Preparation method of high-transmittance photo-thermal glass

By using mixed melting and plasma etching technology of cerium oxide, lithium oxide and composite clarifier in photothermal glass, the problem of double improvement of transmittance and mechanical properties of photothermal glass is solved, and high light transmission and high mechanical properties are achieved Performance effect.

CN118978332APending Publication Date: 2024-11-19JIANGSU SIMBA NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411069271.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When existing photothermal glasses reduce iron content to improve transmittance, their heat transmittance increases, resulting in difficulty in clarifying glass, increasing micro bubbles, affecting product quality, and it is difficult to improve light transmittance and mechanical properties at the same time.

Method used

The mixture of cerium oxide, lithium oxide and composite clarifier is used to accelerate combustion and enhance the oxidation potential through ozone gas, reduce iron ion absorption, combine plasma etching and diamond-like deposition to form an urgency film, and enhance the light transmission and mechanics of the glass. performance.

Benefits of technology

The glass preparation with high light transmission and high mechanical properties is achieved. Through bubble floating and network structure transformation, the optical and mechanical uniformity of the glass is improved, the light transmittance and mechanical properties are enhanced, and the clarification effect is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980358650000071
    Figure BDA0004980358650000071
Patent Text Reader

Abstract

The invention discloses a preparation method of high-transmittance photo-thermal glass, and relates to the technical field of glass. Oxidation potential energy during combustion is enhanced by utilizing high-speed ozone, the light transmittance of the glass is improved, a small amount of molten cerium oxide looses and destroys a network structure of the cerium oxide, bubbles are separated from wrapping of glass liquid, scattering of light rays by the glass is reduced, the optical and mechanical uniformity of the glass is improved, and along with the increase of the melting amount of the cerium oxide, the light transmittance of the glass is improved. Lithium oxide is filled in gaps among network structures, so that the glass network structures are more compact, the mechanical property of the glass is improved, the clarification range of the glass is expanded by utilizing a compound clarifying agent, the gas flow is adjusted, the temperature difference between the upper surface and the lower surface of molten glass is properly increased, and the clarification effect is enhanced; and performing hydrogen plasma etching, introducing methane to generate silicon carbide, and performing diamond-like precipitation to form an antireflection film, thereby realizing the effects of high light transmittance and high mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of glass technology, and in particular to a method for preparing high-light-transmittance photothermal glass. Background Art

[0002] Energy shortage has become a major problem hindering the development of the world economy today, and the development of new energy has been widely recognized; as a pollution-free and renewable energy source, the use of solar energy has received more and more attention. With the maturity of research and development technology, solar thermal products have emerged; solar thermal power generation has gradually become an important part of the solar power generation industry due to its advantages of heat storage, high efficiency, and strong power generation continuity. In the field of construction, the application of photothermal glass will become more and more extensive. Its unique performance can convert solar radiation into electrical energy, which not only effectively reduces indoor temperature and air conditioning energy consumption, but also provides renewable energy for buildings and achieves green energy saving. With the support of the state for new energy power generation, solar thermal power generation will usher in rapid development. Photothermal glass is the basic material for producing the core basic component of solar thermal power generation, the concentrator. It must meet the high solar transmittance, and the iron content is an important factor affecting the glass transmittance. To achieve the transmittance requirements of photothermal glass, as the iron content in the glass decreases, the heat permeability of the glass increases, the vertical temperature gradient is small, making it difficult to clarify the glass, and the number of microbubbles in the glass increases, which directly affects the quality of the product. Therefore, it is particularly necessary to invent a high-transmittance photothermal glass. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing high-light-transmittance photothermal glass to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing high-transmittance photothermal glass, comprising the following preparation steps:

[0005] (1) mixing batch materials, composite clarifier, cerium oxide and lithium oxide, introducing ozone at 100 to 300 mL / s, heating and melting, and introducing air when the melting time reaches two-thirds, increasing the gas flow rate, and obtaining glass liquid;

[0006] (2) pouring the glass liquid into a mold, performing annealing treatment, and then cooling to room temperature in a furnace, then placing it in anhydrous ethanol and deionized water in turn, performing ultrasonic cleaning, and then blowing it dry with nitrogen to obtain an intermediate A;

[0007] (3) Place the intermediate A under vacuum at 4×10 -3Pa environment, introduce protective gas - argon to a gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to a gas pressure of 3-6kPa for plasma etching, then introduce methane at 4mL / min and maintain the gas pressure at 4-8kPa, react for 20-60min, then carry out diamond-like deposition to obtain high-transmittance photothermal glass.

[0008] Furthermore, the mass percentages of the ingredients of the batch in step (1) are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide, and 7.4% sodium oxide.

[0009] Furthermore, the composite clarifier in step (1) is composed of mirabilite, sodium chloride, tin oxide and carbon powder in a mass ratio of 1 to 3:0.4 to 0.6:0.5 to 1:5.

[0010] Furthermore, in step (1), the mass ratio of the batch material, the composite clarifier, the cerium oxide and the lithium oxide is 10:0.3-1:0.2-0.5:0.2-0.5.

[0011] Furthermore, the air flow rate in step (1) is 15 to 30 m / s.

[0012] Furthermore, the melting process parameters of step (1) are: heating rate of 3 to 10°C / min, temperature of 1450 to 1800°C, and holding time of 3 to 6h.

[0013] Furthermore, the parameters of the annealing treatment in step (2) are: temperature of 400-700° C. and holding time of 0.5-2 h.

[0014] Furthermore, the frequency of the ultrasound in step (2) is 21 kHz and the time is 15 min.

[0015] Furthermore, the process parameters of the plasma etching in step (3) are: microwave power of 500-900 W, time of 20-60 s, and temperature of 100-300° C.

[0016] Furthermore, in step (3), the deposition temperature is 400-700° C. and the deposition time is 10-30 min.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0018] The glass of the invention is prepared by melting and mixing cerium oxide, lithium oxide, a composite clarifier and a batch material, and then an anti-reflection film is deposited thereon to achieve the effects of high light transmittance and high mechanical properties.

[0019] First, by using ozone gas at a higher rate, when the batch material is converted into glass melt, by increasing the ratio of wind in the combustion system and increasing the amount of gas, the oxidation potential after combustion is enhanced, so that the inevitable very small amount of iron ions are oxidized to a trivalent state, which minimizes the absorption of light and enhances the light transmittance of the glass. By adding cerium oxide and lithium oxide, as the melting temperature increases, lithium ions are more likely to migrate in the matrix. In addition, the small amount of cerium oxide melted at this time is in the network gaps of the glass matrix, loosening and destroying its network structure, reducing the degree of matrix connection, thereby effectively reducing The low viscosity and viscous force of the glass liquid increase the buoyancy of the bubbles, allowing them to break away from the glass liquid and reduce the scattering of light by the glass. As more and more bubbles are gradually discharged from the glass liquid, their specific gravity gradually increases. Under the action of gravity, they flow downward, mix, and homogenize, thereby improving the optical and mechanical uniformity of the glass and improving its light transmittance and mechanical properties. At this time, the melting amount of cerium oxide increases, which plays a gathering role in the glass network, reconnecting the non-bridging oxygen in the original glass network. At the same time, lithium oxide fills the gaps between the network structure, making the glass network structure more compact and improving the mechanical properties of the glass.

[0020] Secondly, variable valence oxides and halides are used to replace part of the Glauber's salt as a composite clarifier. By expanding the clarification range of the glass, step-by-step clarification is achieved to improve the clarification effect. At the same time, the gas flow rate is adjusted to appropriately increase the temperature difference between the upper and lower surfaces of the glass liquid to enhance the clarification effect. Then, hydrogen plasma is used for etching to produce nano-dents, and methane is introduced to react with the surface of the glass substrate to generate silicon carbide, and diamond-like carbon is precipitated to form a flat and dense anti-reflection film, which enables the substrate to achieve high light transmittance and high mechanical properties. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high light transmittance photothermal glass prepared in the following examples are as follows:

[0023] Light transmittance: Take the embodiment and comparative example of the same size and refer to GB / T12997 to test their transmittance in the visible light range.

[0024] Mechanical properties: The same size of the embodiment and the comparative example were taken and tested according to GB / T7962.6 and GB / T7962.18, respectively, to test their Young's modulus and Knoop hardness.

[0025] Example 1; (1) Glauber's salt, sodium chloride, tin oxide and carbon powder are mixed in a mass ratio of 1:0.4:0.5:5 to obtain a composite clarifier; the batch material, the composite clarifier, cerium oxide and lithium oxide are mixed, ozone is introduced at 100 mL / s, and the temperature is increased to 1450°C at 3°C / min to melt, and the temperature is kept for 3 hours. When the melting time reaches two-thirds, air is introduced at 15 m / s to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratios of the batch material, the composite clarifier, cerium oxide and lithium oxide are 10:0.3:0.2:0.2;

[0026] (2) pouring the glass liquid into the mold, annealing it at 400°C for 0.5 h, then cooling it to room temperature, then placing it in anhydrous ethanol and deionized water, ultrasonic cleaning at 21 kHz for 15 min each, and then drying it with nitrogen to obtain intermediate A;

[0027] (3) Place the intermediate A under vacuum at 4×10 -3 Pa environment, introduce protective gas - argon to the gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to the gas pressure of 3kPa, and carry out plasma etching with the process parameters as follows: microwave power of 500W, time of 20s, temperature of 100°C, then introduce methane at 4mL / min, and maintain the gas pressure at 4kPa, react for 20min, then, at 400°C, carry out diamond-like carbon deposition for 10min to obtain high-transmittance photothermal glass.

[0028] Example 2; (1) Glauber's salt, sodium chloride, tin oxide and carbon powder are mixed in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; the batch material, the composite clarifier, cerium oxide and lithium oxide are mixed, ozone is introduced at 200 mL / s, and the temperature is increased to 1650°C at 8°C / min to melt, and the temperature is kept for 4.5 hours. When the melting time reaches two-thirds, air is introduced at 20 m / s to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier, cerium oxide and lithium oxide is 10:0.7:0.4:0.4;

[0029] (2) pouring the glass liquid into a mold, annealing the mold at 400-700°C for 1.5 hours, then cooling the mold to room temperature, then placing it in anhydrous ethanol and deionized water, ultrasonically cleaning it at 21kHz for 15 minutes each, and then drying it with nitrogen to obtain intermediate A;

[0030] (3) Place the intermediate A under vacuum at 4×10 -3 Pa environment, introduce protective gas - argon to the gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to the gas pressure of 4.5kPa, and carry out plasma etching with the process parameters as follows: microwave power of 700W, time of 30s, temperature of 200℃, then, introduce methane at 4mL / min, and maintain the gas pressure at 6kPa, react for 40min, then, at 600℃, carry out diamond-like deposition for 20min to obtain high-transmittance photothermal glass.

[0031] Example 3; (1) Glauber's salt, sodium chloride, tin oxide and carbon powder are mixed in a mass ratio of 3:0.6:1:5 to obtain a composite clarifier; the batch material, the composite clarifier, cerium oxide and lithium oxide are mixed, ozone is introduced at 300 mL / s, and the temperature is increased to 1800°C at 10°C / min to melt, and the temperature is kept for 6 hours. When the melting time reaches two-thirds, air is introduced at 30 m / s to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier, cerium oxide and lithium oxide is 10:1:0.5:0.5;

[0032] (2) pouring the glass liquid into the mold, annealing it at 700°C for 2 hours, then cooling it to room temperature, then placing it in anhydrous ethanol and deionized water, ultrasonic cleaning at 21kHz for 15 minutes each, and then drying it with nitrogen to obtain intermediate A;

[0033] (3) Place the intermediate A under vacuum at 4×10 -3 Pa environment, introduce protective gas - argon to the gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to the gas pressure of 6kPa, and carry out plasma etching with the process parameters as follows: microwave power of 900W, time of 60s, temperature of 300℃, then, introduce methane at 4mL / min, and maintain the gas pressure at 8kPa, react for 60min, then, at 700℃, carry out diamond-like deposition for 30min to obtain high-transmittance photothermal glass.

[0034] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt, sodium chloride, tin oxide and carbon powder in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; mix the batch material, the composite clarifier, cerium oxide and lithium oxide, introduce ozone at 50 mL / s, and heat to 1650° C. at 8° C. / min to melt, and keep warm for 4.5 hours. When the melting time reaches two-thirds, air is introduced to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier, cerium oxide and lithium oxide is 10:0.7:0.4:0.4; the remaining steps are the same as Example 2.

[0035] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt, sodium chloride, tin oxide and carbon powder in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; mix the batch material, the composite clarifier and lithium oxide, introduce ozone at 200 mL / s, and heat to 1650°C at 8°C / min to melt, and keep warm for 4.5 hours. When the melting time reaches two-thirds, air is introduced to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier and lithium oxide is 10:0.7:0.4; the remaining steps are the same as Example 2.

[0036] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt, sodium chloride, tin oxide and carbon powder in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; mix the batch material, the composite clarifier and cerium oxide, introduce ozone at 200 mL / s, and heat to 1650°C at 8°C / min to melt, and keep warm for 4.5 hours. When the melting time reaches two-thirds, air is introduced to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier and the cerium oxide is 10:0.7:0.4; the remaining steps are the same as Example 2.

[0037] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt, sodium chloride, tin oxide and carbon powder in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; mix the batch material and the composite clarifier, introduce ozone at 200 mL / s, and heat to 1650°C at 8°C / min to melt, and keep warm for 4.5 hours. When the melting time reaches two-thirds, air is introduced to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide, and 7.4% sodium oxide; the mass ratio of the batch material to the composite clarifier is 10:0.7; the remaining steps are the same as Example 2.

[0038] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt and carbon powder in a mass ratio of 2:5 to obtain a clarifier; mix the batch material, composite clarifier, cerium oxide and lithium oxide, introduce ozone at 200 mL / s, and heat to 1650°C at 8°C / min to melt, and keep warm for 4.5 hours. When the melting time reaches two-thirds, air is introduced to increase the gas flow rate to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, clarifier, cerium oxide and lithium oxide is 10:0.7:0.4:0.4; the remaining steps are the same as Example 2.

[0039] Comparative Example 6: The difference between Comparative Example 6 and Example 2 is that step (1) is different. Step (1) is changed to: mix Glauber's salt, sodium chloride, tin oxide and carbon powder in a mass ratio of 2:0.5:0.9:5 to obtain a composite clarifier; mix the batch material, the composite clarifier, cerium oxide and lithium oxide, introduce ozone at 200 mL / s, and heat to 1650°C at 8°C / min to melt, and keep warm for 4.5 hours to obtain glass liquid; the mass percentages of the batch material components are 71.5% silicon dioxide, 1.5% aluminum oxide, 8.5% calcium oxide, 4.5% magnesium oxide, 6.6% potassium oxide and 7.4% sodium oxide; the mass ratio of the batch material, the composite clarifier, cerium oxide and lithium oxide is 10:0.7:0.4:0.4; the remaining steps are the same as Example 2.

[0040] Comparative Example 7: The difference between Comparative Example 7 and Example 2 is that step (3) is different, and step (3) is changed to: the intermediate A is placed in a vacuum degree of 4×10 -3Pa environment, introduce protective gas - argon to a gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to a gas pressure of 4.5kPa, and perform plasma etching with the following process parameters: microwave power of 700W, time of 30s, and temperature of 200°C. Then, introduce methane at 4mL / min, and maintain the gas pressure at 6kPa. The reaction is carried out for 40min to obtain high-transmittance photothermal glass. The remaining steps are the same as those in Example 2.

[0041] Comparative Example 8; The difference between Comparative Example 8 and Example 2 is that there is no step (3); the remaining steps are the same as Example 2.

[0042] Effect example

[0043] Table 1 below shows the performance analysis results of the high light transmittance photothermal glass using Examples 1 to 3 of the present invention and Comparative Examples 1 to 8.

[0044] Table 1

[0045]

[0046] From the comparison of the experimental data of the embodiment and the comparative example in Table 1, it can be found that the present invention utilizes ozone gas at a higher rate. When the batch material is converted into a glass melt, by increasing the ratio of wind in the combustion system and increasing the amount of gas used, the oxidation potential after combustion is enhanced, so that the inevitable very small amount of iron ions therein are oxidized to a trivalent state, the absorption of light is reduced to the greatest extent, and the light transmittance of the glass is enhanced. The added cerium oxide and lithium oxide make it easier for lithium ions to migrate in the matrix as the melting temperature increases. In addition, the small amount of cerium oxide melted at this time is located between the network gaps of the glass matrix, loosening and destroying its network structure, effectively reducing the viscosity of the glass liquid, increasing the buoyancy of the bubbles, and breaking away from the wrapping of the glass liquid, so that the glass reduces the scattering of light. As more and more bubbles are gradually discharged from the glass liquid, their specific gravity gradually increases, and they move downward under the action of gravity. Flowing, mixing and homogenization can improve the optical and mechanical uniformity of the glass, and improve the transmittance and mechanical properties. At this time, the melting amount of cerium oxide increases, which plays a gathering role in the glass network, reconnecting the non-bridging oxygen in the original glass network, and at the same time, lithium oxide fills the gaps between the network structure, thereby making the glass network structure more compact and improving the mechanical properties of the glass. Then, variable valence oxides and halides are used to replace part of the sodium sulfate as a composite clarifier. By expanding the clarification range of the glass, step-by-step clarification is achieved. At the same time, the gas flow rate is adjusted to appropriately increase the temperature difference between the upper and lower surfaces of the glass liquid and enhance the clarification effect. Then, it is etched by hydrogen plasma to produce nano-dents, and then methane is introduced to react with the surface of the glass substrate to generate silicon carbide, and diamond-like precipitation is performed to form a smooth and dense anti-reflection film, so that the substrate can achieve high transmittance and high mechanical properties.

[0047] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and range of equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing high-transmittance photothermal glass, characterized in that: The method comprises the following preparation steps: (1) Mix the batch material, composite clarifier, cerium oxide and lithium oxide, introduce ozone at 100-300 mL / s, heat and melt, and introduce air when the melting time reaches two-thirds, increase the gas flow rate, and obtain glass liquid; (2) pouring the glass liquid into a mold, performing annealing treatment, and then cooling it to room temperature in a furnace. Then, placing it in anhydrous ethanol and deionized water in turn, performing ultrasonic cleaning, and then blowing it dry with nitrogen to obtain an intermediate A. (3) Set the intermediate A to a vacuum degree of 4×10 -3 Pa environment, introduce protective gas - argon to a gas pressure of 0.3Pa, then introduce working gas - hydrogen at 100mL / min to a gas pressure of 3~6kPa for plasma etching, then introduce methane at 4mL / min and maintain the gas pressure at 4~8kPa, react for 20~60min, then carry out diamond-like deposition to obtain high-transmittance photothermal glass.

2. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The mass percentages of the ingredients in step (1) are silicon dioxide 71.5%, aluminum oxide 1.5%, calcium oxide 8.5%, magnesium oxide 4.5%, potassium oxide 6.6%, and sodium oxide 7.4%.

3. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The composite clarifier in step (1) is composed of mirabilite, sodium chloride, tin oxide and carbon powder in a mass ratio of 1-3:0.4-0.6:0.5-1:

5.

4. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: In step (1), the mass ratio of the batch material, the composite clarifier, the cerium oxide and the lithium oxide is 10:0.3~1:0.2~0.5:0.2~0.

5.

5. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The air flow rate in step (1) is 15-30 m / s.

6. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The melting process parameters of step (1) are as follows: heating rate of 3-10°C / min, temperature of 1450-1800°C, and holding time of 3-6h.

7. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The parameters of the annealing treatment in step (2) are: temperature of 400-700° C. and holding time of 0.5-2 h.

8. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The frequency of the ultrasound in step (2) is 21 kHz and the duration is 15 min.

9. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The process parameters of the plasma etching in step (3) are as follows: microwave power of 500-900 W, time of 20-60 s, and temperature of 100-300 °C.

10. The method for preparing a high light transmittance photothermal glass according to claim 1, characterized in that: The deposition temperature in step (3) is 400-700°C and the deposition time is 10-30 minutes.

Citation Information

Patent Citations

  • Method for producing low-iron high-pervious self-cleaning ultra-white rolling glass

    CN103073182A

  • Clarifying agent used for TFT-LCD substrate glass and preparation method thereof

    CN103408223A

  • Surface-coated glass, making method thereof, and solar module

    CN103570253A

  • Glass clarifying agent and method for preparing ultra-high aluminosilicate cover plate glass by using same

    CN112624603A

  • A high-transparency, wear-resistant, and light-transmitting material, its preparation method, and its application.

    CN114934264A