Hydrophobic underwater epoxy curing agent and epoxy resin cross-linking agent
Through the Mannich reaction and polyepoxy reaction of polyamines, phenolic compounds and aldehyde compounds, a hydrophobic underwater epoxy curing agent is formed, which solves the problem of excessive curing speed and whitening of underwater epoxy adhesives, and achieves the High strength curing and convenient construction.
Patent Information
- Application Number
- CN202411268522.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
AI Technical Summary
The existing underwater epoxy adhesive cures too fast in humid environments, resulting in increased construction difficulty, increased cost, and prone to whitening, affecting stability.
Polyamines, phenolic compounds and aldehyde compounds are used to form a hydrophobic underwater epoxy curing agent through the Mannich reaction and polyepoxy reaction, avoiding the addition of coupling agents, prolonging the curing time, reducing the reaction activity, and increasing the hydrophobic carbon chains to increase bond strength and adjust viscosity by organic solvents.
It realizes high-strength curing in underwater environments, avoids whitening, reduces costs, extends the construction operation time window, and improves construction convenience and bonding performance.
Smart Images

Figure BDA0005037928620000041 
Figure BDA0005037928620000051 
Figure BDA0005037928620000052
Abstract
Description
Technical Field
[0001] The invention mainly belongs to the technical field of new organic functional materials, and in particular relates to a preparation method of a novel underwater epoxy curing agent. Background Art
[0002] With the development of industries such as offshore shipping and offshore wind power, there are more and more offshore engineering buildings. Long-term scouring and erosion by seawater will cause damage and corrosion of concrete and steel structures inside the building. Conventional adhesives can only be applied to dry surfaces and cannot be directly applied underwater. In view of the complex underwater application environment, high requirements for comprehensive properties such as adhesive bonding strength and hardness are required. There are few types of underwater adhesives available, and there are few reports on underwater adhesive systems. The available information mostly comes from degree theses and domestic journals. Therefore, it is necessary to develop an adhesive system that can be cured underwater.
[0003] During the curing process, the adhesive must be in direct contact with the adherend to achieve bonding. Unlike the curing of adhesives in the air environment, there is a layer of water film between the two underwater, and the bonding strength will be greatly reduced in this case. Due to the special conditions of curing in water, in general, adhesives need to have the following three characteristics: remain stable before curing and not miscible with water; have good wetting with the adhesive interface; have a certain strength after curing, and do not hydrolyze after being placed in water for a long time.
[0004] Epoxy resins can remain relatively stable in water, and epoxy adhesives have been widely used in the construction field in the last century. They have high production capacity and can be cured on wet interfaces and underwater after being mixed with specific curing agents. They show high bonding strength. Therefore, existing underwater adhesives are mainly epoxy adhesives. It is known that single epoxy resins have no practical value and must be combined with curing agents. Accelerators, toughening agents, diluents, coupling agents, fillers, defoaming agents and other auxiliary materials must be added according to conditions to obtain a network structure cured product with practical value. At present, there are many reports on modifying amine curing agents through Mannich reaction to obtain underwater epoxy curing agents.
[0005] The patent with publication number CN106242372A is an underwater epoxy mortar developed based on the existing curing agent. The main epoxy resin is removed from its formula and a cashew nut shell-modified phenolic amine curing agent is used to cure and cross-link with the epoxy resin. The short underwater curing time window brings inconvenience to construction. It also contains active diluents, toughening agents and fillers. Unlike conventional two-component epoxy adhesives, this patent contains three components, which is inconvenient during the specific construction operation. In addition, the dissolution of the components in water may cause whitening. For application scenarios such as buildings and hulls, this whitening can be regarded as a great instability factor.
[0006] In the formula of an underwater epoxy resin grouting material disclosed in the publication number CN1211451, in addition to adding phenol formaldehyde hexamethylenediamine condensate or phenol formaldehyde metaphenylenediamine condensate on the basis of the main epoxy resin, furfural, acetone and silane coupling agent must also be added. The furfural and acetone in the patent will cause whitening when they are miscible with water, and the curing agent must also be combined with a silane coupling agent to ensure the mechanical strength of the cured slurry, which further increases the cost and construction difficulty.
[0007] In the prior art, since coupling agents must be added to ensure mechanical strength after curing, and since all the existing curing agents are phenolic amine curing agents, their curing speed is too fast, which increases the cost and construction difficulty. In addition, since the formula ingredients partially dissolve in water, whitening occurs. For application scenarios such as buildings and hulls, this whitening can be regarded as a great instability factor. Therefore, it is very necessary to prepare an epoxy curing agent that can avoid underwater whitening, can achieve room temperature curing and has high strength. Summary of the invention
[0008] Purpose of the invention: In view of the above existing problems and shortcomings, the purpose of the present invention is to provide a hydrophobic underwater epoxy curing agent and epoxy resin crosslinking agent.
[0009] Technical solution: To achieve the above-mentioned invention object, the present invention adopts the following technical solution: A hydrophobic underwater epoxy curing agent is prepared by the following preparation method:
[0010] S1, 15-30 parts of polyamine and 20-25 parts of phenolic compound are added to a reaction container successively, no more than 60 parts of organic solvent are added under stirring, stirring and maintaining the system temperature not higher than 50° C., 13-28 parts of aldehyde compound are added to the system in batches, after ensuring complete dissolution, the temperature is gradually raised to 60-80° C., after ensuring complete reaction in the system, the temperature is cooled to room temperature, and an organic solution containing a curing agent precursor is obtained;
[0011] S2, after the organic solution containing the curing agent precursor obtained in step S1 is preheated to 50-75°C, a polyepoxy reaction substrate is added to the system until the epoxy groups inside the system are completely reacted, and excess organic solvent is removed by reduced pressure distillation to obtain a hydrophobic underwater epoxy curing agent.
[0012] Preferably, the polyamine is 1,6-hexanediamine, 1,8-octanediamine, 1,4-pentanediamine, diethylenetriamine, triethylenetetramine, polyethylenepolyamine, N-phenylethylenediamine, 2,4-diaminotoluene, DDM, DDS, 4,4'-diaminodiphenyl ether, m-phenylenediamine, m-phenylenediamine, diaminomethylcyclohexane, isophoronediamine, o-cyclohexyldiamine, m-cyclohexyldiamine, p-cyclohexyldiamine and cyclohexyldimethylamine, 1,3-cyclohexyldimethylamine, 1,4-cyclohexyldimethylamine.
[0013] Preferably, the phenolic compound is phenol, p-diphenol, nonylphenol or dodecylphenol.
[0014] Preferably, the aldehyde compound is paraformaldehyde, paraacetaldehyde, propionaldehyde, n-butyraldehyde or isobutyraldehyde.
[0015] Preferably, the polyepoxy reaction substrate includes 1,1'-dieoxirane ethyl sulfide, 1,4-di(oxirane-2-yl)benzene, (3,4,3',4'-diexyl)bicyclohexane, 1,5-diexyl hexane, 1,2,7,8-diexyl octane, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether, 2,2'-[[2-(allyloxy)-1,3-phenylene]bis(methylene)]bis(oxirane), propylene glycol dicyclohexane, 1,4-Butanediol diglycidyl ether, glycidyl terminated bisphenol A epichlorohydrin copolymer, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, 1,3-diepoxyglyceryl ether glycerol, 711 epoxy resin.
[0016] Preferably, the mass ratio of the polyamine, the phenolic compound and the aldehyde compound is (12-30):(20-25):(13-28).
[0017] Preferably, the organic solvent is ethyl acetate, ethanol, chloroform, acetone, butanone, DMF, DMSO, toluene, xylene or dioxane.
[0018] The present invention also provides a hydrophobic underwater epoxy resin crosslinking agent, comprising the following components in parts by weight: 35-55 parts of the above-mentioned curing agent, 40-60 parts of epoxy resin, and 0-10 parts of an auxiliary agent;
[0019] The epoxy resin includes bisphenol A epoxy resin, bisphenol F epoxy resin, hydroxylated epoxy resin, tetraphenol ethane epoxy resin; the auxiliary agent includes a defoamer and / or a accelerator.
[0020] Preferably, the defoaming agent includes isooctanoic acid, dimethyl silicone oil, lauryl phenylacetate or natural oil; the accelerator includes MP-10, DMP-30, N,N-diethylaniline, N,N-dimethylaniline, phenol, zinc isooctanoate, and cobalt isooctanoate.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0022] The curing agent of the present invention is based on the Mannich reaction of three types of substrates, phenol, aldehyde and amine, and the subsequent ring-opening reaction of the primary amine group with the terminal epoxy group of the polyepoxy reaction substrate structure. The curing agent structure of the present invention contains a relatively long hydrophobic carbon chain, which ensures its adhesive performance at the underwater adhesive interface.
[0023] At the same time, the primary and secondary amine groups and epoxy resins can react with the epoxy groups of the polyepoxy substrates to open the ring to form a network cross-linking, which improves the mechanical strength of the curing. At the same time, there is no need to add a coupling agent, which reduces costs and improves construction convenience while further avoiding the whitening phenomenon. The primary amine in the curing agent becomes a secondary amine, which reduces the reactivity of the curing agent and reduces the curing speed, thereby having a larger time window for underwater construction operations.
[0024] In addition, organic solvents are added during the preparation process to avoid uneven reactions caused by the increase in system viscosity as the reaction progresses. DETAILED DESCRIPTION
[0025] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0026] As shown below, the preparation synthesis route of the hydrophobic underwater epoxy curing agent of the present invention includes: ① synthesis of a phenolic amine curing agent precursor; ② synthesis of a hydrophobic underwater epoxy curing agent.
[0027]
[0028] The phenols involved in reaction ① of the present invention mainly include phenol, p-diphenol, nonylphenol, dodecylphenol and other phenolic compounds; the aldehydes involved in reaction ① mainly include paraformaldehyde, paraacetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde and other fatty aldehydes; the polyamines involved in reaction ① mainly include 1,6-hexanediamine, 1,8-octanediamine, 1,4-pentanediamine, diethylenetriamine, triethylenetetramine, polyethylenepolyamine and other fatty amines, N-phenylethylenediamine, 2,4 -diaminotoluene, DDM, DDS, 4,4'-diaminodiphenyl ether, m-phenylenediamine, m-phenylenediamine and other aromatic amines and diaminomethylcyclohexane, isophoronediamine, o-cyclohexyldiamine, m-cyclohexyldiamine, p-cyclohexyldiamine and cyclohexyldimethylamine, 1,3-cyclohexyldimethylamine, 1,4-cyclohexyldimethylamine and other alicyclic amines; the end-capping agents involved in reaction ② mainly include 1,1'-dioxirane ethyl sulfide, 1,4-di(oxirane-2- Benzene, (3,4,3',4'-diepoxy)bicyclohexane, 1,5-diepoxyhexane, 1,2,7,8-diepoxyoctane, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether, 2,2'-[[2-(allyloxy)-1,3-phenylene]bis(methylene)]bis(ethylene oxide), propylene glycol diglycidyl ester, diepoxybutadiene MSDS, vinyl cyclohexene dioxide, polyethylene glycol Alcohol diglycidyl ether, 9,10,12,13-diepoxyoctadecanoic acid, dicyclopentadiene epoxide, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, diglycidyl ether, 1,4-butanediol diglycidyl ether, glycidyl-terminated bisphenol A epichlorohydrin copolymer, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, 1,3-diglycidyl ether glycerol, 711 epoxy resin, epoxy resin E51 and other compounds.
[0029] Example 1
[0030] Synthesis of phenolic amine curing agent precursor: Add polyamine and phenolic compound respectively into a 500mL round-bottom flask, add 50mL solvent toluene, stir evenly, maintain the system temperature at 50±3°C, then add aldehyde compound into the system four times with an interval of 20min each time to ensure that the polyformaldehyde can be completely dissolved each time, stabilize the temperature of the reaction system and gradually increase the system temperature to 60-80°C. After ensuring that the reaction in the system is complete, cool to room temperature to obtain an organic solution containing a curing agent precursor.
[0031] Synthesis of curing agent: Preheat the solution containing the curing agent precursor to 60°C, then add the polyepoxy reaction substrate into the system, maintain the system temperature until the epoxy groups of the internal materials are completely reacted, then perform reduced pressure distillation to remove the internal organic solvent, and the result is a high-efficiency underwater epoxy curing agent with hydrophobic properties.
[0032] Epoxy resin crosslinker formula: The adhesive system is developed based on the hydrophobic underwater epoxy curing agent, and the mass fractions of each component are as follows:
[0033]
[0034] In the underwater environment system, the above components were added and mixed, and the curing time was recorded to reach 14 hours, and the cured surface properties were observed after 48 hours. According to the standard QJ 1634A-1996, the adhesive was poured into the mold, and after curing and molding, it was taken out to obtain a rubber strip with a diameter of 10mm and a height of 25mm. The material compression strength was measured to be 11.3MPa. Then, the standard specimen was prepared according to GJB 94-1986, and the shear strength was tested. The tensile strength was measured to be 10.4MPa. According to the standard GB / T 10247-2008, the kinematic viscosity of the adhesive was tested to be 265mPa·s.
[0035] Compared with Example 1, Examples 2-5 have the same synthesis and preparation methods, except that the synthesis of the curing agent and the formula components and contents of the epoxy resin crosslinking agent are different, as shown in Table 1 below.
[0036] Table 1 shows the components and contents of the curing agents in various embodiments of the present invention.
[0037]
[0038] Different epoxy resin crosslinking agents were prepared according to the above method, and their physical and chemical properties were tested. The curing agent in the embodiment and the comparative example was selected from the curing agent prepared above or T-31 curing agent and P-1134 curing agent purchased from Baling Petrochemical and Chuzhou Huisheng Electronics, respectively. The test results are shown in Tables 2 and 3 below.
[0039] Table 2 is the formula of epoxy resin crosslinking agent of each embodiment of the present invention and comparative example
[0040]
[0041] Table 3 shows the physical and chemical performance parameters of epoxy resin crosslinking agents of various embodiments and comparative examples of the present invention.
[0042]
[0043] As shown in Tables 1-3, the phenolic amine curing agent prepared by the present invention has good compatibility with epoxy resin, good adhesion to interfaces such as metals, and can be rapidly cured underwater within the range of -10-90°C. After curing, the obtained cured product has good mechanical properties, and can not only be applied to underwater epoxy coatings at metal or concrete interfaces, but can also be further used in underwater building epoxy structural adhesives or grouting materials, with compression strength and tensile strength reaching 11.6MPa and 10.4MPa, respectively. The present invention modifies traditional polyamine small molecules with hydrophobic long chains, and then caps the terminal primary amine groups with alkyl / aryl glycidyl ethers, effectively reducing underwater solubility, avoiding the problems of whitening that are easy to occur in traditional epoxy resin curing agents underwater, and can stably exist underwater, and have good bonding strength. At the same time, by secondary aminated the primary amine of the phenolic amine curing agent precursor, the curing time is extended to ensure sufficient construction operation time window, which is convenient for underwater construction.
Claims
1. A hydrophobic underwater epoxy curing agent, characterized in that: Prepared by the following preparation method: S1, 15-30 parts of polyamine and 20-25 parts of phenolic compound are added to a reaction container successively, no more than 60 parts of organic solvent are added under stirring, stirring and maintaining the system temperature not higher than 50° C., 13-28 parts of aldehyde compound are added to the system in batches, after ensuring complete dissolution, the temperature is gradually raised to 60-80° C., after ensuring complete reaction in the system, the temperature is cooled to room temperature, and an organic solution containing a curing agent precursor is obtained; S2, after the organic solution containing the curing agent precursor obtained in step S1 is preheated to 50-75°C, a polyepoxy reaction substrate is added to the system until the epoxy groups inside the system are completely reacted, and excess organic solvent is removed by reduced pressure distillation to obtain a hydrophobic underwater epoxy curing agent.
2. The method for preparing a hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The polyamines are 1,6-hexanediamine, 1,8-octanediamine, 1,4-pentanediamine, diethylenetriamine, triethylenetetramine, polyethylenepolyamine, N-phenylethylenediamine, 2,4-diaminotoluene, DDM, DDS, 4,4'-diaminodiphenyl ether, m-phenylenediamine, m-phenylenediamine, diaminomethylcyclohexane, isophoronediamine, o-cyclohexyldiamine, m-cyclohexyldiamine, p-cyclohexyldiamine and cyclohexyldimethylamine, 1,3-cyclohexyldimethylamine, and 1,4-cyclohexyldimethylamine.
3. The hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The phenolic compound is phenol, p-diphenol, nonylphenol or dodecylphenol.
4. The hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The aldehyde compound is paraformaldehyde, paraacetaldehyde, propionaldehyde, n-butyraldehyde or isobutyraldehyde.
5. The hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The polyepoxy reaction substrates include 1,1'-dieoxirane ethyl sulfide, 1,4-di(oxiran-2-yl)benzene, (3,4,3',4'-diexyl)bicyclohexane, 1,5-diexyl hexane, 1,2,7,8-diexyl octane, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether, 2,2'-[[2-(allyloxy)-1,3-phenylene]bis(methylene)]bis(ethylene oxide), propylene glycol diexylene Ester, diepoxy butadiene, vinyl cyclohexene dioxide, polyethylene glycol diglycidyl ether, 9,10,12,13-diepoxyoctadecanoic acid, dicyclopentadiene epoxide, cyclohexane-1,2-dicarboxylic acid diglycidyl ester, diglycidyl ether, 1,4-butanediol diglycidyl ether, glycidyl-terminated bisphenol A epichlorohydrin copolymer, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, 1,3-diglycidyl ether glycerol, 711 epoxy resin.
6. The hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The mass ratio of the polyamine, the phenolic compound and the aldehyde compound is (12-30):(20-25):(13-28).
7. The hydrophobic underwater epoxy curing agent according to claim 1, characterized in that: The organic solvent is ethyl acetate, ethanol, chloroform, acetone, butanone, DMF, DMSO, toluene, xylene or dioxane.
8. A hydrophobic underwater epoxy resin crosslinking agent, characterized in that: The composition comprises the following components in parts by weight: 35-55 parts of the curing agent according to any one of claims 1 to 7, 40-60 parts of the epoxy resin, and 0-10 parts of the auxiliary agent; The epoxy resin includes bisphenol A epoxy resin, bisphenol F epoxy resin, hydroxylated epoxy resin, tetraphenol ethane epoxy resin; the auxiliary agent includes a defoamer and / or a accelerator.
9. The hydrophobic underwater epoxy resin crosslinking agent according to claim 1, characterized in that: The defoaming agent includes isooctanoic acid, dimethyl silicone oil, lauryl phenylacetate or natural oil; the accelerator includes DMP-10 (dimethylaminomethylphenol), DMP-30, N,N-diethylaniline, N,N-dimethylaniline, phenol, zinc isooctanoate, and cobalt isooctanoate.
10. The hydrophobic underwater epoxy resin crosslinking agent according to claim 9, characterized in that: The accelerator is selected from DMP-30 or N,N-dimethylaniline.
Citation Information
Cited By
Water-insensitive cold-mixed epoxy resin and use method thereof
CN120795549A
A water-insensitive cold-mix epoxy resin and method of use
CN120795549B