Boron-containing polysilsesquioxane, modified aerogel, boron-silicon hybrid phenolic aldehyde-based composite material as well as preparation method and application of boron-containing polysilsesquioxane, modified aerogel and boron-silicon hybrid phenolic aldehyde-based composite material
By introducing boron elements and preparing boron-containing polysilsesquioxane, combined with phenolic aerogel, the problems of poor compatibility and insufficient heat resistance of polysilsesquioxane and phenolic materials are solved, and the modified aerogel is realized or high heat and ablation resistance of borosilicate hybrid phenolic composites.
Patent Information
- Application Number
- CN202411127768.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-19
AI Technical Summary
The existing polysilsesquioxane materials have poor compatibility with phenolic materials, are prone to agglomeration and settlement, and are deficient in improving the heat and ablation resistance of phenolic materials.
Boron element is introduced to prepare boron-containing polysilsesquioxane with excellent heat resistance and high carbonization properties, and combined with phenolic aerogels to improve the heat resistance and ablation resistance of the material through polycondensation reaction and curing process. performance.
The good compatibility between polysilsesquioxane and phenolic aerogel is achieved, and the heat resistance and ablation resistance of phenolic aerogel are improved, forming a modified gas with excellent heat insulation, heat resistance and mechanical properties. Gel or borosilicate hybrid phenolic composites.
Smart Images

Figure CN118978703A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal protection materials, and specifically relates to a boron-containing polysilsesquioxane, a modified aerogel, a boron-silicon hybrid phenolic-based composite material, and a preparation method and application thereof. Background Art
[0002] Polysilsesquioxane is a special type of siloxane polymer, the main composition of which is (RSiO 1.5 ) n , wherein R is an organic group; the polymer structure of polysilsesquioxane can be ladder-shaped, tree-shaped or lantern-shaped; when R is phenyl, due to the influence of steric hindrance and other factors, its hydrolysis product can form a regular three-dimensional ordered ladder structure through catalytic rearrangement reaction.
[0003] Polysilsesquioxane has excellent heat resistance and low surface energy, making it suitable for the preparation of base materials for high temperature resistant coatings, and has significant application potential in aerospace thermal protection materials. However, existing polysilsesquioxanes are generally organic-inorganic hybrid materials with Si-O-Si as the skeleton. Its special hybrid structure enables it to have the advantages of both inorganic and organic phases, such as high temperature resistance, weather resistance, insulation performance, dielectric properties, radiation resistance, chemical resistance, flame retardancy and fire resistance. However, on the one hand, traditional polysilsesquioxane materials have poor compatibility with phenolic materials and are prone to agglomeration and sedimentation; on the other hand, they still need to be improved in improving the heat resistance and ablation resistance of phenolic materials. Summary of the invention
[0004] The purpose of the present invention is to provide a boron-containing polysilsesquioxane, a modified aerogel, a boron-silicon hybrid phenolic-based composite material, and a preparation method and application thereof. The present invention provides a novel boron-containing polysilsesquioxane with excellent heat resistance, thermal stability and high carbonization; the polysilsesquioxane material has good compatibility with phenolic aerogel, is not prone to agglomeration and sedimentation, and can effectively improve the heat resistance and ablation resistance of phenolic aerogel.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a boron-containing polysilsesquioxane having a structure shown in Formula I:
[0007]
[0008] In Formula I, R includes at least one of a phenyl group, a vinyl group, and a methacryloxypropyl group.
[0009] The present invention provides a method for preparing the boron-containing polysilsesquioxane described in the above technical solution, comprising the following steps:
[0010] Mixing a boron source, silane and a first organic solvent to perform a polycondensation reaction to obtain the boron-containing polysilsesquioxane;
[0011] The silane has a structure shown in Formula II:
[0012]
[0013] In Formula II, R 1 It includes at least one of methyl, ethyl and isopropyl; R in formula II is the same as R in formula I.
[0014] Preferably, the boron source comprises at least one of boric acid, boric acid ester and phenylboric acid;
[0015] The first organic solvent comprises at least one of methanol, ethanol, acetone, dichloromethane and acetonitrile;
[0016] The molar ratio of the boron source to the silane is 0.1 to 5:1, and the mass ratio of the total mass of the boron source and the silane to the first organic solvent is 1:1 to 100;
[0017] The polycondensation reaction is carried out under acidic conditions; the temperature of the polycondensation reaction is 0 to 180° C., and the time is 0.5 to 96 hours.
[0018] The invention provides a modified aerogel, wherein the preparation raw materials include phenolic aerogel and boron-containing polysilsesquioxane; the mass ratio of the phenolic aerogel to the boron-containing polysilsesquioxane is 1-100:1-30; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane described in the above technical scheme or the boron-containing polysilsesquioxane obtained by the preparation method described in the above technical scheme.
[0019] Preferably, the method for preparing the phenolic aerogel comprises the following steps:
[0020] The first phenolic prepolymer, the first catalyst and the pore-forming agent are mixed and cured; after the curing, the pore-forming agent is removed to obtain the phenolic aerogel.
[0021] Preferably, the first catalyst comprises at least one of hydrochloric acid, sulfuric acid and benzenesulfonyl chloride;
[0022] The pore-forming agent includes at least one of methanol, ethanol, acetone, tetrahydrofuran, dichloromethane and acetonitrile;
[0023] The mass ratio of the pore-forming agent to the first phenolic prepolymer is 0.1-100:1.
[0024] The invention provides a boron-silicon hybrid phenolic-based composite material, wherein the preparation raw materials include boron-containing polysilsesquioxane, a second organic solvent, a second phenolic prepolymer, a three-dimensional braided preform and a second catalyst; the mass ratio of the boron-containing polysilsesquioxane, the second phenolic prepolymer and the three-dimensional braided preform is 0.1-30:100:50-300; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane described in the above technical scheme or the boron-containing polysilsesquioxane obtained by the preparation method described in the above technical scheme.
[0025] Preferably, the fibers used in the three-dimensional braided preform include at least one of carbon fiber, glass fiber, basalt fiber and aramid fiber;
[0026] The second catalyst comprises at least one of hydrochloric acid, sulfuric acid, benzenesulfonyl chloride, sodium hydroxide and potassium hydroxide;
[0027] The second organic solvent includes at least one of methanol, ethanol, acetone, tetrahydrofuran, dichloromethane and acetonitrile.
[0028] The present invention provides a method for preparing the boron-silicon hybrid phenolic-based composite material described in the above technical solution, comprising the following steps:
[0029] The boron-containing polysilsesquioxane, the second organic solvent and the second phenolic prepolymer are mixed, and a condensation reaction is carried out in the presence of a second catalyst to obtain a boron-containing polysilsesquioxane-modified phenolic prepolymer;
[0030] The boron-containing polysilsesquioxane-modified phenolic prepolymer is mixed with a three-dimensional braided preform, and cured in the presence of a second catalyst to obtain the boron-silicon hybrid phenolic-based composite material.
[0031] Preferably, the condensation reaction temperature is 20 to 80°C and the time is 0.5 to 2 hours;
[0032] The curing temperature is 0-100° C. and the curing time is 0.5-96 hours.
[0033] The present invention provides an application of a modified aerogel or a borosilicate hybrid phenolic-formaldehyde-based composite material in a thermal protection material; the modified aerogel is the modified aerogel described in the above technical scheme; the borosilicate hybrid phenolic-formaldehyde-based composite material is the borosilicate hybrid phenolic-formaldehyde-based composite material described in the above technical scheme or the borosilicate hybrid phenolic-formaldehyde-based composite material obtained by the preparation method described in the above technical scheme.
[0034] The present invention introduces boron element into silsesquioxane to obtain boron-containing polysilsesquioxane having a structure shown in Formula I, which has a novel structure, excellent heat resistance, thermal stability and high carbon-forming property, and can be used as a modifier and ceramic precursor for thermal protection materials.
[0035] The present invention also provides a method for preparing the boron-containing polysilsesquioxane, specifically, mixing a boron source, silane and a first organic solvent, and performing a polycondensation reaction to obtain the boron-containing polysilsesquioxane. The preparation method provided by the present invention has the advantages of mild reaction conditions, simple reaction system, high synthesis efficiency and high safety.
[0036] The present invention also provides a modified aerogel, the raw materials for preparation include phenolic aerogel and boron-containing polysilsesquioxane; the preparation method of the phenolic aerogel includes the following steps: mixing a first phenolic prepolymer, a first catalyst and a pore-forming agent, and curing; after curing, removing the pore-forming agent to obtain the phenolic aerogel. In the present invention, the role of the boron-containing polysilsesquioxane is to modify the phenolic aerogel, improve the heat resistance and ablation resistance of the obtained material, the boron-containing polysilsesquioxane has good compatibility with the phenolic aerogel, is not easy to agglomerate and precipitate, and can effectively improve the heat resistance and ablation resistance of the phenolic aerogel; the phenolic aerogel has nano-scale micropores, adjustable density, and has excellent thermal insulation performance, heat resistance, ablation resistance and mechanical properties, and is an ideal thermal insulation material; the present invention combines the phenolic aerogel and the boron-containing polysilsesquioxane to obtain a modified aerogel, which can effectively improve its heat resistance and ablation resistance without reducing the mechanical properties of the obtained material.
[0037] Furthermore, in the present invention, the raw materials of the phenolic aerogel are widely available, and the aerogel has the advantages of simple synthesis method, mild conditions, no need for a pressure vessel, low reaction temperature, simple post-treatment, and can be dried at room temperature and pressure.
[0038] The present invention also provides a borosilicate hybrid phenolic-formaldehyde-based composite material, and the raw materials for preparation include boron-containing polysilsesquioxane, a second organic solvent, a second phenolic prepolymer, a three-dimensional braided preform, and a second catalyst. In the present invention, the boron-containing polysilsesquioxane has the characteristics of good heat resistance, high thermal stability, and high carbonization rate, and can be used as a modifier for the borosilicate hybrid phenolic-formaldehyde-based composite material; the three-dimensional braided preform can be used as a reinforcing material for the borosilicate hybrid phenolic-formaldehyde-based composite material, and is copolymerized with the boron-containing polysilsesquioxane and the second phenolic prepolymer to obtain the borosilicate hybrid phenolic-formaldehyde-based composite material. The borosilicate hybrid phenolic-formaldehyde-based composite material provided by the present invention has low density, excellent ablation resistance, thermal insulation performance, and mechanical properties; compared with the unmodified material, the introduction of the boron-containing polysilsesquioxane also effectively improves the heat resistance and carbonization performance of the borosilicate hybrid phenolic-formaldehyde-based composite material.
[0039] The present invention also provides a method for preparing the boron-silicon hybrid phenolic-based composite material, comprising the following steps: mixing a boron-containing polysilsesquioxane having a structure shown in formula I, a second organic solvent and a second phenolic prepolymer, and performing a condensation reaction to obtain a boron-containing polysilsesquioxane-modified phenolic prepolymer; the temperature of the condensation reaction is 20 to 80°C, and the time is 0.5 to 2 hours; mixing the boron-containing polysilsesquioxane-modified phenolic prepolymer with a three-dimensional braided preform, and curing in the presence of a second catalyst to obtain the boron-silicon hybrid phenolic-based composite material; the curing temperature is 0 to 100°C, and the time is 0.5 to 96 hours. The method provided by the present invention has a low preparation temperature, not exceeding 100°C; a simple process, fewer steps; less energy consumption, and low cost; no need for solvent replacement and supercritical drying; the boron-silicon hybrid phenolic-based composite material prepared thereby has a low density, excellent thermal and mechanical properties, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0041] Figure 1 is the hydrogen spectrum of boron-containing polysilsesquioxane-1;
[0042] Figure 2 is the hydrogen spectrum of boron-containing polysilsesquioxane-2;
[0043] Figure 3 This is the microscopic morphology of borosilicate hybrid phenolic-based thermal protection material-1;
[0044] Figure 4 This is the microscopic morphology of borosilicate hybrid phenolic-based thermal protection material-1 after ablation;
[0045] Figure 5 This is a microscopic morphology of the phenolic aerogel obtained in Comparative Example 1;
[0046] Figure 6 This is a microscopic morphology of the phenolic-based thermal protection material obtained in Comparative Example 2;
[0047] Figure 7 This is the microscopic morphology of the phenolic-based thermal protection material obtained in Comparative Example 2 after ablation. DETAILED DESCRIPTION
[0048] The present invention provides a boron-containing polysilsesquioxane having a structure shown in Formula I:
[0049]
[0050] In Formula I, R comprises at least one of a phenyl group, a vinyl group and a methacryloxypropyl group, and is preferably a phenyl group, a vinyl group or a methacryloxypropyl group.
[0051] In an embodiment of the present invention, the boron-containing polysilsesquioxane has a structure shown in Formula III or Formula IV:
[0052]
[0053]
[0054] The present invention also provides a method for preparing the boron-containing polysilsesquioxane described in the above technical solution, comprising the following steps:
[0055] Mixing a boron source, silane and a first organic solvent to perform a polycondensation reaction to obtain the boron-containing polysilsesquioxane;
[0056] The silane has a structure shown in Formula II:
[0057]
[0058] In Formula II, R 1 It includes at least one of methyl, ethyl and isopropyl, preferably methyl or ethyl; R in formula II is the same as R in formula I.
[0059] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.
[0060] In the present invention, the boron source preferably includes at least one of boric acid, boric acid ester and phenylboric acid, and more preferably boric acid; the molar ratio of the boron source to silane is preferably 0.1 to 5:1, and more preferably 0.3 to 2:1.
[0061] In the present invention, the first organic solvent preferably includes at least one of methanol, ethanol, acetone, dichloromethane and acetonitrile, and is more preferably methanol or ethanol; the mass ratio of the total mass of the boron source and silane to the first organic solvent is preferably 1:1-100, and is more preferably 1:5-50.
[0062] In the present invention, the polycondensation reaction is preferably carried out under acidic conditions; the acidic conditions are preferably pH 1 to 5; the reagent used to provide the acidic conditions is preferably hydrochloric acid with a concentration of 1 to 12 mol / L, and more preferably hydrochloric acid with a concentration of 5 to 10 mol / L. The polycondensation reaction of the present invention is preferably carried out by stirring under a nitrogen atmosphere. The temperature of the polycondensation reaction of the present invention is preferably 0 to 180°C, more preferably 50 to 120°C, and more preferably 75 to 100°C; the time is preferably 0.5 to 96h, and more preferably 1 to 6h; the stirring rate is preferably 100 to 500r / min, and more preferably 300r / min. After the polycondensation reaction is completed, the present invention preferably sequentially performs a first drying and pulverization on the obtained reaction liquid, mixes the obtained pulverized material with water, and then precipitates it, and then performs solid-liquid separation, and performs a second drying on the obtained solid material to obtain the boron-containing polysilsesquioxane. In the present invention, the precipitation time is preferably 30 minutes; the solid-liquid separation is preferably suction filtration; the second drying is preferably rotary evaporation; the temperature of the second drying is preferably 60-100°C, specifically 60°C, 80°C or 100°C; the time is preferably 24-72 hours, specifically 24 hours, 48 hours or 72 hours.
[0063] The present invention also provides a modified aerogel, the preparation raw materials of which include phenolic aerogel and boron-containing polysilsesquioxane; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane described in the above technical solution or the boron-containing polysilsesquioxane obtained by the preparation method described in the above technical solution.
[0064] The present invention has no special limitation on the source of the first phenolic prepolymer. In the embodiment of the present invention, the first phenolic prepolymer used is a phenolic resin with ethanol as solvent and a solid content of 60%. The mass ratio of the phenolic aerogel and the boron-containing polysilsesquioxane of the present invention is preferably 1-100:1-30, more preferably 10-50:5-20.
[0065] In the present invention, the preparation method of the phenolic aerogel comprises the following steps: mixing a first phenolic prepolymer, a first catalyst and a pore-forming agent, and curing the mixture; and removing the pore-forming agent after curing to obtain the phenolic aerogel.
[0066] In the present invention, the first catalyst preferably includes at least one of hydrochloric acid, sulfuric acid and benzenesulfonyl chloride, more preferably hydrochloric acid or sulfuric acid. In the present invention, when the first catalyst is hydrochloric acid or sulfuric acid, the concentration of hydrochloric acid or sulfuric acid is preferably 0.1 to 10 mol / L, more preferably 1 to 5 mol / L.
[0067] In the present invention, the pore-forming agent preferably includes at least one of methanol, ethanol, acetone, tetrahydrofuran, dichloromethane and acetonitrile, and is more preferably methanol, ethanol or acetone; the mass ratio of the pore-forming agent to the first phenolic prepolymer is preferably 0.1 to 100:1, and is more preferably 1 to 50:1.
[0068] In the present invention, the curing temperature is preferably 0 to 100° C., more preferably 40 to 70° C.; the curing time is preferably 0.5 to 96 hours, more preferably 2 to 20 hours.
[0069] In the present invention, the method of removing the pore-forming agent preferably includes normal pressure drying, supercritical CO 2 At least one of drying and freeze drying, more preferably atmospheric pressure drying, supercritical CO 2 In the present invention, the temperature of the atmospheric pressure drying is preferably 0 to 100°C; the supercritical CO 2 The drying temperature is preferably 30 to 100°C; the freeze-drying temperature is preferably -80 to 0°C.
[0070] The present invention also provides a boron-silicon hybrid phenolic-based composite material, the preparation raw materials of which include boron-containing polysilsesquioxane, a second organic solvent, a second phenolic prepolymer, a three-dimensional woven preform and a second catalyst; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane described in the above technical scheme or the boron-containing polysilsesquioxane obtained by the preparation method described in the above technical scheme.
[0071] The present invention has no special limitation on the source of the second phenolic prepolymer. In the embodiment of the present invention, the second phenolic prepolymer is a phenolic resin with ethanol as solvent and 60% solid content. The mass ratio of the boron-containing polysilsesquioxane, the second phenolic prepolymer and the three-dimensional braided preform of the present invention is preferably 0.1-30:100:50-300, more preferably 1-10:100:100-200.
[0072] In the present invention, the fiber used in the three-dimensional braided preform preferably includes at least one of carbon fiber, glass fiber, basalt fiber and aramid fiber, more preferably carbon fiber or aramid fiber. In the embodiment of the present invention, carbon fiber felt (ie, carbon fiber three-dimensional braided preform) is used.
[0073] In the present invention, the second catalyst preferably includes at least one of hydrochloric acid, sulfuric acid, benzenesulfonyl chloride, sodium hydroxide and potassium hydroxide, and more preferably hydrochloric acid, sulfuric acid, benzenesulfonyl chloride or sodium hydroxide. In the present invention, when the second catalyst is hydrochloric acid or sulfuric acid, the concentration of hydrochloric acid or sulfuric acid is preferably 0.1 to 10 mol / L, more preferably 1 to 5 mol / L. In the present invention, the amount of the second catalyst is preferably adjusted to a pH value of 1 to 5 or 9 to 14 when the solidification is performed.
[0074] In the present invention, the second organic solvent preferably includes at least one of methanol, ethanol, acetone, tetrahydrofuran, dichloromethane and acetonitrile, and more preferably methanol, ethanol or acetone. The mass ratio of the boron-containing polysilsesquioxane to the second organic solvent is preferably 1:0.1-100, and more preferably 1:1-50.
[0075] The present invention also provides a method for preparing the boron-silicon hybrid phenolic-formaldehyde-based composite material described in the above technical scheme, comprising the following steps: mixing a boron-containing polysilsesquioxane, a second organic solvent and a second phenolic-formaldehyde prepolymer, and performing a condensation reaction in the presence of a second catalyst to obtain a boron-containing polysilsesquioxane-modified phenolic-formaldehyde prepolymer; mixing the boron-containing polysilsesquioxane-modified phenolic-formaldehyde prepolymer with a three-dimensional braided preform, and curing them in the presence of a second catalyst to obtain the boron-silicon hybrid phenolic-formaldehyde-based composite material.
[0076] In the present invention, the temperature of the condensation reaction is preferably 20 to 80°C, more preferably 25 to 60°C; the time is preferably 0.5 to 2 hours, more preferably 1 hour. The condensation reaction of the present invention is preferably carried out under the condition of mechanical stirring; the speed of the mechanical stirring is preferably 50 to 500 r / min, more preferably 100 to 300 r / min. After the condensation reaction, the present invention preferably performs post-treatment on the obtained feed liquid, and the post-treatment preferably includes at least one of rotary evaporation, filtration and drying.
[0077] The mixing method of the boron-containing polysilsesquioxane-modified phenolic prepolymer and the three-dimensional braided preform of the present invention preferably includes vacuum infusion and / or normal pressure infusion. In the present invention, the curing temperature is preferably 0 to 100°C, more preferably 40 to 70°C; the time is preferably 0.5 to 96h, more preferably 2 to 20h. After the curing is completed, the present invention preferably dries the obtained material to obtain the borosilicate hybrid phenolic-based composite material. In the present invention, the drying is preferably drying at room temperature and pressure, and the drying time is preferably 24h.
[0078] The present invention also provides an application of a modified aerogel or a borosilicate hybrid phenolic-formaldehyde-based composite material in a thermal protection material; the modified aerogel is the modified aerogel described in the above technical scheme; the borosilicate hybrid phenolic-formaldehyde-based composite material is the borosilicate hybrid phenolic-formaldehyde-based composite material described in the above technical scheme or the borosilicate hybrid phenolic-formaldehyde-based composite material obtained by the preparation method described in the above technical scheme.
[0079] In the present invention, the thermal protection material is preferably an aerospace thermal protection material.
[0080] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] The first phenolic prepolymer and the second phenolic prepolymer used in the embodiment are both phenolic resins with ethanol as solvent and a solid content of 60%, and are produced by Beijing Glass Steel Institute Composite Materials Co., Ltd.;
[0082] The three-dimensional braided prepolymer used in the embodiment is a carbon fiber felt (carbon fiber three-dimensional braided prepolymer) with a density of 0.12-0.15 g / cm 3 , produced by Hebei Jingtan Technology Co., Ltd.
[0083] Example 1
[0084] Boric acid (1.7549 g, 0.03 mol) and phenyltriethoxysilane (1.9829 g, 0.01 mol) were dissolved in ethanol (100 mL) and reacted for 6 h at 75 ° C under nitrogen protection and acidic environment (pH = 2, 6 mol / L hydrochloric acid was used to provide an acidic environment). After the reaction was completed, the obtained reaction liquid was mixed with 1 L of deionized water and stirred for 30 min, then filtered, and the obtained solid material was dried in a vacuum oven at 60 ° C for 24 h to obtain boron-containing polysilsesquioxane-1.
[0085] The hydrogen spectrum of the boron-containing polysilsesquioxane-1 is as follows Figure 1 As shown, the structural formula is as follows:
[0086]
[0087] The residual carbon rate of the obtained boron-containing polysilsesquioxane-1 was tested according to GB / T 13464-2008 standard, and the result obtained was: the residual carbon rate at 900° C. was 78.29%.
[0088] Example 2
[0089] Boric acid (0.37098 g, 0.006 mol) and vinyltrimethoxysilane (1.4823 g, 0.01 mol) were dissolved in methanol (200 mL) and reacted for 1 h at 75 ° C, nitrogen protection, and acidic environment (pH = 2, 6 mol / L hydrochloric acid was used to provide an acidic environment). After the reaction, the obtained reaction liquid was dried and crushed in turn, and the obtained crushed material was mixed and stirred with 3L of deionized water for 2 h, and then filtered, and the obtained solid material was dried in a blast oven at 100 ° C for 72 h to obtain boron-containing polysilsesquioxane-2.
[0090] The hydrogen spectrum of the boron-containing polysilsesquioxane-2 is as follows Figure 2 As shown, the structural formula is as follows:
[0091]
[0092] The residual carbon rate of the obtained boron-containing polysilsesquioxane-2 was tested according to GB / T 13464-2008 standard, and the result obtained was: the residual carbon rate at 900° C. was 88.67%.
[0093] Example 3
[0094] The boron-containing polysilsesquioxane-1 (1 g) obtained in Example 1 was dissolved in methanol (199 g), and phenolic resin (100 g) and sodium hydroxide (1.5 g) were added to the resulting mixture. The mixture was reacted at 25° C. for 1 h to obtain a slurry of a boron-containing polysilsesquioxane-modified phenolic prepolymer.
[0095] The boron-containing polysilsesquioxane-modified phenolic prepolymer solution was mixed with a carbon fiber three-dimensional braided preform (100 g) and benzenesulfonyl chloride (10 mL), cured at 60° C. for 2 h, and then dried at room temperature and pressure for 24 h to obtain a modified phenolic aerogel.
[0096] The residual carbon rate of the modified phenolic aerogel was tested according to GB / T 13464-2008 standard, and the result was: the residual carbon rate at 900° C. was 59.76%.
[0097] The thermal conductivity of the modified phenolic aerogel was tested according to GB / T 10297-2015 standard, and the result was: the thermal conductivity was 0.0477 W / m·K.
[0098] The compressive strength of the modified phenolic aerogel was tested according to GB / T 8813-2020 standard, and the results were: the compression modulus was 56.5 MPa and the compression strength was 1.76 MPa.
[0099] Example 4
[0100] The boron-containing polysilsesquioxane-1 (1 g) obtained in Example 1 was dissolved in methanol (199 g), and phenolic resin (100 g) and sodium hydroxide (1.5 g) were added to the resulting mixture. The mixture was reacted at 25° C. for 1 h to obtain a slurry of a boron-containing polysilsesquioxane-modified phenolic prepolymer.
[0101] The boron-containing polysilsesquioxane-modified phenolic prepolymer liquid was mixed with a carbon fiber three-dimensional woven preform (100 g) and benzenesulfonyl chloride (10 mL) by vacuum infusion, cured at 60° C. for 2 h, and then dried at room temperature and pressure for 24 h to obtain a borosilicate hybrid phenolic thermal protection material-1.
[0102] The residual carbon rate of the borosilicate hybrid phenolic-based thermal protection material-1 was tested according to GB / T 13464-2008 standard, and the result was: the residual carbon rate at 900°C was 79.54%.
[0103] The mass ablation rate of the obtained borosilicate hybrid phenolic-based thermal protection material-1 was tested according to the GJB 323A-96 standard, and the result obtained was: the mass ablation rate was 0.0314 mm / s.
[0104] The thermal conductivity of the borosilicate hybrid phenolic-based thermal protection material-1 was tested according to GB / T 10297-2015 standard, and the result was: the thermal conductivity was 0.0662 W / m·K.
[0105] The compressive strength of the borosilicate hybrid phenolic-based thermal protection material-1 obtained was tested according to GB / T 8813-2020 standard, and the results were: the compression modulus was 544.25 MPa and the compression strength was 2.16 MPa.
[0106] The microstructure of boron-silicon hybrid phenolic-based thermal protection material-1 is as follows Figure 3 As shown. Figure 3 It can be seen that the modified phenolic aerogel has good bonding with the carbon fiber, and there is no gap between them, which shows that the boron-containing polysilsesquioxane helps the modified phenolic aerogel to bond with the carbon fiber and helps to improve the mechanical properties of the obtained boron-silicon hybrid phenolic-based thermal protection material.
[0107] Figure 4 This is the microscopic morphology of borosilicate hybrid phenolic thermal protection material-1 after ablation at 3000℃. Figure 4 It can be seen that the phenolic aerogel still adheres to the surface of the carbon fiber after ablation, indicating that the boron-containing polysilsesquioxane improves the heat resistance and ablation performance of the phenolic aerogel, so that the obtained boron-silicon hybrid phenolic-based thermal protection material still has a complete structure under high-temperature erosion and can adhere to the surface of the carbon fiber to form a protective layer. This is different from the unmodified material ( Figure 7 ) formed a sharp contrast.
[0108] Comparative Example 1
[0109] Phenolic resin (100 g) was used as a raw material, methanol (200 g) as a pore-forming agent, and benzenesulfonyl chloride (10 mL) as a catalyst. The mixture was cured at 60° C. for 2 h and then dried at room temperature and pressure for 24 h to obtain a phenolic aerogel.
[0110] The carbon residue rate of the obtained phenolic aerogel was tested according to GB / T 13464-2008 standard, and the result was: the carbon residue rate at 900°C was 55.18%.
[0111] The thermal conductivity of the phenolic aerogel was tested according to GB / T 10297-2015 standard, and the result was: the thermal conductivity was 0.0491 W / m·K.
[0112] The compressive strength of the obtained phenolic aerogel was tested according to GB / T 8813-2020 standard, and the results were: the compression modulus was 46.90 MPa and the compression strength was 1.46 MPa.
[0113] Figure 5 This is the microscopic morphology of the phenolic aerogel obtained in Comparative Example 1. Figure 3 and Figure 5 It can be seen that the microstructure of the modified borosilicate hybrid phenolic-based thermal protection material-1 has no obvious difference in morphology from the unmodified phenolic aerogel, indicating that the boron-containing polysilsesquioxane does not change the micromorphology of the phenolic aerogel.
[0114] Comparative Example 2
[0115] The preparation method is basically the same as that of Example 4, except that no boron-containing polysilsesquioxane-1 is added during the preparation process to obtain a phenolic-based thermal protection material.
[0116] The residual carbon rate of the phenolic-based thermal protection material was tested according to GB / T 13464-2008 standard, and the result was: the residual carbon rate at 900°C was 70.76%.
[0117] The mass ablation rate of the obtained phenolic-based thermal protection material was tested according to the GJB 323A-96 standard, and the result obtained was: the mass ablation rate was 0.0408 mm / s.
[0118] The thermal conductivity of the phenolic-based thermal protection material was tested according to GB / T 10297-2015 standard, and the result was: the thermal conductivity was 0.0696 W / m·K.
[0119] The compressive strength of the phenolic-based thermal protection material obtained was tested according to GB / T 8813-2020 standard, and the results were: the compression modulus was 445.23 MPa and the compression strength was 1.62 MPa.
[0120] Figure 6 This is a microscopic morphology of the phenolic-based thermal protection material obtained in Comparative Example 2. Figure 6 It can be seen that the carbon fibers are randomly interspersed in the phenolic aerogel, and there are gaps between some carbon fibers, indicating that the phenolic aerogel is not fully filled.
[0121] Figure 7 This is a microscopic morphology of the phenolic-based heat protection material obtained in Comparative Example 2 after ablation. Figure 7It can be seen that only carbon fibers remain in the phenolic-based thermal protection material after ablation, and no protective layer appears on the surface of the carbon fibers, indicating that the material without boron polysilsesquioxane has poor thermal and ablation properties.
[0122] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A boron-containing polysilsesquioxane having a structure shown in Formula I: In Formula I, R includes at least one of a phenyl group, a vinyl group, and a methacryloxypropyl group.
2. The method for preparing the boron-containing polysilsesquioxane according to claim 1, comprising the following steps: Mixing a boron source, silane and a first organic solvent to perform a polycondensation reaction to obtain the boron-containing polysilsesquioxane; The silane has a structure shown in Formula II: In Formula II, R1 includes at least one of methyl, ethyl and isopropyl; R in Formula II is the same as R in Formula I.
3. The preparation method according to claim 2, characterized in that: The boron source comprises at least one of boric acid, boric acid ester and phenylboric acid; The first organic solvent comprises at least one of methanol, ethanol, acetone, dichloromethane and acetonitrile; The molar ratio of the boron source to the silane is 0.1 to 5:1, and the mass ratio of the total mass of the boron source and the silane to the first organic solvent is 1:1 to 100; The polycondensation reaction is carried out under acidic conditions; the temperature of the polycondensation reaction is 0 to 180° C., and the time is 0.5 to 96 hours.
4. A modified aerogel, wherein the raw materials for preparing the aerogel include phenolic aerogel and boron-containing polysilsesquioxane; the mass ratio of the phenolic aerogel to the boron-containing polysilsesquioxane is 1-100:1-30; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane according to claim 1 or the boron-containing polysilsesquioxane obtained by the preparation method according to claim 2 or 3.
5. The modified aerogel according to claim 4, characterized in that The preparation method of the phenolic aerogel comprises the following steps: The first phenolic prepolymer, the first catalyst and the pore-forming agent are mixed and cured; after the curing, the pore-forming agent is removed to obtain the phenolic aerogel.
6. A borosilicate hybrid phenolic-based composite material, wherein the raw materials for preparation include boron-containing polysilsesquioxane, a second organic solvent, a second phenolic prepolymer, a three-dimensional woven preform and a second catalyst; the mass ratio of the boron-containing polysilsesquioxane, the second phenolic prepolymer and the three-dimensional woven preform is 0.1-30:100:50-300; the boron-containing polysilsesquioxane is the boron-containing polysilsesquioxane according to claim 1 or the boron-containing polysilsesquioxane obtained by the preparation method according to claim 2 or 3.
7. The boron-silicon hybrid phenolic-based composite material according to claim 6, characterized in that: The fibers used in the three-dimensional braided preform include at least one of carbon fiber, glass fiber, basalt fiber and aramid fiber; The second catalyst comprises at least one of hydrochloric acid, sulfuric acid, benzenesulfonyl chloride, sodium hydroxide and potassium hydroxide; The second organic solvent includes at least one of methanol, ethanol, acetone, tetrahydrofuran, dichloromethane and acetonitrile.
8. The method for preparing the boron-silicon hybrid phenolic-based composite material according to claim 6 or 7, comprising the following steps: The boron-containing polysilsesquioxane, the second organic solvent and the second phenolic prepolymer are mixed, and a condensation reaction is carried out in the presence of a second catalyst to obtain a boron-containing polysilsesquioxane-modified phenolic prepolymer; The boron-containing polysilsesquioxane-modified phenolic prepolymer is mixed with a three-dimensional braided preform, and cured in the presence of a second catalyst to obtain the boron-silicon hybrid phenolic-based composite material.
9. The preparation method according to claim 8, characterized in that: The condensation reaction temperature is 20-80°C and the time is 0.5-2h; The curing temperature is 0-100° C. and the curing time is 0.5-96 hours.
10. Use of a modified aerogel or a borosilicate hybrid phenolic-based composite material in a thermal protection material; the modified aerogel is the modified aerogel according to claim 4 or 5; the borosilicate hybrid phenolic-based composite material is the borosilicate hybrid phenolic-based composite material according to claim 6 or 7 or the borosilicate hybrid phenolic-based composite material obtained by the preparation method according to claim 8 or 9.
Citation Information
Patent Citations
High-strength nanoporous ceramizable ablation heatproof composite material and preparation method thereof
CN110951210A
Ablation-resistant modified phenolic aerogel thermal protection material and preparation method thereof
CN113980343A
Boron-containing silsesquioxane and preparation method thereof, modified phenolic resin and preparation method and application thereof
CN114835903A
Cited By
Phenylene boron hybrid silicon resin aerogel and preparation method thereof
CN119591871A
A phenylene-boron hybrid silicone resin aerogel and a method of making the same
CN119591871B
Fiber-reinforced silicon-boron modified phenolic aerogel multi-phase composite material with ablation resistance and heat management functions and preparation method of fiber-reinforced silicon-boron modified phenolic aerogel multi-phase composite material
CN122103679A
A fiber-reinforced silicon-boron modified phenolic aerogel multiphase composite material with anti-ablation and thermal management functions and a preparation method thereof
CN122103679B