Water-based PI resin and application thereof in water-based insulating paint
The aqueous PI resin is prepared by reacting tung oleic anhydride and multifunctional epoxy resin in aqueous insulating paint, and adding wetting agents and defoaming agents, the problem of insufficient curing speed and performance of water-based insulating paint is solved, and rapid curing and excellent performance is achieved The electrical properties are suitable for the coating of enameled wire and silicon steel sheets, and are environmentally friendly and efficient.
Patent Information
- Application Number
- CN202411266923.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The existing water-based insulating paint has shortcomings in curing speed, dielectric loss, high temperature resistance, adhesion, acid and alkali resistance and electrical properties, especially in the application of enameled wire and silicon steel sheet paint.
The aqueous PI resin is prepared by reacting tung oleic anhydride, multifunctional epoxy resin and para-aminobenzoic acid in diethylene glycol tert-butyl ether, and combined with an appropriate amount of wetting agent and defoaming agent to form an aqueous insulating paint, which significantly shortens the curing. Time, reduce dielectric loss, and improve the temperature, adhesion and electrical properties of the coating.
It realizes rapid curing, low dielectric loss, good temperature resistance and electrical properties of water-based insulating paint. It is suitable for the coating of enameled wire and silicon steel sheets, and is environmentally friendly and has few VOC emissions, and has better performance than traditional solvent-based insulating paint.
Smart Images

Figure CN118978699A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of water-based insulating paints, and in particular relates to a water-based PI resin and application thereof in water-based insulating paints. Background Art
[0002] Insulating varnish is an important insulating material based on polymer materials that can solidify into an insulating film or an insulating whole under certain conditions. According to the scope of use, insulating varnish can be divided into five categories: impregnating varnish, wire enamel, covering varnish, silicon steel sheet varnish, and anti-corona varnish.
[0003] Among them, wire enamel is mainly used for coating insulation of enameled wire core. Since the wire will be subjected to heat, chemical and various mechanical forces during the process of winding coils and embedding wires, the wire enamel is required to have good coating properties (i.e., uniform coating), strong paint film adhesion, smooth, soft and tough surface, certain wear resistance and elasticity, good electrical properties, heat resistance, solubility resistance, no corrosion to conductors, etc.
[0004] Silicon steel sheet paint is used to coat silicon steel sheets to reduce the eddy current loss of the core and enhance corrosion resistance. After coating, the silicon steel sheet paint needs to be dried at high temperature for a short time. Its characteristics are thin coating, strong adhesion, hardness, smoothness, uniform thickness, oil resistance, moisture resistance, and good electrical performance.
[0005] Traditional insulating varnishes are solvent-based products with a VOC content of nearly 70%, so water-based insulating varnishes have been the focus of development in recent years. However, both enameled wire varnishes and silicon steel sheet varnishes have high requirements for the electrical properties, adhesion, and high temperature resistance of the coating. There is still room for improvement in existing water-based insulating varnishes. For example, in the invention patent application with application number 202311812016.8, the applicant proposed a water-based insulating varnish that can meet the needs of automotive motor flat wires, thermal management system capillaries, heat dissipation appliances, etc., and is especially suitable for enameled copper, aluminum tubes / wires, electromagnetic wires and other wires, but its curing speed is average and needs further improvement. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention synthesizes a water-based PI (polyimide) resin and applies it to wire enamel and silicon steel sheet paint, which can significantly shorten the curing time and reduce dielectric loss. At the same time, the coating has good temperature resistance, adhesion, acid and alkali resistance, electrical properties, hardness and flexibility, which can meet the product performance requirements of wire enamel and silicon steel sheet paint at the same time, and is environmentally friendly with low VOC emissions.
[0007] The present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides a water-based PI resin, which is prepared by the following method: 80-130 parts of tung oil anhydride, 100 parts of multifunctional epoxy resin, 20-50 parts of p-aminobenzoic acid and 210-270 parts of diethylene glycol tert-butyl ether are mixed and dispersed evenly by weight, and then the temperature is raised to 120°C while dispersing and maintained for 3 hours, and then the temperature is reduced and the material is filtered out.
[0009] The polyimide water-based resin is prepared by first reacting tung oil anhydride and multifunctional epoxy resin in a solvent of diethylene glycol tert-butyl ether under the catalytic action of p-aminobenzoic acid, and can be further used to prepare water-based insulating paint.
[0010] Preferably, the multifunctional epoxy resin is a phenolic epoxy resin, such as 638s.
[0011] The invention also provides a water-based insulating varnish, comprising the water-based PI resin.
[0012] The present invention also provides a water-based insulating varnish for enameled wires, wherein 100 parts by weight of raw materials are composed of the following components: 40-60 parts of the water-based PI resin, 2.5-6.5 parts of diethanolamine, 0-10 parts of a solvent, 0.2-2 parts of a wetting agent, and the balance of deionized water.
[0013] Preferably, the wetting agent consists of BYK349 and Digo 4100 in a weight ratio of 1:1.
[0014] Preferably, the solvent is one or both of diethylene glycol butyl ether and diethylene glycol tert-butyl ether.
[0015] The present invention also provides a water-based insulating paint for silicon steel sheets, wherein 100 parts by weight of raw materials are composed of the following components: 57 parts of the water-based PI resin as described in claim 1 or 2, 4-10 parts of diethanolamine, 0-10 parts of a solvent, 0.1-1.5 parts of a wetting agent, 0.1-1.5 parts of a defoaming agent, and the remainder of deionized water.
[0016] The silicon steel sheet mentioned above can be electrical steel coil, silicon steel sheet and the like.
[0017] Preferably, the solvent is one or both of diethylene glycol butyl ether and diethylene glycol tert-butyl ether.
[0018] Preferably, the wetting agent is Digo 4100.
[0019] Preferably, the defoaming agent is Efcona 2524.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention synthesizes a water-based PI resin and applies the resin to water-based insulating paint, thereby obtaining an insulating paint with fast curing speed, low dielectric loss, safety, environmental protection, and no irritating odor volatilization; temperature resistance ≥310°C; good coating adaptability, good adhesion, and good acid and alkali resistance on metal substrates such as copper, aluminum, and steel; strong electrical breakdown resistance, the normal breakdown voltage of the coating is ≥3200V / 10μm, which is 40% or more higher than that of ordinary coatings; the coating has good density, no pinholes, and good flexibility, and completely overcomes the disadvantages of oily PI becoming hard and brittle with thick coating and having many pinholes and slow drying; and can be applied to insulating paint for coating enameled wires and / or silicon steel sheets. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The dielectric loss test results of the samples in Example 3 of the present invention are shown in FIG.
[0023] Figure 2 The dielectric loss test results of the samples of Example 4 of the present invention are shown in FIG.
[0024] Figure 3 The dielectric loss test results of the samples of Example 5 of the present invention are shown in FIG.
[0025] Figure 4 This is a schematic diagram of coating an enameled wire according to an embodiment of the present invention;
[0026] Figure 5 This is a schematic diagram of the coated enameled wire;
[0027] Figure 6 This is one of the schematic diagrams of silicon steel sheets;
[0028] Figure 7 This is the second schematic diagram of silicon steel sheet. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings and embodiments. Preferred embodiments of the present invention are given in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0031] The reagents used in the following examples, unless otherwise specified, are all commercially available; the methods used in the following examples, unless otherwise specified, are all achievable by conventional methods.
[0032] Water-based PI resin
[0033] Table 1 Raw material composition of water-based PI resin in Examples 1 to 3
[0034] Example 1 Example 2 Example 3 Tung oil anhydride 80 100 130 638S 100 100 100 p-Aminobenzoic acid 34 20 50 Diethylene glycol tert-butyl ether 214 238 270
[0035] Example 1
[0036] According to weight, 80 parts of tung oil anhydride, 100 parts of multifunctional epoxy resin, 34 parts of p-aminobenzoic acid and 214 parts of diethylene glycol tert-butyl ether are mixed and dispersed evenly, then heated to 120°C while dispersing and maintained for 3 hours, then cooled and filtered to obtain a water-based modified PI resin.
[0037] The obtained sample has the appearance of yellow transparent liquid, solid content: 57% (150°C / 90min), viscosity: 1100mpa·s / 33°C.
[0038] Example 2
[0039] According to weight parts, 100 parts of tung oil anhydride, 100 parts of multifunctional epoxy resin, 40 parts of p-aminobenzoic acid and 238 parts of diethylene glycol tert-butyl ether are mixed and dispersed evenly, then heated to 120°C while dispersing and maintained for 3 hours, then cooled and filtered to obtain a water-based modified PI resin.
[0040] The obtained sample has the appearance of yellow transparent liquid, solid content: 58% (150°C / 90min), viscosity: 1250mpa·s33°C.
[0041] Example 3
[0042] According to weight parts, 130 parts of tung oil anhydride, 100 parts of multifunctional epoxy resin, 50 parts of p-aminobenzoic acid and 270 parts of diethylene glycol tert-butyl ether are mixed and dispersed evenly, then heated to 120°C while dispersing and maintained for 3 hours, then cooled and filtered to obtain a water-based modified PI resin.
[0043] The obtained sample has the appearance of yellow transparent liquid, solid content: 57% (150°C / 90min), viscosity: 1160mpa·s / 33°C.
[0044] Water-based insulating varnish for enameled wire
[0045] Table 2 Formulas of various embodiments and comparative examples of water-based insulating varnishes for enameled wire
[0046]
[0047] Embodiments 4 to 6
[0048] According to weight, 55 parts of the water-based modified PI resin prepared in Examples 1 to 3 were neutralized with 5.5 parts of diethanolamine, 0.3 parts of BYK349 wetting agent, 0.3 parts of Digo 4100 wetting agent, and 38.9 parts of deionized water, stirred evenly, filtered and packaged, and the water-based insulating varnish for enameled wire was obtained. Table 2 shows the test results of the apparent properties of each sample.
[0049] Comparative Example 1
[0050] The difference from Example 4 is that only a single wetting agent, Digo 4100, is used.
[0051] Comparative Example 2
[0052] The difference from Example 4 is that only a single wetting agent BYK349 is used.
[0053] Comparative Example 3
[0054] The difference from Example 4 is that the proportion of the wetting agent is different.
[0055] Comparative Example 4
[0056] The insulating varnish in Example 3 in the applicant's prior application 202311812016.8.
[0057] Table 3 Test results of apparent properties of each sample of water-based insulating varnish for enameled wire
[0058]
[0059]
[0060] Furthermore, the above samples were processed by a 4-head DV60 medium-speed enameled wire machine (reference Figure 1 ) was used to carry out coating experiments, using the same primer and the same wire material. Its curing process and main performance indexes are shown in Table 3. It can be seen that compared with the comparative example, which contains only one wetting agent or the wetting agent ratio is not 1:1, and the water-based insulating paint in the previous application, the dielectric loss of the insulating paint in the embodiment of the present application is significantly reduced, and the curing speed is improved, and the curing line speed is increased from the original maximum of 24m / min to 40-90m / min. Figure 1-3 The dielectric loss test results of the samples of Examples 4-6 are respectively, Figure 4 This is a schematic diagram of enameled wire coating. Figure 5 Schematic diagram of coated enameled wire.
[0061] Table 4 Curing process and main performance indicators of each sample of water-based insulating varnish for enameled wire
[0062]
[0063]
[0064] Water-based insulating varnish for silicon steel sheets
[0065] Table 5 Comparative Examples of Water-Based Insulating Paints for Silicon Steel Sheets
[0066]
[0067] Embodiment 7-9
[0068] According to weight parts, 57 parts of the water-based modified PI resin prepared in Examples 1 to 3 were neutralized with 5.7 parts of diethanolamine, and then 10 parts of diethylene glycol butyl ether, 0.6 parts of Digo 4100 wetting agent, 0.5 parts of Efcona 2524 defoaming agent, and 26.2 parts of deionized water were added. After stirring evenly, the mixture was filtered and packaged to obtain the water-based insulating paint for coating silicon steel sheets.
[0069] Comparative Example 5
[0070] The difference from Example 7 is that no defoaming agent is contained.
[0071] Comparative Example 6
[0072] The difference from Example 7 is that no wetting agent is contained.
[0073] Comparative Example 7
[0074] The difference from Example 7 is that the ratio of the wetting agent to the defoaming agent is different.
[0075] The test results of the apparent properties of the water-based insulating varnishes obtained in Examples 7-9 and Comparative Examples 5-7 are shown in Table 6.
[0076] Table 6 Test results of apparent properties of each water-based self-adhesive insulating varnish in Examples 7-9
[0077]
[0078] Further, the above sample is coated on the surface of the silicon steel sheet by roller coating. Figure 6 As shown, the insulating paint is then cured by baking in a chain-type tunnel furnace. At the same time, it is compared with the insulating paint of comparative examples 4-7.
[0079] The specific curing process and main performance indicators are shown in Table 7.
[0080] Table 7 Curing process and main performance indicators of water-based insulating varnish for silicon steel sheets
[0081]
[0082] It can be seen that the performance of the paint film is affected by adding only a wetting agent or a defoamer. Only when the Digo 4100 wetting agent and the Efcona 2524 defoamer are used in combination and the ratio is appropriate can a better effect be achieved. Moreover, compared with the water-based insulating paint previously applied, the curing ability is significantly improved, and the curing time is reduced from 1 minute 40 seconds to 50 seconds.
[0083] Apart from Figure 6 The insulating varnish of the present invention can also be used for the silicon steel sheet shown in Figure 7 The silicon steel sheet shown.
[0084] In summary, it can be seen that the scheme of the present invention prepares a polyimide water-based resin by first reacting tung oil anhydride and a multifunctional epoxy resin in a solvent of diethylene glycol tert-butyl ether under the catalytic action of p-aminobenzoic acid. The polyimide water-based resin can be further used to prepare a water-based insulating paint by adding a suitable wetting agent, a defoaming agent, etc. The obtained water-based paint has a fast curing speed, a small dielectric loss, and excellent performance in all aspects.
[0085] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0086] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A water-based PI resin, characterized in that: The water-based PI resin is prepared by the following method: 80-130 parts of tung oil anhydride, 100 parts of multifunctional epoxy resin, 20-50 parts of p-aminobenzoic acid and 210-270 parts of diethylene glycol tert-butyl ether are mixed and dispersed uniformly according to weight parts, and then the temperature is raised to 120° C. and maintained for 3 hours while dispersing, and then the temperature is lowered and filtered to discharge the material.
2. The water-based PI resin according to claim 1, characterized in that The multifunctional epoxy resin is a phenolic epoxy resin.
3. A water-based insulating varnish comprising the water-based PI resin as claimed in any one of claims 1 to 2.
4. A water-based insulating varnish for enameled wire, characterized in that: Every 100 parts by weight of the raw materials are composed of the following components: 40-60 parts of the water-based PI resin as claimed in claim 1 or 2, 2.5-6.5 parts of diethanolamine, 0-10 parts of a solvent, 0.2-2 parts of a wetting agent, and the balance of deionized water.
5. The water-based insulating varnish for enameled wire according to claim 4, characterized in that: The wetting agent consists of BYK349 and Digo 4100, with a weight ratio of 1:
1.
6. The water-based insulating varnish for enameled wire according to claim 4, characterized in that: The solvent is one or both of diethylene glycol butyl ether and diethylene glycol tert-butyl ether.
7. A water-based insulating varnish for silicon steel sheets, characterized in that: The raw materials per 100 parts by weight are as follows Composition: 57 parts of the water-based PI resin as claimed in claim 1 or 2, 4-10 parts of diethanolamine, 0-10 parts of a solvent, 0.1-1.5 parts of a wetting agent, 0.1-1.5 parts of a defoaming agent, and the balance of deionized water.
8. The water-based insulating varnish for silicon steel sheets according to claim 7, characterized in that: The solvent is one or both of diethylene glycol butyl ether and diethylene glycol tert-butyl ether.
9. The water-based insulating varnish for silicon steel sheets according to claim 7, characterized in that: The wetting agent is Digo 4100.
10. The water-based insulating varnish for silicon steel sheets according to claim 7, characterized in that: The defoamer is Efcona 2524.
Citation Information
Patent Citations
Full-biobased epoxy resin composition and condensate
CN102206324A
Water-based modified novolac epoxy resin as well as preparation method and application thereof
CN117777407A
Water-based modified tung oil anhydride curing agent as well as preparation method and application thereof
CN117777814A
Water-based insulating paint and preparation method thereof
CN117777821A