Environment-friendly mine road dust suppressant and preparation method thereof
Environmentally friendly mining road dust suppressors prepared through copolymerization reactions of starch, acrylamide, maleic anhydride and other materials have solved the problems of short acting time and secondary pollution of existing dust suppressors, and achieved efficient, environmentally friendly and low-cost dust discharge. Suppress the effect and provide curing effect after multiple sprays.
Patent Information
- Application Number
- CN202411063112.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing mine road dust suppressors have short working time, poor cementing and curing effects, secondary environmental pollution and high usage costs, and traditional methods such as sprinkling water and dust suppressors have insufficient environmental protection.
An environmentally friendly mining road dust inhibitor is prepared by copolymerization reaction using starch, acrylamide, maleic anhydride and other materials. Ester monomer compounds and catalysts are added, and the reaction is stirred under mild conditions through copolymerization reaction to prepare a colorless and viscous As a dust inhibitor.
The prepared dust inhibitor has an efficient dust suppression effect, is stable for a long time, is cheap and has strong biodegradability. It has a certain curing effect after multiple sprays, making it suitable for continuous large-scale production.
Smart Images

Figure CN118978640A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dust suppression sprays, and in particular to an environmentally friendly mine road dust suppressant and a preparation method thereof. Background Art
[0002] Dust has become one of the world's biggest public hazards. With the vigorous development of open-pit mines, dust pollution on production surfaces and transportation roads is becoming increasingly serious, which not only pollutes the surrounding environment and destroys the ecosystem; it also harms the health of workers and increases the risk of pneumoconiosis.
[0003] At present, dust suppression on mine roads at home and abroad can be divided into two methods: water sprinkling and chemical dust suppressants. Water sprinkling is a traditional method of road dust suppression. Water sprinkling can moisten fine dry dust particles, increase the moisture content of dust, and prevent it from flying under the action of external force. However, the time of water sprinkling is short, and it needs to be sprayed repeatedly and a lot of labor is invested every day. Chemical dust suppressants include wetting dust suppressants, bonding dust suppressants and condensing dust suppressants, such as surfactants (sodium dodecylbenzene sulfonate, stearic acid, lauric acid, etc.) + hygroscopic inorganic salts (NaCl, MgCl2, CaCl2, Na2CO3, Na2SiO3, etc.) Wetting dust suppressants. Surfactants can reduce the surface tension of water and enhance the wetting effect of water on dust, while hygroscopic inorganic salts can make up for the shortcomings of surfactants in moisture absorption and water retention, and strengthen the role of surfactants, but they have the disadvantages of short action time, large usage, and limited dust suppression effect. Asphalt, coal tar, paraffin oil, heavy oil and other oil-based dust suppressants are first emulsified to obtain an emulsion, and then the emulsion is sprayed to bond with dust particles to achieve the purpose of dust suppression. However, oil-based dust suppressants cannot be naturally degraded, and there is a secondary environmental pollution problem. Highly absorbent resin (sodium polyacrylate, polyvinyl alcohol) condensation-type dust suppressants absorb moisture from the air to increase the moisture content of dust, thereby achieving a dust suppression effect. It has the advantages of stable chemical properties, non-toxicity, strong hydrophilicity, and degradability, but it has the disadvantages of high preparation cost and difficulty, high price, and high use cost. Therefore, it is urgent to develop an economical, practical, efficient and environmentally friendly dust suppressant for mine roads. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention aims to provide an environmentally friendly mine road dust suppressant and a preparation method thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing an environmentally friendly mine road dust suppressant, the specific process is as follows:
[0007] Starch, acrylamide and maleic anhydride are mixed and dissolved in water, alkali is added to adjust the pH to 6-7, and an ester monomer compound and a catalyst are added. The mixture is stirred and reacted at 30-50° C. for 3-6 hours to obtain a colorless viscous liquid, which is an environmentally friendly mine road dust suppressant.
[0008] Furthermore, the alkali is one or both of sodium hydroxide and potassium hydroxide.
[0009] Furthermore, the ester monomer compound is one or more of ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate.
[0010] Furthermore, the catalyst is at least one of potassium persulfate, ammonium persulfate, and azobisisobutyronitrile.
[0011] Furthermore, the weight proportions of water, starch, acrylamide, maleic anhydride, alkali, ester monomer compound and catalyst are respectively 73-80 parts of water, 7-12 parts of starch, 8-12 parts of acrylamide, 0.5-2 parts of maleic anhydride, 0.6-2.1 parts of alkali, 0.3-0.8 parts of ester monomer compound and 0.1-0.2 parts of catalyst.
[0012] The present invention also provides an environmentally friendly mine road dust suppressant prepared by the preparation method.
[0013] The beneficial effects of the present invention are:
[0014] 1. The present invention uses cheap starch, acrylamide and maleic anhydride as main reaction monomer raw materials to prepare a highly efficient and environmentally friendly dust suppressant through copolymerization, which solves the problems of short action time, poor cementation and curing effect, secondary environmental pollution and high use cost of existing mine road dust suppressants;
[0015] 2. The preparation method of the present invention is simple and easy to operate, easy to operate and control, has little dependence on equipment, mild reaction conditions and no three wastes are discharged, is suitable for continuous large-scale production, and has high promotion and application value.
[0016] 3. The present invention uses starch as the hydrophilic main chain, introduces different grafting monomers and hydrophilic functional groups, and synthesizes highly water-absorbing environmentally friendly dust inhibitors through free radical initiation catalysis. There are a large number of carboxyl (-COOH), hydroxyl (-OH) and amide (-CONH2) hydrophilic functional groups on the molecular chain, which can absorb moisture in the air. At the same time, the charged groups can capture particulate dust and adsorb its particles, so that the dust settles quickly, which plays a good dust reduction role.
[0017] 4. The present invention uses environmentally friendly and non-toxic starch as the main matrix to prepare a highly water-absorbent dust suppressant, which is not only inexpensive but also has excellent biodegradability. At the same time, during the synthesis of the product, ester monomer compounds are added to participate in the copolymerization reaction, which not only enhances the water resistance of the mine road after spraying the dust suppressant, but also has a certain effect of solidifying the mine road after multiple spraying. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a flow chart of the preparation method of Examples 1-3. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0020] Example 1
[0021] like Figure 1 As shown, 7g starch, 11.5g acrylamide, and 0.5g maleic anhydride were weighed and added into a 250mL three-necked flask equipped with a stirring device, a thermometer, and a reflux condenser, and then 80mL water was added to dissolve, and 0.6g sodium hydroxide was added to adjust the pH to 6, and 0.3g butyl acrylate and 0.10g catalyst potassium persulfate were added, and the reaction was stirred at 30°C for 6 hours to obtain a colorless viscous liquid, which is an environmentally friendly mine road dust suppressant.
[0022] Example 2
[0023] like Figure 1 As shown, 12g starch, 10g acrylamide, and 1.0g maleic anhydride were weighed and added into a 250mL three-necked flask equipped with a stirring device, a thermometer and a reflux condenser, and then 75mL water was added to dissolve, and 1.4g sodium hydroxide was added to adjust the pH to 6.5, and 0.45g butyl acrylate and 0.15g catalyst ammonium persulfate were added at the same time. The colorless viscous liquid obtained by stirring and reacting at 40°C for 4 hours was the environmentally friendly mine road dust suppressant.
[0024] Example 3
[0025] like Figure 1 As shown, 10g starch, 12g acrylamide, and 2.0g maleic anhydride were weighed and added into a 250mL three-necked flask equipped with a stirring device, a thermometer and a reflux condenser, and then 73mL water was added to dissolve, and 2.1g sodium hydroxide was added to adjust the pH to 7, and 0.8g butyl acrylate and 0.10g catalyst ammonium persulfate were added at the same time. The colorless viscous liquid obtained by stirring and reacting at 50°C for 3 hours was the environmentally friendly mine road dust suppressant.
[0026] Example 4
[0027] like Figure 1 As shown, 12g starch, 8g acrylamide, and 2.0g maleic anhydride were weighed and added into a 250mL three-necked flask equipped with a stirring device, a thermometer and a reflux condenser, and then 75mL water was added to dissolve, and 2.1g sodium hydroxide was added to adjust the pH to 7, and 0.7g butyl acrylate and 0.20g catalyst ammonium persulfate were added at the same time. The colorless viscous liquid obtained by stirring and reacting at 40°C for 6 hours was the environmentally friendly mine road dust suppressant.
[0028] Example 5
[0029] The test was conducted on a road of a copper open pit mine. A section of road surface with a length of 4 km and a width of 15 m was selected as the test object (divided into four sections, each section of 1 km was used as the test object of the environmentally friendly mine road dust suppressant prepared in Examples 1-4), and another section of road surface with a length of 1 km and a width of 15 m was selected as a control example. The control example used clean water as the dust suppressant. The transportation road surface was mainly composed of ordinary crushed stone and copper tailings powder, the floating layer thickness was about 50 mm, the ore transportation vehicle was a 100-ton heavy-duty vehicle, and the vehicle flow rate was 50 vehicles / h. 150 kg of the environmentally friendly mine road dust suppressant of Examples 1-4 was added to a 5-ton watering truck to prepare a 3% concentration aqueous solution, and sprayed on the 4 sections of the test object road surface respectively. During the spraying process, each section of the road surface was sprayed as evenly as possible. Under the same test conditions, the dust suppression effect of each section of the road surface after spraying the dust suppressant was detected, and at the same time, the dust suppression effect of the road surface after spraying with clean water was compared. The results are shown in Table 1.
[0030] Table 1
[0031]
[0032]
[0033] In addition, after the dust suppression period (20 days) of spraying the road surface with the dust suppressant of Example 3, the dust suppressant aqueous solution of 3% concentration was sprayed again, and the spraying was cyclically sprayed for 5 cycles. The road surface sprayed with the dust suppressant multiple times had a certain cementing and curing effect on the surface layer of the mine road surface after rolling by the transport vehicle. When water was used as a dust suppressant, the strength of the mine road surface was 0.2MPa, and fatigue cracking would occur in the lower layer after long-term action; after cyclically spraying the dust suppressant of Example 3 for 5 cycles, the strength of the mine road surface increased to 0.8MPa, indicating that the road surface sprayed with the environmentally friendly dust suppressant multiple times had a certain cementing and curing effect on the surface layer of the mine road surface after rolling by the transport vehicle.
[0034] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing an environmentally friendly mine road dust suppressant, It is characterized in that The specific process is as follows: Starch, acrylamide and maleic anhydride are mixed and dissolved in water, alkali is added to adjust the pH to 6-7, and an ester monomer compound and a catalyst are added. The mixture is stirred and reacted at 30-50° C. for 3-6 hours to obtain a colorless viscous liquid, which is an environmentally friendly mine road dust suppressant.
2. The preparation method according to claim 1, It is characterized in that The alkali is one or both of sodium hydroxide and potassium hydroxide.
3. The preparation method according to claim 1, It is characterized in that The ester monomer compound is one or more of ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate.
4. The preparation method according to claim 1, It is characterized in that The catalyst is at least one of potassium persulfate, ammonium persulfate and azobisisobutyronitrile.
5. The preparation method according to claim 1, It is characterized in that The weight parts of water, starch, acrylamide, maleic anhydride, alkali, ester monomer compound and catalyst are respectively 73-80 parts of water, 7-12 parts of starch, 8-12 parts of acrylamide, 0.5-2 parts of maleic anhydride, 0.6-2.1 parts of alkali, 0.3-0.8 parts of ester monomer compound and 0.1-0.2 parts of catalyst.