C, 30C, 45C, and 60C compared to 1C was measured. The test results are shown in Table 1:

[0066] Table 1

[0067]

[0068] It can be seen from the data in Table 1 that the lithium cobalt oxide obtained in Examples 1-4 has better discharge specific capacity and capacity retention rate than the lithium cobalt oxide obtained in Comparative Examples 1-3. It can be seen that the lithium cobalt oxide sintering process provided in the present invention shows that the doping of aluminum hydroxide and the regulation of the two sintering temperatures can reduce the particle size of lithium cobalt oxide and stabilize the crystal structure, so that the lithium cobalt oxide has better rate discharge performance.

[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A lithium cobalt oxide sintering process, characterized in that: The following steps are involved: Step 1, mixing cobalt tetroxide, lithium carbonate and aluminum hydroxide evenly to obtain a primary mixed material; Step 2, sintering, crushing and drying the primary mixed material to obtain a primary sintered material; Step 3, uniformly mixing the primary sintered material with titanium dioxide to obtain a secondary mixed material; Step 4: sintering, crushing and drying the secondary mixed material.

2. A lithium cobalt oxide sintering process according to claim 1, characterized in that: In step 1, the mass ratio of cobalt tetroxide, lithium carbonate and aluminum hydroxide is 16.5-17:6-7:0.032-0.

035.

3. A lithium cobalt oxide sintering process according to claim 1, characterized in that: The particle size of the cobalt trioxide is 3-5 μm.

4. A lithium cobalt oxide sintering process according to claim 1, characterized in that: The particle size of the aluminum hydroxide is 20-30 nm.

5. A lithium cobalt oxide sintering process according to claim 1, characterized in that: The amount of titanium dioxide used in step 3 is 0.14%-0.15% of the mass of the primary sintering material.

6. A lithium cobalt oxide sintering process according to claim 1, characterized in that: In step 2, the sintering temperature is 800-850° C. and the sintering time is 10-14 hours.

7. A lithium cobalt oxide sintering process according to claim 1, characterized in that: In step 2, the powder is crushed to a particle size of 3-6 μm.

8. A lithium cobalt oxide sintering process according to claim 1, characterized in that: In step 4, the sintering temperature is 900-1100° C. and the sintering time is 8-12 hours.

9. A lithium cobalt oxide sintering process according to claim 1, characterized in that: In step 4, the powder is crushed to a particle size of 3-6 μm.