Hydroxyl acrylate resin and preparation method thereof

By preparing a long-chain hydroxyacrylate resin, the problem of insufficient flexibility caused by the improvement of drying properties of existing quick-drying repair paints is solved, and the combination of high-active hydroxyl and long-chain structure is achieved, and the drying rate of the paint film is improved. and flexibility ensures the impact resistance of the paint film.

CN118978632AActive Publication Date: 2024-11-19WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411130566.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
2044-08-16

Smart Images

  • Figure BDA0004997695780000051
    Figure BDA0004997695780000051
  • Figure BDA0004997695780000061
    Figure BDA0004997695780000061
Patent Text Reader

Abstract

The invention provides a method for preparing hydroxyl acrylate resin, the hydroxyl acrylate resin obtained by the method, and a coating prepared from the hydroxyl acrylate resin. The method comprises the following steps: a) adding CnH2n (OH) 2 into a reactor, heating to 50-100 DEG C, slowly adding a functional monomer containing an isocyanate group, reacting, reacting until the content of NCO is less than 0.1% after charging is completed, and cooling to obtain a long-chain-segment hydroxyl monomer; b) adding an organic solvent into the reactor, heating and refluxing, dropwise adding a mixed solution of an acrylate monomer, an acrylic monomer, styrene, a long-chain-segment hydroxyl monomer and an initiator in an inert atmosphere, and reacting at 70-130 DEG C, n = 4-8, and the isocyanate group-containing functional monomer contains carbon-carbon double bonds. A coating prepared from the hydroxyl acrylate resin has excellent quick-drying property, and a formed coating film has excellent flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of polymers, and specifically relates to a method for preparing a hydroxy acrylate resin, a hydroxy acrylate resin obtained by the method, and a coating prepared from the hydroxy acrylate resin. The coating prepared from the hydroxy acrylate resin has excellent quick-drying properties, and the formed coating film has excellent flexibility. Background Art

[0002] With the development of China's economy and the improvement of domestic consumption capacity, the market for vehicles manufactured in China has expanded, especially the rapid development of electric vehicles. The number of vehicles has increased, and the speed of road development has increased. The number of accidents has increased, and the demand for paint repair has increased. The demand for quick repair has also increased. However, at present, quick-drying repair paints often need to use expensive special isocyanate curing agents to provide quick-drying properties, or use hard resins to improve drying properties, but this often leads to insufficient flexibility, and there are risks of subsequent cracking and poor impact resistance.

[0003] These have limited the development of the quick repair paint market to a certain extent, and new raw materials need to be developed to further improve these situations. Summary of the invention

[0004] The present invention aims to provide a hydroxy acrylate resin and a preparation method thereof.

[0005] The present invention is achieved through the following technical solutions:

[0006] According to a first aspect of the present invention, there is provided a method for preparing a hydroxy acrylate resin, comprising the following steps:

[0007] a) Long chain segment diol C n H 2n (OH)2 is added to the reactor, heated to 50-100°C, and the functional monomer containing isocyanate group is slowly added and reacted. After the addition is completed, the reaction is carried out until the NCO content is less than 0.1%, and the long-chain hydroxyl monomer is obtained by cooling;

[0008] b) adding an organic solvent into the reactor and heating it to reflux, and in an inert atmosphere, dropwise adding a mixture of acrylate monomer, acrylic acid monomer, styrene, long-chain hydroxyl monomer and initiator, the reaction temperature being 70-130° C.,

[0009] Wherein, n=4-8, the functional monomer containing an isocyanate group contains a carbon-carbon double bond,

[0010] The molar ratio of the long-chain segment diol to the functional monomer containing an isocyanate group is 1:0.9-1.

[0011] The mass ratio of acrylate monomer: acrylic acid monomer: styrene monomer: long-chain hydroxyl monomer: solvent is 25-50: 0.5-4: 4-20: 20-50: 20-40.

[0012] Preferably, the functional monomer containing an isocyanate group is one or more selected from the group consisting of isocyanate ethyl acrylate, isocyanate ethyl methacrylate and 2-(2-isocyanateethoxy)ethyl methacrylate.

[0013] Preferably, the acrylic acid monomer is one or more selected from acrylic acid and methacrylic acid.

[0014] Preferably, the acrylic acid ester monomer is one or more selected from methyl acrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate and isobutyl methacrylate.

[0015] Preferably, the solvent is one or more of ethyl acetate, butyl acetate, sec-butyl acetate, toluene and xylene.

[0016] The initiator is a free radical initiator. Preferably, the initiator is one or more selected from azobisisobutyronitrile, benzoyl peroxide, tert-butyl pivaloyl peroxide, tert-butyl benzoyl peroxide and potassium persulfate.

[0017] Preferably, the mass ratio of the initiator: (monomer+solvent) is 0.5-4:100.

[0018] Preferably, in step b), the mixed solution is added dropwise for 120 to 300 minutes, and the reaction is kept warm for 60 to 300 minutes.

[0019] According to a second aspect of the present invention, a hydroxy acrylate resin is provided, which is prepared by the method for preparing a hydroxy acrylate resin according to the present invention.

[0020] According to a third aspect of the present invention, a coating is provided, which comprises the hydroxy acrylate resin according to the present invention.

[0021] Beneficial Effects

[0022] The polyacrylate prepared by the method according to the present invention introduces long-chain and highly active hydroxyl groups. On the one hand, the highly active hydroxyl groups increase the drying rate of the paint film to achieve quick-drying performance. On the other hand, the long chains increase the flexibility of the paint film to ensure that the paint film is not easy to crack after drying and is more resistant to impact. DETAILED DESCRIPTION

[0023] The hydroxy acrylate resin and its preparation method described in the present invention are further described below in conjunction with specific implementation examples. It should be understood that the embodiments given in the present invention are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0024] The raw materials and sources of this embodiment are as follows:

[0025] Acrylic acid monomer: methacrylic acid-Wanhua Chemical, acrylic acid-alfa.

[0026] Acrylate monomers: methyl methacrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate—alfa.

[0027] Functional monomers containing isocyanate: isocyanate ethyl acrylate, isocyanate ethyl methacrylate, 2-(2-isocyanateethoxy)ethyl methacrylate—adamas.

[0028] Initiator: azobisisobutyronitrile, benzoyl peroxide—aladdin; dibenzoyl peroxide, potassium persulfate—sigma-aldrich.

[0029] Solvent: ethyl acetate, butyl acetate, sec-butyl acetate, toluene, xylene - Sinopec.

[0030] Example 1

[0031] a) adding 1180 g (10 mol) of hexanediol into a reactor, heating to 70° C., slowly adding 1410 g (10 mol) of ethyl isocyanate acrylate to react, and reacting until the NCO content is less than 0.1% after the addition is completed, cooling and discharging to obtain a long-chain hydroxyl monomer I;

[0032] b) Add 100g butyl acetate and 100g xylene into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g methyl acrylate, 50g butyl acrylate, 10g acrylic acid, 40g styrene, 500g long-chain hydroxyl monomer I and 40g initiator azobisisobutyronitrile, the reaction temperature is 70°C, the dropping time is 300min, the reaction is kept warm for 60min, and the material is cooled and discharged.

[0033] Example 2

[0034] a) adding 1180 g (10 mol) of hexanediol into a reactor, heating to 70° C., slowly adding 1269 g (9 mol) of ethyl isocyanate acrylate to react, and reacting until the NCO content is less than 0.1% after the addition is completed, cooling and discharging to obtain a long-chain hydroxyl monomer II;

[0035] b) Add 100g butyl acetate and 100g xylene into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g methyl acrylate, 50g butyl acrylate, 10g acrylic acid, 40g styrene, 500g long-chain hydroxyl monomer II and 40g initiator azobisisobutyronitrile, the reaction temperature is 70°C, the dropping time is 300min, the reaction is kept warm for 60min, and the material is cooled and discharged.

[0036] Example 3

[0037] a) adding 1460 g (10 mol) of octanediol into a reactor, heating to 50° C., slowly adding 1470 g (9.48 mol) of ethyl isocyanate methacrylate to react until the NCO content is less than 0.1%, and cooling the discharged material to obtain a long-chain hydroxyl monomer III;

[0038] b) Add 200g of sec-butyl acetate and 100g of toluene into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g of methyl methacrylate, 60g of butyl methacrylate, 40g of methacrylic acid, 200g of styrene, 200g of long-chain hydroxyl monomer III and 20g of initiator benzoyl peroxide, the reaction temperature is 100°C, the dropping time is 120min, the reaction is kept warm for 300min, and the material is cooled and discharged.

[0039] Example 4

[0040] a) adding 900 g (10 mol) of butanediol into a reactor, heating to 100° C., slowly adding 1990 g (10 mol) of 2-(2-isocyanateethoxy)ethyl methacrylate to react, reacting until the NCO content is less than 0.1% after the addition is completed, cooling and discharging to obtain a long-chain hydroxyl monomer IV;

[0041] b) Add 300g of xylene and 100g of ethyl acetate into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g of methyl methacrylate, 100g of ethyl methacrylate, 5g of methacrylic acid, 40g of styrene, 255g of long-chain hydroxyl monomer IV and 5g of initiator potassium persulfate, the reaction temperature is 130°C, the dropping time is 210min, the reaction is kept warm for 180min, and the material is cooled and discharged.

[0042] Example 5

[0043] a) adding 900 g (10 mol) of butanediol into a reactor, heating to 100° C., slowly adding 1410 g (10 mol) of ethyl isocyanate acrylate to react, reacting until the NCO content is less than 0.1% after the addition is completed, cooling and discharging to obtain a long-chain hydroxyl mono-V;

[0044] b) Add 250g of butyl acetate into the reactor, raise the temperature to reflux, introduce nitrogen protection, dropwise add a mixture of 400g of methyl acrylate, 100g of isobutyl acrylate, 5g of acrylic acid, 40g of styrene, 205g of long-chain hydroxyl monomer V and 10g of initiator azobisisobutyronitrile, the reaction temperature is 80°C, the dropping time is 210min, the reaction is kept warm for 180min, and the material is cooled and discharged.

[0045] Comparative Example 1

[0046] Commercially available resin ACR6875-Tongde resin.

[0047] Comparative Example 2

[0048] Add 250g of butyl acetate into the reactor, heat and reflux, pass nitrogen protection, add dropwise a mixture of 400g of methyl acrylate, 100g of isobutyl acrylate, 5g of acrylic acid, 40g of styrene, 205g of hydroxyethyl acrylate and 10g of initiator azobisisobutyronitrile, the reaction temperature is 80°C, the dropping time is 210min, keep the reaction warm for 180min, add additional solvent, cool and discharge.

[0049] Comparative Example 3

[0050] a) adding 1180 g (10 mol) of hexanediol into a reactor, heating to 70° C., slowly adding 1130 g (8 mol) of ethyl isocyanate acrylate to react, and reacting until the NCO content is less than 0.1% after the addition is completed, cooling and discharging to obtain a long-chain hydroxyl monomer VI;

[0051] b) Add 100g of butyl acetate and 100g of xylene into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g of methyl acrylate, 50g of butyl acrylate, 10g of acrylic acid, 40g of styrene, 500g of long-chain hydroxyl monomer VI and 40g of initiator azobisisobutyronitrile, the reaction temperature is 70°C, the dropping time is 300min, the reaction is kept warm for 60min, and the material is cooled and discharged.

[0052] Comparative Example 4

[0053] a) 1180 g (10 mol) of hexanediol was added to a reactor, heated to 70° C., 1550 g (11 mol) of ethyl isocyanate acrylate was slowly added to react until the NCO content was less than 0.1%, and the product was cooled and discharged to obtain a long-chain hydroxy mono-VII;

[0054] b) Add 100g of butyl acetate and 100g of xylene into the reactor, heat and reflux, introduce nitrogen protection, dropwise add a mixture of 200g of methyl acrylate, 50g of butyl acrylate, 10g of acrylic acid, 40g of styrene, 500g of long-chain hydroxyl monomer VII and 40g of initiator azobisisobutyronitrile, the reaction temperature is 70°C, the dropping time is 300min, the reaction is kept warm for 60min, and the material is cooled and discharged.

[0055] The above resin and curing agent are prepared into a two-component varnish according to the following formula, as shown in Table 1.

[0056] Table 1: Main paint components and curing agent components

[0057]

[0058] Among them, HT-100 is HDI trimer, Wanhua Chemical;

[0059] IT-170B is IPDI trimer, Wanhua Chemical;

[0060] Additive TI is a dehydrating agent, Borchers.

[0061] The main paint component contains hydroxyl groups, while the curing agent component contains isocyanate groups. The coating is formulated by weighing the main paint component and the curing agent component at a molar ratio of NCO:OH of 1.2:1.

[0062] During the test, the main paint component and curing agent were mixed evenly, and after standing for 15 minutes, the above paint was heated to 100g / m 2 The coating was sprayed onto the tinplate with primer for performance testing.

[0063] Table 2: Performance test results of Examples 1 to 5 and Comparative Examples 1 to 4

[0064]

[0065] Surface drying time: Touch the surface of the paint film with your finger. When there is no paint adhering to your finger, the surface is considered dry and the recorded time is the surface drying time.

[0066] Finger-pressure drying time: Press the surface of the paint film hard with your thumb. If there are no fingerprints or marks, the time recorded is the finger-pressure drying time.

[0067] Pencil hardness test standard: GB / T 6739-2006;

[0068] Pendulum hardness test standard: GB / T 1730-2007;

[0069] Flexibility test standard: GB / T 6742-2007;

[0070] Impact test standard: GB / T 1732-2020;

[0071] Adhesion test standard: GB / T 9286-2021;

[0072] Recoating means spraying another layer on the original coating and then testing the adhesion. This is to examine the adhesion between coatings. This test is more stringent than the conventional adhesion test.

[0073] As shown in Table 2, Examples 1 to 5 have excellent drying rate, flexibility and impact resistance. Comparative Examples 1 and 2 have average drying properties, and average flexibility and impact resistance; Comparative Example 3 has too much small molecule alcohol and low drying properties; Comparative Example 4 has excessive carbon-carbon double bonds due to excessive isocyanate-containing functional monomers, resulting in excessive crosslinking, and the product is in a gel state and cannot be used.

Claims

1. A method for preparing a hydroxy acrylate resin, comprising the following steps: a) Long chain segment diol C n H 2n (OH)2 is added to the reactor, heated to 50-100°C, and the functional monomer containing isocyanate group is slowly added and reacted. After the addition is completed, the reaction is carried out until the NCO content is less than 0.1%, and the long-chain hydroxyl monomer is obtained by cooling; b) adding an organic solvent into the reactor and heating it to reflux, and in an inert atmosphere, dropwise adding a mixture of acrylate monomer, acrylic acid monomer, styrene, long-chain hydroxyl monomer and initiator, the reaction temperature being 70-130° C., Wherein, n=4-8, the functional monomer containing an isocyanate group contains a carbon-carbon double bond, The molar ratio of the long-chain segment diol to the functional monomer containing an isocyanate group is 1:0.9-1. The mass ratio of acrylate monomer: acrylic acid monomer: styrene monomer: long-chain hydroxyl monomer: solvent is 25-50: 0.5-4: 4-20: 20-50: 20-40.

2. The method for preparing a hydroxy acrylate resin according to claim 1, wherein: The functional monomer containing an isocyanate group is one or more selected from the group consisting of isocyanate ethyl acrylate, isocyanate ethyl methacrylate and 2-(2-isocyanate ethoxy)ethyl methacrylate.

3. The method for preparing a hydroxy acrylate resin according to claim 1 or 2, wherein: The acrylic acid monomer is one or more selected from acrylic acid and methacrylic acid.

4. The method for preparing a hydroxy acrylate resin according to any one of claims 1 to 3, wherein: The acrylic acid ester monomer is one or more selected from the group consisting of methyl acrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate and isobutyl methacrylate.

5. The method for preparing a hydroxy acrylate resin according to any one of claims 1 to 4, wherein: The solvent is one or more of ethyl acetate, butyl acetate, sec-butyl acetate, toluene and xylene; and / or The initiator is a free radical initiator.

6. The method for preparing a hydroxy acrylate resin according to any one of claims 1 to 5, wherein: The initiator is one or more selected from azobisisobutyronitrile, benzoyl peroxide, tert-butyl pivaloyl peroxide, tert-butyl benzoyl peroxide and potassium persulfate.

7. The method for preparing a hydroxy acrylate resin according to any one of claims 1 to 6, wherein: The mass ratio of initiator: (monomer + solvent) is 0.5-4:

100.

8. The method for preparing a hydroxy acrylate resin according to any one of claims 1 to 7, wherein: In step b), the mixed solution is added dropwise for 120 to 300 minutes, and the reaction is kept warm for 60 to 300 minutes.

9. A hydroxy acrylate resin prepared by the method according to any one of claims 1 to 8. 10 . A coating comprising the hydroxy acrylate resin according to claim 9 .

Citation Information

Patent Citations

  • Hydroxy acrylic resin with high reactive activity and preparation method and application thereof

    CN102181007A

  • Hydroxyl acrylic resin for low-temperature fast-dry type varnish and preparation method and application thereof

    CN107082843A

  • Thermosetting acrylic resin with high hardness and deep-drawing resistance, and synthetic method and application thereof

    CN109053947A

  • Hydroxy acrylic acid dispersion composition for water-based amino baking varnish and preparation method thereof

    CN111732686A

  • Preparation method for high-solid acrylic resin

    US20190389990A1