Method for blending combustion of sulfur slag in rotary kiln based on ardealite-to-sulfuric acid and cement co-production process
By mixing sulfur slag with silica and homogenizing it with phosphogypsum raw materials, calcining it in a rotary kiln, and using kiln gas to make sulfuric acid, the energy consumption and cost problems of sulfur slag absorption and sulfuric acid production of phosphogypsum combined with sulfuric acid are solved. Improved SO2 concentration and production efficiency.
Patent Information
- Application Number
- CN202411064066.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The technology of phosphogypsum sulfuric acid co-production cement produced by co-production of phosphogypsum has problems such as high energy consumption, low SO2 gas concentration, difficulty in handling sulfur slag and high production costs.
By mixing the broken sulfur slag with silica, finely crushed and screened, homogenized with phosphogypsum raw materials, calcined by rotary kilns, using sulfur-containing kiln gas as a preheating heat source and making sulfuric acid, reducing coal consumption and silica consumption .
It solves the problem of sulfur slag absorption, improves the SO2 concentration of kiln gas, reduces the coal consumption and silica consumption of clinker firing, and reduces production costs.
Smart Images

Figure CN118978352A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical industry, and in particular relates to a method for mixing sulfur slag with a rotary kiln in a process for producing sulfuric acid and cement from phosphogypsum. Background Art
[0002] The technology of producing sulfuric acid and cement from phosphogypsum is mainly used in phosphate fertilizer production enterprises. It mainly solves the problem of disposing of large amounts of phosphogypsum produced by wet phosphoric acid units in phosphate fertilizer enterprises. It produces concentrated sulfuric acid and silicate cement at the same time, which solves the problem of disposing of phosphogypsum and realizes the resource recovery of phosphogypsum.
[0003] However, the technology of producing sulfuric acid and cement from phosphogypsum also has the disadvantages of high energy consumption, low concentration of decomposed SO2 gas, high investment in supporting sulfuric acid equipment, high coal consumption for clinker burning, and excessively high production costs.
[0004] Sulfur slag is the waste residue produced by filtration of the sulfur melting process of the sulfuric acid plant. Its sulfur content is about 50% to 80%, and other impurities are calcium sulfate, diatomaceous earth, and inorganic salts. The accumulation of a large amount of sulfur slag will pollute the environment, and it is easy to burn when it comes into contact with a fire source, causing safety hazards. At present, it is more troublesome to handle sulfur slag, and most of them are sent out for treatment, but they need to pay the corresponding disposal fee. There are also factories that handle it themselves, but most of their processing equipment is expensive and requires a large investment, which is not practical. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a method for burning sulfur slag in a rotary kiln based on the process of producing sulfuric acid and cement from phosphogypsum. The method can not only solve the problem of sulfur slag disposal and recycle sulfur slag as a resource, but also increase the SO2 concentration of kiln gas when producing sulfuric acid and cement from phosphogypsum, while reducing the coal consumption in clinker burning and the consumption of silica, thereby reducing production costs.
[0006] The present invention provides a method for mixing sulfur slag in a rotary kiln based on a process for producing sulfuric acid and cement from phosphogypsum, comprising the following steps:
[0007] The sulfur slag is crushed and then mixed with silica to obtain a sulfur-silicon mixture;
[0008] The sulfur-silicon mixture is finely crushed and sieved, and then homogenized with phosphogypsum raw material to obtain a raw material mixture;
[0009] The raw material mixture is preheated and then calcined in a rotary kiln to obtain cement clinker; the sulfur-containing kiln gas generated during the calcination in the rotary kiln is used as a heat source for preheating and then sulfuric acid is produced.
[0010] Preferably, the specific process of the crushing includes: firstly using a roll crusher for coarse crushing, and then using a jaw crusher for medium crushing.
[0011] Preferably, the preheating method is five-stage preheating.
[0012] Preferably, the temperature of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 800-1100°C, and the temperature at the outlet of the first-stage preheater is ≤350°C.
[0013] Preferably, the SO2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 8.5-9.5 vol%, and the SO2 concentration at the outlet of the first-stage preheater is 9.5-10.5 vol%.
[0014] Preferably, the O2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 0.5-1.5 vol%, and the O2 concentration at the outlet of the first-stage preheater is 0.8-2 vol%.
[0015] Preferably, the temperature of the raw material mixture after preheating is ≥720°C.
[0016] Preferably, the particle size of the sulfur-silicon mixture after fine crushing and screening is 50 to 120 μm.
[0017] Preferably, the components of the sulfur slag include: 60-70wt% of elemental sulfur, 15-20wt% of calcium sulfate, 5-15wt% of diatomaceous earth and 1-5wt% of sodium sulfide.
[0018] Preferably, the raw material mixture comprises: 75-83wt% hemihydrate phosphogypsum, 1-5wt% silica, 2-10wt% sulfur slag, 1-5wt% bauxite and 3-5wt% coke.
[0019] Compared with the prior art, the present invention provides a method for mixing sulfur slag in a rotary kiln based on the process of producing sulfuric acid and cement from phosphogypsum, the method comprising the following steps: crushing the sulfur slag and mixing it with silica to obtain a sulfur-silicon mixture; finely crushing and screening the sulfur-silicon mixture and homogenizing it with phosphogypsum raw material to obtain a raw material mixture; preheating the raw material mixture and then calcining it in a rotary kiln to obtain cement clinker; the sulfur-containing kiln gas generated during the calcination of the rotary kiln is used as the heat source for the preheating and then sulfuric acid is produced. The method provided by the present invention has at least the following advantages:
[0020] (1) It can solve the problem of disposing of the waste sulfur slag generated in the sulfur melting process of sulfuric acid plants, and at the same time recycle sulfur, calcium and silicon, thus generating better economic benefits;
[0021] (2) It can reduce the coal consumption of cement clinker burning in the phosphogypsum sulfuric acid co-production cement plant, thereby reducing production costs;
[0022] (3) It can increase the SO2 concentration in the kiln gas of the phosphogypsum sulfuric acid and cement production plant, which is beneficial to the stable production of the acid production plant and reduces the investment in the acid production plant;
[0023] (4) It can reduce the silica consumption in the sulfuric acid and cement production plant of phosphogypsum, thereby reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0025] Figure 1 It is a process flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides a method for mixing sulfur slag in a rotary kiln based on a process for producing sulfuric acid and cement from phosphogypsum, comprising the following steps:
[0028] The sulfur slag is crushed and then mixed with silica to obtain a sulfur-silicon mixture;
[0029] The sulfur-silicon mixture is finely crushed and sieved, and then homogenized with phosphogypsum raw material to obtain a raw material mixture;
[0030] The raw material mixture is preheated and then calcined in a rotary kiln to obtain cement clinker; the sulfur-containing kiln gas generated during the calcination in the rotary kiln is used as a heat source for preheating and then sulfuric acid is produced.
[0031] In the method provided by the present invention, the sulfur slag comes from a sulfur melting process, and its components preferably include: 60-70wt% of elemental sulfur, 15-20wt% of calcium sulfate, 5-15wt% of diatomaceous earth and 1-5wt% of sodium sulfide; wherein the content of the elemental sulfur in the sulfur slag can be specifically 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 65.6wt%, 66wt%, 67wt%, 68wt%, 69wt% or 70wt%; the content of the calcium sulfate in the sulfur slag can be specifically 15wt%, 15.5wt%, 16wt%, 16. %, 5wt%, 17wt%, 17.5wt%, 18wt%, 18.5wt%, 19wt%, 19.5wt% or 20wt%; the content of diatomaceous earth in the sulfur slag can be specifically 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 9.65wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%; the content of sodium sulfide in the sulfur slag can be specifically 1wt%, 1.5wt%, 2wt%, 2.3wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%.
[0032] In the method provided by the present invention, the specific process of crushing preferably includes: firstly using a roll crusher for coarse crushing, and then using a jaw crusher for medium crushing.
[0033] In the method provided by the present invention, sulfur slag and silica are mixed, which can solve the ignition problem of sulfur slag in the subsequent fine crushing process.
[0034] In the method provided by the present invention, the particle size of the sulfur-silicon mixture after fine crushing and screening is preferably 50-120 μm, specifically 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 105 μm, 110 μm, 115 μm or 120 μm.
[0035] In the method provided by the present invention, the components of the raw material mixture include: 75-83wt% of hemihydrate phosphogypsum, 1-5wt% of silica, 2-10wt% of sulfur slag, 1-5wt% of bauxite and 3-5wt% of coke; wherein the content of the hemihydrate phosphogypsum in the raw material mixture can be specifically 75wt%, 75.5wt%, 76wt%, 76.5wt%, 77wt%, 77.5wt%, 78wt%, 78.5wt%, 79wt%, 79.5wt%, 80wt%, 80.5wt%, 81wt%, 81.5wt%, 82wt%, 82.5wt% or 83wt%; the content of the silica in the raw material mixture can be specifically 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%. %, 4.5wt% or 5wt%; the content of the sulphur slag in the raw meal mixture can specifically be 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%; the content of bauxite in the raw meal mixture can specifically be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%; the content of the coke in the raw meal mixture can specifically be 3wt%, 3.2wt%, 3.5wt%, 3.7wt%, 4wt%, 4.2wt%, 4.5wt%, 4.7wt% or 5wt%.
[0036] In the method provided by the present invention, the preheating method is preferably five-stage preheating, that is, the raw material mixture is preheated in the first stage preheater, the second stage preheater, the third stage preheater, the fourth stage preheater and the fifth stage preheater in sequence.
[0037] In the method provided by the present invention, the heat source for preheating is the sulfur-containing kiln gas generated during the calcination process of the rotary kiln. For the technical scheme of adopting five-stage preheating, the flow direction of the sulfur-containing kiln gas in the five-stage preheater is opposite to the moving direction of the raw material mixture, and they are in countercurrent contact, that is, the sulfur-containing kiln gas flows through the fifth-stage preheater, the fourth-stage preheater, the third-stage preheater, the second-stage preheater and the first-stage preheater in sequence; wherein, the temperature of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is preferably 800-1100°C, and the temperature at the outlet of the first-stage preheater is preferably ≤350°C; the SO2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is preferably 8.5-9.5vol%, and the SO2 concentration at the outlet of the first-stage preheater is preferably 9.5-10.5vol%; the O2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is preferably 0.5-1.5vol%, and the O2 concentration at the outlet of the first-stage preheater is preferably 0.8-2vol%.
[0038] In the method provided by the present invention, during the preheating process, the temperature of the sulfur slag gradually increases. When entering the fourth preheater, its temperature is preferably ≥480°C, which is higher than the ignition point of sulfur. The contained elemental sulfur burns to generate SO2, so the elemental sulfur is removed and will not enter the rotary kiln. In the present invention, an oxygen supplement port is preferably designed at the kiln gas inlet end of the fifth stage preheater to ensure that the elemental sulfur in the sulfur slag is completely burned.
[0039] In the method provided by the present invention, the temperature of the raw material mixture after preheating is preferably ≥ 720°C. In the present invention, after the raw material mixture is preheated, the elemental sulfur in the sulfur slag is completely burned, and the remaining calcium and silicon enter the rotary kiln. The calcium and silicon have time and space to be fully mineralized in the rotary kiln, and the quality of the clinker is not affected while calcium and silicon are supplemented.
[0040] In the method provided by the present invention, the sulfur-containing kiln gas used as a heat source is transported to an acid-making device to produce sulfuric acid. In the present invention, an oxygen concentration detection instrument is preferably provided on the gas pipeline before the sulfur-containing kiln gas enters the acid-making device to ensure that the supplemented oxygen is sufficient. In the present invention, a SO2 detection instrument is preferably provided on the gas pipeline before the sulfur-containing kiln gas enters the acid-making device, and the blending amount and oxygen supplementation amount can be adjusted in real time according to the SO2 concentration.
[0041] The method provided by the present invention can not only solve the problem of sulfur slag disposal and recycle sulfur slag, but also improve the SO2 concentration of kiln gas when phosphogypsum is used to produce sulfuric acid and cement, while reducing the coal consumption of clinker burning and the consumption of silica, thereby reducing production costs.
[0042] For the purpose of greater clarity, the invention is described in detail through the following examples.
[0043] Example 1
[0044] A method for mixing and burning sulfur slag in a rotary kiln based on a process for producing sulfuric acid and cement from phosphogypsum, including: a mixing and burning batching scheme, a mixing and burning process flow and process indicators, which are specifically described as follows:
[0045] (I) Blending and mixing scheme:
[0046] A 300,000 tons / year phosphogypsum-based sulfuric acid and 400,000 tons / year cement plant uses industrial waste phosphogypsum to produce sulfuric acid and cement. It uses phosphogypsum, silica, and bauxite as ingredients, combined with coke powder as a reducing agent, and uses bituminous coal as a burning fuel. The clinker rate and mineral composition are appropriate, which can meet the requirements of new dry-process cement production and produce high-quality silicate cement clinker.
[0047] The raw material formula and indicators are as follows:
[0048] (1) Raw material ratio
[0049]
[0050] (2) Clinker target rate value:
[0051] Saturation ratio KH = 0.8 ± 0.30;
[0052] Silicic acid rate SM = 3.15 ± 0.25;
[0053] Aluminate rate IM = 2.0 ± 0.30;
[0054] Carbon-sulfur ratio C / SO3=0.65±0.15.
[0055] (3) Heat consumption of clinker burning: 5439 kJ / kg (1300 kcal / kg).
[0056] (4) Amount of coal ash added: 3.50%.
[0057] (5) SO2 concentration in kiln gas: 8% to 8.5%.
[0058] (6) Raw material temperature entering the kiln: ≥650℃.
[0059] (7) Coal consumption for clinker burning: 0.186kgce / kg.
[0060] The components of sulfur slag produced by the sulfur melting process of a sulfur acid plant with an annual sulfur production capacity of 800,000 tons are as follows:
[0061]
[0062] According to the sulfur slag composition and the clinker rate requirements of the phosphogypsum sulfuric acid co-production cement unit, the blending formula is designed as shown in the following table:
[0063]
[0064] The clinker indicators obtained according to the sulfur slag blending formula are as follows
[0065] (1) Clinker rate value:
[0066] Saturation ratio KH = 0.8 ± 0.20;
[0067] Silicic acid rate SM = 3.15 ± 0.05;
[0068] Aluminate rate IM = 2.0 ± 0.10;
[0069] Carbon-sulfur ratio C / SO3=0.65±0.15,
[0070] (2) Heat consumption of clinker burning: 5266 kJ / kg (1260 kcal / kg).
[0071] (3) Amount of fly ash added: 2.8% to 3.00%.
[0072] (4) Raw material temperature entering the kiln: ≥720℃.
[0073] (5) SO2 concentration in kiln gas: 9.5%~10.5%.
[0074] (6) Coal consumption for clinker burning: 0.180kgce / kg.
[0075] According to the formula of the rotary kiln blended with sulfur slag, the clinker index, clinker rate value and mineral composition are suitable, which can meet the requirements of new dry process cement production and produce high-quality silicate cement clinker. After blending with sulfur slag, the SO2 concentration in the kiln gas increases by 1%, the raw material temperature entering the kiln increases by 70℃, the coal consumption for clinker burning decreases by about 3%, and the silica consumption can be reduced by up to 4%.
[0076] (II) Blending process flow:
[0077] The process flow of blending is as follows: Figure 1 As shown, specifically: the sulfur slag from the sulfur melting process of the sulfur-fired acid-making device is in blocks of different sizes, and is first coarsely crushed and medium-crushed in sequence by a roll crusher and a jaw crusher; the sulfur slag after medium crushing is sent to the joint warehouse of the phosphogypsum acid-making and cement-making device, and is blended with silica in proportion, and the blended mixture is sent to the mixing mill for fine crushing; the finely crushed mixture is sent to the homogenization warehouse and the phosphogypsum raw meal for homogenization; the homogenized sulfur slag and the raw meal are evenly mixed, and are preheated in a five-stage preheater (the first stage preheater, the second stage preheater, the third stage preheater, the fourth stage preheater and the fifth stage preheater arranged in series) and then enter the rotary kiln for calcination; the sulfur-containing kiln gas generated during the calcination process of the rotary kiln is used as the heat source of the five-stage preheater, and is then transported to the acid-making device to make sulfuric acid; the cement clinker obtained after calcination in the rotary kiln is removed from the grate cooler.
[0078] In the above process flow of this embodiment, during the preheating process, the temperature of the sulfur slag gradually increases. When entering the fourth preheater, the temperature is greater than 480°C. The temperature of the sulfur slag is higher than the ignition point of sulfur. The elemental sulfur contained in it burns to generate SO2, so the elemental sulfur is removed.
[0079] In the above process flow of this embodiment, the rotary kiln head is designed with an oxygen supply port, which uses negative pressure to supply air to the kiln gas inlet end of the fifth-stage preheater to supplement the oxygen required for the combustion of sulfur slag.
[0080] In the above process flow of this embodiment, the kiln gas from the rotary kiln is sequentially heat exchanged through a five-stage preheater, gradually cooled from 800°C to 1100°C to below 350°C, passes through an induced draft fan, and enters the acid making device after dust removal.
[0081] In the above process flow of this embodiment, the sulfur slag is burned in the 4th and 5th stage preheaters, so that the SO2 concentration of the kiln gas entering the acid-making device is further increased, thereby increasing the production capacity of the sulfuric acid device and reducing the investment in the sulfuric acid device. Because the sulfur slag is burned and releases heat, the temperature of the raw material entering the rotary kiln head is further increased, thereby reducing the coal consumption of clinker burning.
[0082] In the above process flow of the present embodiment, an oxygen supply port is designed at the kiln gas inlet end of the fifth-stage preheater to ensure complete combustion of elemental sulfur in the sulfur slag.
[0083] In the above process flow of this embodiment, a SO2 detection instrument is designed before the kiln gas enters the acid-making device, and the mixing amount and oxygen supplement amount can be adjusted in real time according to the SO2 concentration.
[0084] (III) Process indicators:
[0085] 1. Kiln gas temperature:
[0086] (1) Kiln gas temperature at the inlet of the fifth stage preheater: 800℃~1100℃;
[0087] (2) Kiln gas temperature at the outlet of the first stage preheater: ≤350℃.
[0088] 2. SO2 concentration in kiln gas:
[0089] (1) SO2 concentration of kiln gas at the inlet of the fifth stage preheater: 8.5% to 9.5%;
[0090] (2) SO2 concentration of kiln gas at the outlet of the first stage preheater: 9.5%~10.5%.
[0091] 3. Kiln gas O2 concentration:
[0092] (1) O2 concentration of kiln gas at the inlet of the fifth stage preheater (before oxygen supplementation): 0.5% to 1.5%;
[0093] (2) O2 concentration of kiln gas at the outlet of the first stage preheater: 0.8%~2%.
[0094] 4. Raw material temperature:
[0095] Raw material temperature entering kiln: ≥720℃.
[0096] 5. Granularity:
[0097] The fine particle size of the sulfur slag and silica mixture is 50μm~120μm.
[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for burning sulfur slag in a rotary kiln based on the process of producing sulfuric acid and cement from phosphogypsum, characterized in that: The following steps are involved: The sulfur slag is crushed and then mixed with silica to obtain a sulfur-silicon mixture; The sulfur-silicon mixture is finely crushed and sieved, and then homogenized with phosphogypsum raw material to obtain a raw material mixture; The raw material mixture is preheated and then calcined in a rotary kiln to obtain cement clinker; the sulfur-containing kiln gas generated during the calcination in the rotary kiln is used as a heat source for preheating and then sulfuric acid is produced.
2. The method according to claim 1, characterized in that The specific process of the crushing includes: firstly using a roll crusher for coarse crushing, and then using a jaw crusher for medium crushing.
3. The method according to claim 1, characterized in that The preheating method is five-stage preheating.
4. The method according to claim 3, characterized in that The temperature of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 800-1100°C, and the temperature at the outlet of the first-stage preheater is ≤350°C.
5. The method according to claim 3, characterized in that: The SO2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 8.5-9.5 vol%, and the SO2 concentration at the outlet of the first-stage preheater is 9.5-10.5 vol%.
6. The method according to claim 3, characterized in that The O2 concentration of the sulfur-containing kiln gas at the inlet of the fifth-stage preheater is 0.5-1.5 vol%, and the O2 concentration at the outlet of the first-stage preheater is 0.8-2 vol%.
7. The method according to claim 1, characterized in that The temperature of the raw material mixture after preheating is ≥720°C.
8. The method according to claim 1, characterized in that The particle size of the sulfur-silicon mixture after fine crushing and screening is 50-120 μm.
9. The method according to claim 1, characterized in that: The components of the sulfur slag include: 60-70wt% of elemental sulfur, 15-20wt% of calcium sulfate, 5-15wt% of diatomaceous earth and 1-5wt% of sodium sulfide.