Oxygen vacancy-containing calcium cerium niobate / polyetherimide composite dielectric as well as preparation method and application thereof
By introducing oxygen vacancy and Zn-O bonds into the calcium cerium niobate @MOF/polyetherimide composite dielectric, the problem of high conductivity loss and dielectric mismatch of polyetherimide film at high temperature is solved, and the problem of high conductivity loss and dielectric mismatch of polyetherimide film at high temperature is improved. Breakdown field strength and energy storage efficiency achieve more efficient energy storage performance.
Patent Information
- Application Number
- CN202411072987.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, the polyetherimide film has high conductivity loss at high temperatures, resulting in a decrease in charge and discharge efficiency, and the dielectric mismatch when the inorganic filler is modified, and the breakdown field strength is reduced, which affects the energy storage efficiency.
Using the oxygen-containing vacancies @MOF/polyetherimide composite dielectric, oxygen-vacancies are generated by replacing Ca2+ ions through Ce4+, enhancing the binding force of ZIF-8 and calcium-cerium niobate, and through Zn-O bonds and PEI The crosslinked area improves the degree of bonding between fillers and dielectric materials and improves interface compatibility.
It improves the breakdown field strength and energy storage efficiency of the material, enhances the overall performance of the composite material, reduces the interface mismatch between the filler and the dielectric material, and improves the energy storage capacity of polymer-based composite dielectrics.
Smart Images

Figure HDA0004981390400000011 
Figure HDA0004981390400000012 
Figure HDA0004981390400000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric energy storage film material development, and relates to a calcium cerium niobate / polyetherimide composite dielectric containing oxygen vacancies, and a preparation method and application thereof. Background Art
[0002] Among various dielectrics, polymer dielectrics have attracted more and more attention in recent years due to their advantages such as high breakdown strength, low dielectric loss, easy processing, and diverse structures. In order to meet the new requirements of the modern power electronics industry for polymer films, it is urgent to develop polymer film dielectrics with high discharge energy density and high charge-discharge efficiency at high temperatures.
[0003] Polyetherimide (PEI) is a high-performance thermoplastic polymer with a high dielectric constant and excellent thermal stability. However, due to the transition of carriers at high temperatures, pure polyetherimide films have high conductivity losses at high temperatures, which reduces their charge and discharge efficiency and applied electric field. The work reported on polyetherimide currently focuses on improving the defects of the polymer matrix itself through material composite technology and improving the energy storage performance of the polymer matrix. This includes the use of inorganic fillers to further improve the dielectric properties of polymer composites. Compared with polymers, these inorganic fillers have better insulation and thermal conductivity. By compounding with polymer matrices, the energy storage performance of polymer-based composites can be effectively improved. However, this method often requires a large amount of doping with inorganic fillers to achieve a significant increase in the dielectric constant. On the one hand, it will affect the flexibility and processing performance of polymer-based composites, resulting in a lack of mechanical properties; on the other hand, it will inevitably introduce structural defects, resulting in the degradation of the breakdown strength of the composite. At the same time, the dielectric mismatch between the filler and the interface reduces the breakdown field strength of the material and affects its energy storage efficiency. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a calcium cerium niobate / polyetherimide composite dielectric containing oxygen vacancies and a preparation method and application thereof, thereby solving the technical problems in the prior art of using inorganic fillers to modify polyetherimide, resulting in dielectric mismatch between the filler and the interface, reduced breakdown field strength of the material, and affecting its energy storage efficiency.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, comprising the following steps:
[0007] S1: K2CO3, CaCO3, Nb2O5 and CeO2 were added to ethanol and ground evenly, dried and calcined to obtain KCa2Nb3O 10(Ce) perovskite precursor, the KCa2Nb3O 10 (Ce) The perovskite precursor is added to fuming nitric acid and magnetically stirred to obtain calcium cerium niobate powder containing oxygen vacancies;
[0008] S2: adding zinc nitrate to the dispersion of the calcium cerium niobate powder containing oxygen vacancies, stirring and mixing evenly, and then adding dimethyl imidazole, standing for reaction, to obtain a calcium cerium niobate@MOF composite filler;
[0009] S3: adding the calcium cerium niobate @MOF composite filler into N-methyl-2-pyrrolidone, and adding 4,4'-diaminodiphenyl ether and bisphenol A dianhydride, stirring the reaction, and obtaining a calcium cerium niobate @MOF / polyetheramic acid composite sol; preparing the calcium cerium niobate @MOF / polyetheramic acid composite sol into a calcium cerium niobate @MOF / polyetheramic acid composite film, and performing imidization treatment to obtain the calcium cerium niobate @MOF / polyetherimide composite dielectric containing oxygen vacancies.
[0010] Preferably, in step S1, the molar ratio of K2CO3, CaCO3, Nb2O5 and CeO2 is 1.1:1.9:3:(0.05-0.1).
[0011] Preferably, in step S1, during the calcination treatment, the calcination temperature is 1100-1200° C., and the calcination time is 12-14 hours.
[0012] Preferably, in step S1, KCa2Nb3O 10 (Ce) The perovskite precursor is added to the fuming nitric acid solution and magnetically stirred for 72 to 120 hours.
[0013] Preferably, in step S2, the mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole is (0.05-0.15):0.07:0.66.
[0014] Preferably, in step S2, the reaction is allowed to stand for 50 to 60 minutes.
[0015] Preferably, in step S3, the ratio of the mass of the calcium cerium niobate@MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is (0.5-3.0):100.
[0016] Preferably, the calcium cerium niobate@MOF / polyetheramic acid composite film has a thickness of 7 to 13 μm.
[0017] A calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies is prepared by the above method.
[0018] The above-mentioned application of the oxygen vacancy-containing calcium cerium niobate@MOF / polyetherimide composite dielectric in capacitors.
[0019] Compared with the prior art, the present invention has the following beneficial technical effects:
[0020] The present invention discloses a method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies. In the preparation process, first, Ce 4+ Replaced Ca in perovskite materials 2+ Ion, here Ce 4+ Ions and Ca 2+ The ion valence is different, and a large number of oxygen vacancies are generated in the replacement layer. The generation of oxygen vacancies here forms a stable synthesis center of ZIF-8, which effectively improves the binding force between ZIF-8 and calcium cerium niobate powder and improves the stability of the material; secondly, the zinc ions in ZIF-8 form Zn-O bonds with the oxygen atoms in calcium cerium niobate, which further enhances the binding force between ZIF-8 and calcium cerium niobate powder; thirdly, due to the effect of tail amino substitution between ZIF-8 and PEI, a cross-linking region is formed, which improves the degree of binding between the two and effectively improves the breakdown field strength of the composite material, that is, ZIF-8 wrapped outside the calcium cerium niobate powder effectively improves the dielectric mismatch between the filler and PEI, improves the breakdown field strength of the material, and improves its energy storage efficiency. Therefore, the present invention provides a method for combining calcium cerium niobate containing oxygen vacancies with polyetherimide through MOF, which has good binding stability between the three-phase materials, reduces the mismatch between the filler and the dielectric material at the interface, forms an enhanced filler-polymer interface, and improves the ability of the energy storage polymer-based composite dielectric.
[0021] Furthermore, in step S1, the molar ratio of K2CO3, CaCO3, Nb2O5 and CeO2 is 1.1:1.9:3:(0.05-0.1), which helps to form a more stable and ordered crystal structure, thereby improving the physical and chemical properties of the material. The addition amount of CeO2 is moderate, and an appropriate amount of oxygen vacancies can be effectively generated during calcination and nitric acid treatment. These oxygen vacancies can not only serve as growth centers of ZIF-8 (MOF), but also improve the conductivity and stability of the material. The appropriate molar ratio can promote chemical reactions between raw materials and improve synthesis efficiency.
[0022] Furthermore, in step S1, during the calcination treatment, the calcination temperature is 1100-1200°C and the calcination time is 12-14 hours. The calcination temperature is within this range, which can ensure that K2CO3, CaCO3, Nb2O5 and CeO2 in the raw materials are fully decomposed and undergo solid phase reaction to form stable KCa2Nb3O 10(Ce) perovskite structure. Long calcination time provides sufficient time for solid phase reaction, making the reaction more complete and reducing the presence of unreacted products or intermediate phases. High temperature and long calcination time are conducive to the formation of KCa2Nb3O 10 (Ce) crystal growth, improve its crystallinity, high crystallinity materials usually have better physical and chemical properties. Appropriate calcination conditions can regulate the porosity and specific surface area of the material, which has an important influence on the loading of MOF and the performance of the composite material in the subsequent steps. High temperature and long time calcination help the uniform distribution of each component in the raw material on the microscopic scale and reduce the occurrence of phase segregation or phase separation. KCa2Nb3O treated with high temperature calcination 10 (Ce) perovskite precursor has better high-temperature stability and can maintain the stability of its structure and performance in subsequent high-temperature processing or applications.
[0023] Furthermore, KCa2Nb3O 10 The (Ce) perovskite precursor was added to the fuming nitric acid solution and magnetically stirred for 72 to 120 hours. + ions can react with KCa2Nb3O 10 (Ce) K between layers + Ions are exchanged to form protonated niobates, such as HCa2Nb3O 10 nH2O, this process expands the interlayer distance, providing more possibilities for subsequent processing and modification. Proton exchange leads to an increase in the interlayer distance, making the interlayer space more open, which is conducive to loading other functional molecules or ions. Magnetic stirring for 72 to 120 hours ensures the full progress of the proton exchange reaction and improves the reaction efficiency. Long-term stirring helps the H in the solution + Ions are evenly distributed in KCa2Nb3O 10 (Ce) surface and between layers, promoting the reaction.
[0024] Furthermore, the mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole is (0.05-0.15):0.07:0.66. The interaction between the calcium cerium niobate powder, zinc nitrate and dimethylimidazole may produce a synergistic effect, thereby enhancing the overall performance of the composite material. This mass ratio allows ZIF-8 to effectively include the calcium cerium niobate powder, effectively reducing the dielectric mismatch between the filler and the dielectric.
[0025] Further, in step S2, the reaction is allowed to stand for 50 to 60 minutes, and the reaction is allowed to stand for 50 to 60 minutes to provide sufficient time for the reactants to fully interact and transform, which helps to ensure that the chemical reaction between the reactants is as complete as possible, thereby improving the purity and yield of the product. Sufficient reaction time can reduce the presence of incomplete reactants or intermediates, thereby reducing the generation of by-products and improving the quality of the product. Standing reaction helps to maintain the temperature and pressure conditions of the reaction system relatively stable, avoid reaction rate fluctuations caused by vigorous stirring or temperature changes, thereby ensuring the smooth progress of the reaction process.
[0026] Furthermore, in step S3, the ratio of the mass of calcium niobate cerium @MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is (0.5-3.0):100. An appropriate amount of calcium niobate cerium @MOF composite filler can be used as a reinforcing phase to improve the internal structure of the composite material and improve the overall performance of the material. Here, too high an amount of calcium niobate cerium @MOF composite filler added will affect the flexibility and processing properties of the polymer-based composite material, resulting in a lack of mechanical properties, while too low an amount will not significantly improve the dielectric constant.
[0027] Furthermore, the thickness of the calcium cerium niobate@MOF / polyetheramic acid composite film is 7 to 13 μm. Within this thickness range, the composite film can exhibit good mechanical strength, flexibility and tear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 X-ray diffraction patterns of CNO(Ce) before exfoliation, CNO(Ce) after exfoliation, CNO(Ce)@MOF and pure ZIF-8 obtained in Comparative Example 1 of the present invention;
[0030] Figure 2 FT-IR spectra of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2;
[0031] Figure 3 The cross-sectional SEM images of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention, wherein (a) is the product of Example 1, (b) is the product of Example 2, and (c) is the product of Example 3;
[0032] Figure 4 The O1s orbital XPS fine spectra of CNO(Ce)@MOF / PEI prepared in Example 1 of the present invention and PEI prepared in Comparative Example 2;
[0033] Figure 5 The dielectric properties of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2;
[0034] Figure 6 The energy storage performance of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0036] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0037] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0038] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0039] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0040] The present invention provides a method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, comprising the following steps:
[0041] S1: K2CO3, CaCO3, Nb2O5 and CeO2 were added to ethanol and ground evenly, dried and calcined to obtain KCa2Nb3O 10 (Ce) perovskite precursor, the KCa2Nb3O 10 (Ce) The perovskite precursor is added to fuming nitric acid and magnetically stirred to obtain calcium cerium niobate powder containing oxygen vacancies;
[0042] Specifically, a certain amount of K2CO3, CaCO3, Nb2O5 and CeO2 powders are weighed, the mixture is ground evenly in anhydrous ethanol, and then placed in an oven for drying. The dried product is placed in a porcelain boat, placed in a muffle furnace, and calcined at 1100-1200°C for 12-14h to obtain KCa2Nb3O 10 (Ce) perovskite precursor. KCa2Nb3O 10 (Ce) powder is added to the fuming nitric acid solution and magnetically stirred for 72 to 120 hours, the replaced product is washed with deionized water to neutrality and dried to obtain calcium cerium niobate powder containing oxygen vacancies; Here, the molar ratio of K2CO3, CaCO3, Nb2O5 and CeO2 is 1.1:1.9:3:(0.05 to 0.1);
[0043] S2: Under ultrasonic conditions, a methanol solution of zinc nitrate is added to a methanol solution of calcium cerium niobate nanosheets, and after stirring evenly, a methanol solution of dimethylimidazole is added, and then the mixture is allowed to react for 50 to 60 minutes to obtain a calcium cerium niobate@MOF composite filler; the mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole is (0.05 to 0.15):0.07:0.66.
[0044] S3: Add the calcium cerium niobate @MOF composite filler to N-methyl-2-pyrrolidone, and add 4,4'-diaminodiphenyl ether and bisphenol A dianhydride, stir and react, and obtain a calcium cerium niobate @MOF / polyetheramic acid composite sol; prepare the calcium cerium niobate @MOF / polyetheramic acid composite sol into a calcium cerium niobate @MOF / polyetheramic acid composite film with a thickness of 7 to 13 μm, and perform imidization treatment to obtain the calcium cerium niobate @MOF / polyetherimide composite dielectric containing oxygen vacancies. The ratio of the mass of the calcium cerium niobate @MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is (0.5 to 3.0):100.
[0045] The above process is specifically as follows:
[0046] (1) dissolving calcium cerium niobate@MOF composite filler in N-methyl-2-pyrrolidone solvent to obtain a dispersion of calcium cerium niobate@MOF composite filler;
[0047] (2) adding 4,4-diaminodiphenyl ether (ODA) to N-methyl-2-pyrrolidone (NMP) in an ice-water bath, and performing ultrasonic dispersion to obtain a diamine dispersion; and adding the diamine dispersion to the dispersion of the calcium cerium niobate@MOF composite filler, and stirring evenly to obtain a diamine dispersion containing the calcium cerium niobate@MOF composite filler;
[0048] (3) adding bisphenol A diether dianhydride (BPADA) to the diamine dispersion containing calcium niobate cerium@MOF composite filler in batches, and the added amount is from large to small. During the addition of bisphenol A diether dianhydride, the external shear force is maintained for stirring. In a preferred embodiment, the bisphenol A diether dianhydride can be added in 7 times, and after each addition, the stirring is continued. The stirring time can be 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, 60 min. After the stirring reaction is completed, the calcium niobate cerium@MOF / polyether amide acid composite sol is obtained;
[0049] (4) coating the calcium cerium niobate@MOF / polyetheramic acid composite sol on a clean glass substrate to obtain a calcium cerium niobate@MOF / polyetheramic acid composite film, wherein the thickness of the composite film can preferably be 8 to 10 μm;
[0050] (5) The calcium cerium niobate @MOF / polyether imide composite film is placed at 80°C, dried in an air atmosphere for 12 hours, and subjected to a gradient temperature imidization treatment in an air atmosphere within a temperature range of 100°C to 300°C, and kept at each temperature for 1 hour. The temperature interval can be 50°C, that is, kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 hour each, to obtain a calcium cerium niobate @MOF / polyether imide composite film, that is, a calcium cerium niobate @MOF / polyether imide composite dielectric containing oxygen vacancies.
[0051] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0052] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0053] Example 1
[0054] (1) Preparation of cerium calcium niobate powder
[0055] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10 The (Ce) powder was added to 100 mL (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies.
[0056] (2) Preparation of calcium cerium niobate filler
[0057] The calcium cerium niobate powder containing oxygen vacancies was dissolved in a methanol solution, and the zinc nitrate hexahydrate methanol solution was added to the calcium cerium niobate methanol solution under ultrasonic conditions. After stirring for 30 seconds, the dimethyl imidazole methanol solution was added to the calcium cerium niobate methanol solution, ultrasonicated for 1 to 2 minutes, and allowed to stand for 60 minutes. -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish and freeze-dried to obtain calcium cerium niobate filler containing oxygen vacancies.
[0058] (3) Preparation of a dispersion containing filler
[0059] 0.028 g of calcium cerium niobate filler containing oxygen vacancies was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0060] (4) Preparation of composite diamine dispersion
[0061] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, and the diamine dispersion was added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler;
[0062] (5) Preparation of polyetheramide acid sol
[0063] Under ice water bath conditions, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing a composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amic acid sol containing a composite filler.
[0064] (6) Preparation of polyetherimide film containing composite fillers
[0065] A 10 μm layer of polyetheramide acid sol containing composite fillers was coated on the surface of a clean glass substrate, placed at 80°C, dried in an air atmosphere for 12 hours, and then kept at 100°C-150°C-200°C-250°C-300°C for 1 hour each. After cooling, a polyetherimide film containing composite fillers was obtained, i.e., calcium cerium niobate @MOF / polyetherimide composite dielectric containing oxygen vacancies. The product can be expressed as 0.5% CNO(Ce)@MOF / PEI
[0066] Example 2
[0067] (1) Preparation of cerium calcium niobate powder
[0068] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10 The (Ce) powder was added to 100 ml (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies.
[0069] (2) Preparation of calcium cerium niobate filler
[0070] Under ultrasonic conditions, add the hexahydrate zinc nitrate methanol solution to the methanol solution containing calcium cerium niobate powder with oxygen vacancies, stir for 30 seconds, then add the dimethyl imidazole methanol solution to the zinc nitrate methanol solution containing calcium cerium niobate, ultrasonicate for 1 to 2 minutes, and let stand for 60 minutes. -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish for freeze-drying to obtain calcium cerium niobate@MOF filler.
[0071] (3) Preparation of a dispersion containing filler
[0072] 0.056 g of calcium cerium niobate filler was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0073] (4) Preparation of composite diamine dispersion
[0074] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, and the diamine dispersion was added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler;
[0075] (5) Preparation of polyetheramide acid sol
[0076] Under ice water bath conditions, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing a composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amic acid sol containing a composite filler.
[0077] (6) Preparation of polyetherimide film containing composite fillers
[0078] A 10 μm layer of polyetheramide acid sol containing composite fillers was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, then kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each, and after cooling, a polyetherimide film containing composite fillers was obtained, i.e., calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies. The product can be expressed as 1.0% CNO(Ce)@MOF / PEI.
[0079] Example 3
[0080] (1) Preparation of cerium calcium niobate powder
[0081] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10The (Ce) powder was added to 100 ml (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies.
[0082] (2) Preparation of calcium cerium niobate filler
[0083] Under ultrasonic conditions, add the hexahydrate zinc nitrate methanol solution to the calcium cerium niobate methanol solution containing oxygen vacancies, stir for 30 seconds, then add the dimethyl imidazole methanol solution to the zinc nitrate methanol solution containing calcium cerium niobate, ultrasonicate for 1 to 2 minutes, and let stand for 60 minutes. Centrifuge at 10000 r min -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish for freeze-drying to obtain calcium cerium niobate filler.
[0084] (3) Preparation of a dispersion containing filler
[0085] 0.084 g of calcium cerium niobate filler was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0086] (4) Preparation of composite diamine dispersion
[0087] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, and the diamine dispersion was added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler;
[0088] (5) Preparation of polyetheramide acid sol
[0089] Under ice water bath conditions, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing a composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amic acid sol containing a composite filler.
[0090] (6) Preparation of polyetherimide film containing composite fillers
[0091] A 10 μm layer of polyetheramide acid sol containing composite fillers was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, then kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each, and after cooling, a polyetherimide film containing composite fillers was obtained, i.e., calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies. The product can be expressed as 1.5% CNO(Ce)@MOF / PEI.
[0092] Comparative Example 1
[0093] In order to compare the effect of conventional stripping operation on the prepared calcium cerium niobate powder, this comparative example was conducted. Specifically:
[0094] (1) Preparation of cerium calcium niobate powder
[0095] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10 The (Ce) powder was added to 100 mL (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder, which corresponds to Figure 1 CNO(Ce) before stripping;
[0096] (2) Preparation of calcium cerium niobate filler
[0097] 1.5 g of multilayer calcium cerium niobate powder was dispersed in 150 ml of tetrabutylammonium hydroxide aqueous solution and magnetically stirred for 7 days. After drying, calcium cerium niobate nanosheets (corresponding to Figure 1 The CNO(Ce) stripped from the sample was dissolved in a methanol solution, and the hexahydrated zinc nitrate methanol solution was added to the calcium cerium niobate methanol solution under ultrasonic conditions. After stirring for 30 seconds, the dimethyl imidazole methanol solution was added to the calcium cerium niobate methanol solution, ultrasonicated for 1 to 2 minutes, and allowed to stand for 60 minutes. The solution was centrifuged at 10,000 r min. -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish for freeze-drying to obtain calcium cerium niobate filler (corresponding to Figure 1 CNO(Ce)@MOF).
[0098] Comparative Example 2
[0099] The difference between this comparative example and Example 1 is that no composite filler is added during the preparation of the polyetherimide film, specifically:
[0100] (1) Preparation of diamine dispersion
[0101] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion.
[0102] (2) Preparation of polyetheramide acid sol
[0103] In an ice-water bath, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion in eight times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amide acid sol.
[0104] (3) Preparation of polyetherimide film
[0105] A 10 μm layer of polyetheramide acid sol was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, and kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each. After cooling, a polyetherimide film was obtained, and the sample was marked as PEI.
[0106] Figure 1 The X-ray diffraction patterns of CNO(Ce) before stripping, CNO(Ce) after stripping, CNO(Ce)@MOF and pure ZIF-8 obtained in Comparative Example 1 of the present invention show that there is no shift in the crystal plane of the material or increase or decrease in the characteristic peaks. During the experiment, the silk-like phenomenon that occurs when preparing pure CNO is not observed, and its color changes significantly. Therefore, the conventional tetrabutylammonium hydroxide used in this method fails to successfully strip the calcium cerium niobate filler, and the material has good stability.
[0107] Figure 2 FT-IR spectra of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2. It can be seen from the figure that almost identical characteristic absorption peaks of chemical functional groups are observed in PEI and the composite material, which means that the doped filler does not interrupt or destroy the molecular chain structure of polyetherimide during the reaction with PEI, indicating that the filler (CNO(Ce)@MOF) in the present invention has good compatibility with PEI.
[0108] Figure 3The cross-sectional SEM images of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention show that the cross-sectional area of the filler-doped film is dense and uniform without obvious defects, which proves that the filler has good compatibility with the composite material.
[0109] Figure 4 The O1s orbital XPS fine spectra of CNO(Ce)@MOF / PEI prepared in Example 1 of the present invention and PEI prepared in Comparative Example 2 are shown. Figure 4 The peak of CNO(Ce)@MOF / PEI at 531.48 eV in (b) is Figure 4 The O1s orbital of the PEI composite material in (a) is slightly shifted to the right, which is mainly the result of the Zn-O bond, resulting in a new chemical coordination environment after MOF shell coating, further proving the close connection between calcium cerium niobate and the MOF shell.
[0110] Figure 5 The dielectric properties of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2 are shown in the figure. 3 At 1.5 Hz, the dielectric constant of pure PEI is only 3.14, while the dielectric constant of the composite material with 0.5 wt% of the filling component is significantly increased to 3.25, and with the increase of the filling amount, the dielectric constant is further increased, and the highest dielectric constant of 3.64 is reached when the filling amount is 1.5 wt%, which is 16% higher than that of pure PEI. At the same time, the dielectric loss of each component polymer-based composite material is lower than 0.05 in each frequency band, and the composite material filled with inorganic fillers has significantly reduced dielectric loss.
[0111] Figure 6 The energy storage performance of CNO(Ce)@MOF / PEI prepared in Examples 1 to 3 of the present invention and PEI prepared in Comparative Example 2 is shown in the figure. As can be seen from the figure, with the filling of calcium barium niobate, the discharge energy density of the composite dielectric gradually increases while maintaining a relatively high charge and discharge efficiency under the same electric field.
[0112] Example 4
[0113] (1) Preparation of cerium calcium niobate powder
[0114] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10The (Ce) powder was added into 100 ml (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder.
[0115] (2) Preparation of calcium cerium niobate filler
[0116] Dissolve calcium cerium niobate powder in methanol solution, add zinc nitrate hexahydrate methanol solution to calcium cerium niobate methanol solution under ultrasonic conditions, stir for 30 seconds, add dimethyl imidazole methanol solution to zinc nitrate methanol solution containing calcium cerium niobate, ultrasonicate for 1 to 2 minutes, and let stand for 60 minutes. Centrifuge at 10000 r min -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish and freeze-dried to obtain calcium cerium niobate filler.
[0117] (3) Preparation of a dispersion containing filler
[0118] 0.113 g of calcium cerium niobate filler was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0119] (4) Preparation of diamine dispersion
[0120] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, which was then added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler.
[0121] (5) Preparation of polyetheramide acid sol
[0122] In an ice water bath, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing the composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amide acid sol.
[0123] (6) Preparation of polyetherimide film
[0124] A 10 μm layer of polyetheramide acid sol was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, and kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each, and then cooled to obtain a polyetherimide film.
[0125] Example 5
[0126] (1) Preparation of cerium calcium niobate powder
[0127] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10 The (Ce) powder was added into 100 ml (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder.
[0128] (2) Preparation of calcium cerium niobate filler
[0129] Dissolve calcium cerium niobate powder in methanol solution, add zinc nitrate hexahydrate methanol solution to calcium cerium niobate methanol solution under ultrasonic conditions, stir for 30 seconds, add dimethyl imidazole methanol solution to zinc nitrate methanol solution containing calcium cerium niobate, ultrasonicate for 1 to 2 minutes, and let stand for 60 minutes. Centrifuge at 10000 r min -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish and freeze-dried to obtain calcium cerium niobate filler.
[0130] (3) Preparation of a dispersion containing filler
[0131] 0.142 g of calcium cerium niobate filler was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0132] (4) Preparation of diamine dispersion
[0133] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, which was then added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler.
[0134] (5) Preparation of polyetheramide acid sol
[0135] In an ice water bath, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing the composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amide acid sol.
[0136] (6) Preparation of polyetherimide film
[0137] A 10 μm layer of polyetheramide acid sol was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, and kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each, and then cooled to obtain a polyetherimide film.
[0138] Example 6
[0139] (1) Preparation of cerium calcium niobate powder
[0140] K2CO3, CaCO3, Nb2O5 and CeO2 powders were weighed in a molar ratio of 1.1:1.9:3:0.1, and the mixture was ground evenly in anhydrous ethanol and dried in an oven at 80°C. The dried product was placed in a porcelain boat and calcined in a muffle furnace at 1200°C for 12 hours to obtain KCa2Nb3O 10 (Ce) perovskite precursor. 2.5 g of KCa2Nb3O 10 The (Ce) powder was added into 100 ml (5 M) fuming nitric acid solution and magnetically stirred for 72 h. The replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder.
[0141] (2) Preparation of calcium cerium niobate filler
[0142] Dissolve calcium cerium niobate powder in methanol solution, add zinc nitrate hexahydrate methanol solution to calcium cerium niobate methanol solution under ultrasonic conditions, stir for 30 seconds, add dimethyl imidazole methanol solution to zinc nitrate methanol solution containing calcium cerium niobate, ultrasonicate for 1 to 2 minutes, and let stand for 60 minutes. Centrifuge at 10000 r min -1 Perform multiple centrifugation, taking 3000r min -1 The supernatant was transferred to a culture dish and freeze-dried to obtain calcium cerium niobate filler.
[0143] (3) Preparation of a dispersion containing filler
[0144] 0.171 g of calcium cerium niobate filler was dissolved in 20 ml of N-methyl-2-pyrrolidone (NMP) solvent to obtain a dispersion containing the filler.
[0145] (4) Preparation of diamine dispersion
[0146] In an ice-water bath, 1.5 g of 4,4-diaminodiphenyl ether (ODA) was added to 20 ml of N-methyl-2-pyrrolidone (NMP), and ultrasonicated for 1 min to obtain a diamine dispersion, which was then added to the dispersion of the filler to obtain a diamine dispersion containing a composite filler.
[0147] (5) Preparation of polyetheramide acid sol
[0148] In an ice water bath, a total of 4 g of bisphenol A diether dianhydride (BPADA) was added to the diamine dispersion containing the composite filler in seven times, with 1 g, 1 g, 1 g, 0.5 g, 0.2 g, 0.2 g, and 0.1 g added each time. After each addition, an external shear force was used for stirring for 20 min, 20 min, 20 min, 20 min, 10 min, 10 min, and 60 min to obtain a polyether amide acid sol.
[0149] (6) Preparation of polyetherimide film
[0150] A 10 μm layer of polyetheramide acid sol was coated on the surface of a clean glass substrate, dried at 80°C in an air atmosphere for 12 h, and kept at 100°C, 150°C, 200°C, 250°C, and 300°C for 1 h each, and then cooled to obtain a polyetherimide film.
[0151] Example 7
[0152] A method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, comprising the following steps:
[0153] S1: Add K2CO3, CaCO3, Nb2O5 and CeO2 powders with a molar ratio of 1.1:1.9:3:0.05 into anhydrous ethanol, grind evenly, and place in an oven for drying. The dried product is placed in a porcelain boat, placed in a muffle furnace, and calcined at 1100℃ for 12h to obtain KCa2Nb3O 10 (Ce) perovskite precursor. KCa2Nb3O 10 The (Ce) powder was added to the fuming nitric acid solution and magnetically stirred for 72 hours, and the replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies;
[0154] S2: Under ultrasonic conditions, a methanol solution of zinc nitrate was added to a methanol solution of calcium cerium niobate nanosheets. After stirring evenly, a methanol solution of dimethylimidazole was added, and then the mixture was allowed to react for 50 minutes to obtain a calcium cerium niobate@MOF composite filler. The mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole was 0.05:0.07:0.66.
[0155] S3: In an ice-water bath, 4,4-diaminodiphenyl ether (ODA) is added to N-methyl-2-pyrrolidone (NMP), and ultrasonic dispersion is performed to obtain a diamine dispersion; and the diamine dispersion is added to the dispersion of the calcium niobate cerium @MOF composite filler, and stirred evenly to obtain a diamine dispersion containing the calcium niobate cerium @MOF composite filler; bisphenol A diether dianhydride (BPADA) is added to the diamine dispersion containing the calcium niobate cerium @MOF composite filler in batches, and the amount added is from more to less. During the addition of bisphenol A diether dianhydride, external shear force stirring is maintained. The bisphenol A diether dianhydride can be added in 7 times, and stirring is continued after each addition. The stirring time can be 20min, 20min, 20min, 20min, 10min, 10min, 60min n, stirring the reaction to end, and obtaining a calcium cerium niobate @MOF / polyether amide acid composite sol, wherein the ratio of the mass of the calcium cerium niobate @MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is 0.5:100; coating the calcium cerium niobate @MOF / polyether amide acid composite sol on a clean glass substrate to obtain a calcium cerium niobate @MOF / polyether amide acid composite film, the thickness of the composite film can preferably be 8μm; placing the calcium cerium niobate @MOF / polyether amide acid composite film at 80°C, drying it in an air atmosphere for 12h, and performing a gradient temperature imidization treatment in an air atmosphere within a temperature range of 100°C to 300°C, and heat-keeping treatment at each temperature for 1h, with a temperature interval of 50°C, to obtain a calcium cerium niobate @MOF / polyether imide composite dielectric containing oxygen vacancies.
[0156] Example 8
[0157] A method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, comprising the following steps:
[0158] S1: Add K2CO3, CaCO3, Nb2O5 and CeO2 powders with a molar ratio of 1.1:1.9:3:0.1 into anhydrous ethanol, grind evenly, and place in an oven for drying. The dried product is placed in a porcelain boat, placed in a muffle furnace, and calcined at 1200℃ for 12h to obtain KCa2Nb3O 10 (Ce) perovskite precursor. KCa2Nb3O 10The (Ce) powder was added to the fuming nitric acid solution and magnetically stirred for 120 hours, and the replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies;
[0159] S2: Under ultrasonic conditions, a methanol solution of zinc nitrate was added to a methanol solution of calcium cerium niobate nanosheets, and after stirring evenly, a methanol solution of dimethylimidazole was added, and then allowed to react for 60 minutes to obtain a calcium cerium niobate@MOF composite filler; the mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole was 0.15:0.07:0.66.
[0160] S3: In an ice-water bath, 4,4-diaminodiphenyl ether (ODA) is added to N-methyl-2-pyrrolidone (NMP), and ultrasonic dispersion is performed to obtain a diamine dispersion; and the diamine dispersion is added to the dispersion of the calcium niobate cerium @MOF composite filler, and stirred evenly to obtain a diamine dispersion containing the calcium niobate cerium @MOF composite filler; bisphenol A diether dianhydride (BPADA) is added to the diamine dispersion containing the calcium niobate cerium @MOF composite filler in batches, and the amount added is from more to less. During the addition of bisphenol A diether dianhydride, external shear force stirring is maintained. The bisphenol A diether dianhydride can be added in 7 times, and stirring is continued after each addition. The stirring time can be 20min, 20min, 20min, 20min, 10min, 10min, 60min n, stirring the reaction to end, and obtaining a calcium cerium niobate @MOF / polyether amide acid composite sol, wherein the ratio of the mass of the calcium cerium niobate @MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is 3.0:100; coating the calcium cerium niobate @MOF / polyether amide acid composite sol on a clean glass substrate to obtain a calcium cerium niobate @MOF / polyether amide acid composite film, the thickness of the composite film can preferably be 10 μm; placing the calcium cerium niobate @MOF / polyether amide acid composite film at 80°C, drying it in an air atmosphere for 12 hours, and performing a gradient temperature imidization treatment in an air atmosphere within a temperature range of 100°C to 300°C, and heat-keeping treatment at each temperature for 1 hour, with a temperature interval of 50°C, to obtain a calcium cerium niobate @MOF / polyether imide composite dielectric containing oxygen vacancies.
[0161] Example 9
[0162] A method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, comprising the following steps:
[0163] S1: Add K2CO3, CaCO3, Nb2O5 and CeO2 powders with a molar ratio of 1.1:1.9:3:0.08 into anhydrous ethanol, grind evenly, and place in an oven for drying. The dried product is placed in a porcelain boat, placed in a muffle furnace, and calcined at 1100℃ for 13h to obtain KCa2Nb3O 10 (Ce) perovskite precursor. KCa2Nb3O 10 (Ce) powder was added to the fuming nitric acid solution and magnetically stirred for 100 hours, and the replaced product was washed with deionized water until neutral and dried to obtain calcium cerium niobate powder containing oxygen vacancies;
[0164] S2: Under ultrasonic conditions, a methanol solution of zinc nitrate was added to a methanol solution of calcium cerium niobate nanosheets. After stirring evenly, a methanol solution of dimethylimidazole was added, and then the mixture was allowed to react for 55 minutes to obtain a calcium cerium niobate@MOF composite filler. The mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole was 0.1:0.07:0.66.
[0165] S3: In an ice-water bath, 4,4-diaminodiphenyl ether (ODA) is added to N-methyl-2-pyrrolidone (NMP), and ultrasonic dispersion is performed to obtain a diamine dispersion; and the diamine dispersion is added to the dispersion of the calcium niobate cerium @MOF composite filler, and stirred evenly to obtain a diamine dispersion containing the calcium niobate cerium @MOF composite filler; bisphenol A diether dianhydride (BPADA) is added to the diamine dispersion containing the calcium niobate cerium @MOF composite filler in batches, and the amount added is from more to less. During the addition of bisphenol A diether dianhydride, external shear force stirring is maintained. The bisphenol A diether dianhydride can be added in 7 times, and stirring is continued after each addition. The stirring time can be 20min, 20min, 20min, 20min, 10min, 10min, 60m in, stirring the reaction to end, and obtaining a calcium cerium niobate @MOF / polyether amide acid composite sol, wherein the ratio of the mass of the calcium cerium niobate @MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is 2:100; coating the calcium cerium niobate @MOF / polyether amide acid composite sol on a clean glass substrate to obtain a calcium cerium niobate @MOF / polyether amide acid composite film, the thickness of the composite film can preferably be 9 μm; placing the calcium cerium niobate @MOF / polyether amide acid composite film at 80°C, drying it in an air atmosphere for 12 hours, and performing a gradient temperature imidization treatment in an air atmosphere within a temperature range of 100°C to 300°C, and heat-keeping treatment at each temperature for 1 hour, with a temperature interval of 50°C, to obtain a calcium cerium niobate @MOF / polyether imide composite dielectric containing oxygen vacancies.
[0166] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
[0167] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, characterized in that: The following steps are involved: S1: K2CO3, CaCO3, Nb2O5 and CeO2 were added to ethanol and ground evenly, dried and calcined to obtain KCa2Nb3O 10 (Ce) perovskite precursor, the KCa2Nb3O 10 (Ce) The perovskite precursor is added to fuming nitric acid and magnetically stirred to obtain calcium cerium niobate powder containing oxygen vacancies; S2: adding zinc nitrate to the dispersion of the calcium cerium niobate powder containing oxygen vacancies, stirring and mixing evenly, and then adding dimethyl imidazole, standing for reaction, to obtain a calcium cerium niobate@MOF composite filler; S3: adding the calcium cerium niobate @MOF composite filler into N-methyl-2-pyrrolidone, and adding 4,4'-diaminodiphenyl ether and bisphenol A dianhydride, stirring the reaction, and obtaining a calcium cerium niobate @MOF / polyetheramic acid composite sol; preparing the calcium cerium niobate @MOF / polyetheramic acid composite sol into a calcium cerium niobate @MOF / polyetheramic acid composite film, and performing imidization treatment to obtain the calcium cerium niobate @MOF / polyetherimide composite dielectric containing oxygen vacancies.
2. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S1, the molar ratio of K2CO3, CaCO3, Nb2O5 and CeO2 is 1.1:1.9:3:(0.05-0.1).
3. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S1, during the calcination treatment, the calcination temperature is 1100-1200° C. and the calcination time is 12-14 hours.
4. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S1, KCa2Nb3O 10 (Ce) The perovskite precursor is added to the fuming nitric acid solution and magnetically stirred for 72 to 120 hours.
5. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S2, the mass ratio of the calcium cerium niobate powder to zinc nitrate and dimethylimidazole is (0.05-0.15):0.07:0.
66.
6. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S2, the reaction is allowed to stand for 50 to 60 minutes.
7. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: In step S3, the ratio of the mass of the calcium cerium niobate@MOF composite filler to the total mass of 4,4'-diaminodiphenyl ether and bisphenol A dianhydride is (0.5-3.0):
100.
8. The method for preparing a calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies according to claim 1, characterized in that: The thickness of the calcium cerium niobate@MOF / polyetheramic acid composite film is 7-13 μm.
9. A calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies, characterized in that: It is prepared by the method according to any one of claims 1 to 8.
10. Use of the calcium cerium niobate@MOF / polyetherimide composite dielectric containing oxygen vacancies as described in claim 9 in a capacitor.
Citation Information
Patent Citations
Preparation method of modified strontium titanium niobate nanosheet / polyimide-based energy storage dielectric composite material
CN117362719A
Preparation method of polyetherimide-based nano composite material for energy storage dielectric
CN117362721A
Preparation of indium tin oxide nano-sized particleand conduction film used as display material
KR1020050037729A