Ethylene copolymer with improved melting temperature and glass transition temperature

By mixing ethylene α-olefin copolymers to increase their melting and glass transition temperatures, the problem of slow injection and cooling time of ethylene α-olefin copolymers in the prior art is solved, and faster injection and shorter cooling time is achieved. Improves the economics of the process.

CN118978761APending Publication Date: 2024-11-19BOREALIS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048401.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-27
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing ethylene alpha-olefin copolymers have slow problems during injection and cooling, resulting in limited process economy and the need for improved injection and cooling time.

Method used

By mixing different ethylene alpha-olefin copolymers, their melting and glass transition temperatures are significantly increased, thereby accelerating injection and shortening cooling time while keeping the density and melt flow rate unchanged.

Benefits of technology

Faster injection and shorter cooling times are achieved, improving process economy while maintaining the density and mass average molecular weight of the target ethylene alpha-olefin copolymer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974163620000051
    Figure BDA0004974163620000051
  • Figure BDA0004974163620000052
    Figure BDA0004974163620000052
  • Figure BDA0004974163620000053
    Figure BDA0004974163620000053
Patent Text Reader

Abstract

The invention relates to a copolymer of ethylene and a C3 to C8 alpha-olefin wherein the copolymer has a density, measured according to ISO 1183, of from 890 kg / m3 to 915 kg / m3, an MFR2, measured according to ISO 1133, of from 0.5 g / 10 min to 8.0 g / 10 min, and wherein the alpha-olefin is present in the copolymer in an amount of from 10 wt.% to 20 wt.%, and wherein the copolymer has a melting point, Tm, measured according to ISO 11357-3, of between 100 DEG C and 120 DEG C, and a Vicat softening temperature, Tvicat, of from 80 DEG C to 96 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the PCT national phase application entering China with an application date of September 27, 2021, a date of entry into the Chinese national phase of March 21, 2023, an application number of 202180064536.8 (international application number is PCT / EP2021 / 076517), and an invention name of “Ethylene copolymers with improved melting temperature and glass transition temperature”. Technical Field

[0002] The present invention relates to ethylene copolymers with improved melting temperature, in particular to ethylene α-olefin copolymers with improved melting temperature. The present invention also relates to such ethylene α-olefin copolymers obtained by mixing different ethylene copolymers. Background Art

[0003] Among polyolefin plastomers and polyolefin elastomers, ethylene alpha-olefin copolymers (EOC) are widely used. Ethylene alpha-olefin plastomers are used in various applications such as seals, flexible packaging and rigid packaging. Ethylene alpha-olefin copolymers are particularly used in impact-modified blends of polypropylene homopolymers and copolymers. Ethylene alpha-olefin elastomers are used in applications such as automotive interior and exterior parts, adhesives, cable compounds, etc.

[0004] Some current technical grades of ethylene alpha-olefin copolymers have good properties, but do have the disadvantage of slow injection, particularly before or during copolymer extrusion, which results in a long cooling time. This behavior has a negative impact on the process economics of some applications. Therefore, it is advantageous to obtain improved ethylene alpha-olefin copolymers, the target of which is the same or similar grade, but with faster injection and therefore shorter cooling time. In other words, there is a need in the art to improve the injection and cooling time of the ethylene alpha-olefin copolymers of this target. Summary of the invention

[0005] It is therefore an object of the present invention to provide ethylene alpha-olefin copolymers having improved spraying and shorter cooling times.

[0006] Another object of the present invention is to provide an ethylene alpha-olefin copolymer having improved spraying and shorter cooling time compared to the target ethylene alpha-olefin copolymer.

[0007] A particular object of the present invention is to provide ethylene alpha-olefin copolymers having improved spraying and shorter cooling times compared to target ethylene alpha-olefin copolymers, but at the same time maintaining the density and MFR2 of these target ethylene alpha-olefin copolymers.

[0008] It has surprisingly been found in the present invention that the blending of two different ethylene α-olefin copolymers can give a copolymer having a significantly higher melting temperature Tm and improved glass transition temperature T g The ethylene α-olefin copolymer of the present invention is characterized by maintaining the target density and melt flow rate of the ethylene α-olefin copolymer. The higher melting temperature T m and improved glass transition temperature T g Helps result in faster ejection and shorter cool down times.

[0009] Therefore, the present invention provides a copolymer of ethylene and a C3 to C8 α-olefin, wherein the density of the copolymer according to ISO 1183 is 890 kg / m 3 Up to 915kg / m 3 , and an MFR2 according to ISO 1133 of 0.5 g / 10 min to 8.0 g / 10 min, wherein the amount of the α-olefin present in the copolymer is 10 wt.% to 20 wt.%, wherein the melting temperature T of the copolymer measured according to ISO 11357-3 m Between 100℃ and 120℃, the Vicat softening temperature T vicat 80℃ to 96℃.

[0010] The ethylene α-olefin copolymers of the present invention have several surprising advantages. First, the ethylene α-olefin copolymers of the present invention maintain the density and MFR2 of their target ethylene α-olefin copolymers. Second, they can maintain the mass average molecular weight Mw and comonomer content of their target ethylene α-olefin copolymers. Third, the ethylene α-olefin copolymers of the present invention have improved melting temperatures T while meeting the density, MFR2, comonomer content and Mw requirements. m and improved glass transition temperature T g The latter property allows for faster ejection and shorter cooling times, which in turn improves process economics in some applications.

[0011] The copolymer according to the present invention is a copolymer of ethylene as a monomer and a comonomer, the comonomer being an α-olefin of C3 to C8. The term "α-olefin of C3 to C8" means that the α-olefin contains 3 to 8 carbon atoms, and also includes α-olefins of C4, C5, C6 and C7. C3 represents propylene, C4 represents butene, C5 represents pentene, C6 represents hexene, C7 represents heptene and C8 represents octene.

[0012] Preferably, the C3 to C8 α-olefin is a C8 α-olefin, i.e. octene. Preferably, the copolymer is a copolymer of ethylene and octene.

[0013] The α-olefin is preferably present in the copolymer in an amount of 12 to 18 wt.%, more preferably 13 to 17 wt.%, most preferably 14.5 to 15.5 wt.%.

[0014] Preferably, the density of the copolymer measured according to ISO 1183 is 895 kg / m 3 Up to 910kg / m 3 .

[0015] The MFR2 of the copolymer measured according to ISO 1133 is preferably from 0.6 to 4.0 g / 10 min, preferably from 0.7 to 3.0 g / 10 min, more preferably from 0.9 to 1.5 g / 10 min.

[0016] The MFR of the copolymer measured according to ISO 1133 21 It is preferably 30 g / 10 min to 45 g / 10 min, more preferably 32 g / 10 min to 40 g / 10 min, most preferably 34 g / 10 min to 38 g / 10 min.

[0017] The copolymer has a specific MFR 21 / MFR2 is preferably 30 to 45, more preferably 32 to 40, most preferably 34 to 38.

[0018] The Mw / Mn of the copolymer is preferably from 2.5 to 3.0, most preferably from 2.6 to 2.8.

[0019] The Mw of the copolymer is preferably 75000 g / mol to 90000 g / mol, more preferably 78000 g / mol to 87000 g / mol, most preferably 81000 g / mol to 84000 g / mol. Mw represents the weight average molecular weight.

[0020] The copolymers of the invention are characterized by a melting temperature T between 100° C. and 120° C., measured according to ISO 11357-3. m Preferably, the melting temperature T measured according to ISO 11357-3 m It is between 101°C and 110°C, most preferably between 102°C and 105°C.

[0021] The crystallization temperature T of the copolymer c It is preferably 82°C to 96°C, more preferably 84°C to 94°C, more preferably 86°C to 92°C, most preferably 88°C to 91°C.

[0022] The glass transition temperature T gIt is preferably -35°C to -45°C, more preferably -37°C to -43°C, most preferably -40°C to -42°C.

[0023] The copolymers according to the invention are preferably further characterized by the content of unsaturated groups per 100,000 carbon atoms. These unsaturated groups are vinylene (R2C=CH2), vinyl (RHC=CH2), trisubstituted vinylene (R2C=CHR) and vinylene (RHC=CHR).

[0024] The copolymer preferably has a vinyl content of 4.0 to 8.0 vinyl groups per 100,000 carbon atoms, more preferably 4.5 to 7.5 vinyl groups, most preferably 4.9 to 7.0 vinyl groups.

[0025] The copolymer preferably has a vinylidene content of 9.0 to 14 vinylidene groups, preferably 11.0 to 12.5 vinylidene groups per 100,000 carbon atoms.

[0026] The trisubstituted vinylene content of the copolymer is preferably 15.0 to 24.0 trisubstituted vinylene groups, more preferably 16.0 to 23.0 trisubstituted vinylene groups, and most preferably 17.0 to 22 trisubstituted vinylene groups per 100,000 carbon atoms.

[0027] The copolymer preferably has a vinylene content of 10.0 to 16.0 vinylene groups, preferably 12.0 to 15.0 vinylene groups per 100,000 carbon atoms.

[0028] Preparation method

[0029] The copolymer according to the present invention is preferably produced by mixing two ethylene copolymers. Preferably, the copolymer according to the present invention is obtained by mixing a first ethylene copolymer and a second ethylene copolymer, wherein the first ethylene copolymer has a higher density than the second ethylene copolymer.

[0030] Preferably, each of the first ethylene copolymer and / or the second ethylene copolymer is produced in a high temperature solution polymerization process at a temperature above 100°C. Such a process is essentially based on the polymerization of monomers (i.e. ethylene) and suitable comonomers (i.e. C3 to C8 α-olefins, preferably octene) in a hydrocarbon solvent which is liquid under the polymerization conditions and in which the polymer formed is soluble. The polymerization reaction is carried out at a temperature above the melting point of the polymer, resulting in a polymer solution. The solution is flashed in multiple steps to separate the polymer from the unreacted monomers and the solvent. In this process, the solvent is then recovered and recycled.

[0031] The solution polymerization process is known for its shorter reactor residence time (compared to gas phase or slurry phase processes), thus allowing very fast grade changeovers and significant flexibility in producing a wide range of products in short production cycles.

[0032] The solution polymerization process used for each of the first ethylene copolymer and the second ethylene copolymer is a high temperature solution polymerization process, and the polymerization temperature used is higher than 100° C. Preferably, the polymerization temperature is at least 110° C., more preferably at least 150° C. The polymerization temperature can be as high as 250° C.

[0033] The pressure of each of the first ethylene copolymer and the second ethylene copolymer in the reactor depends on the temperature on the one hand and on the type and content of the comonomer on the other hand. The pressure is preferably 50 bar to 300 bar, preferably 60 bar to 250 bar, more preferably 70 bar to 200 bar.

[0034] The process comprises one or more polymerization reactors. Suitable reactors include unstirred or stirred, spherical, cylindrical and tank-shaped vessels, circulating loop reactors and tubular reactors. Such reactors usually contain feed points for monomers, optional comonomers, solvents, catalysts, optional other reactants and additives and extraction points for polymer solutions. In addition, the reactor may contain heating or cooling devices.

[0035] The hydrocarbon solvent used is preferably C5 -12 Hydrocarbons, which may be unsubstituted or substituted with C 1-4 The unsubstituted C 6-10 Hydrocarbon solvents.

[0036] In addition, other components may be added to the reactor. It is known that hydrogen is added to the reactor to control the molecular weight of the polymer formed during the polymerization process. The use of different antifouling compounds is also known in the art. In addition, different types of active promoters or active retarders may be used to control the activity of the catalyst.

[0037] A preferred process for preparing each of the first ethylene copolymer and the second ethylene copolymer is a high temperature solution process as described above, preferably at a temperature greater than 100°C and in the presence of a metallocene catalyst system, the metallocene catalyst system comprising, or consisting of,

[0038] (i) at least one metallocene complex,

[0039] (ii) an aluminoxane cocatalyst and / or a boron-containing cocatalyst, and

[0040] (iii) optionally an alkyl aluminum compound Al(R 7 )3, where R 7 It is a linear or branched C2-C8 alkyl group.

[0041] Preferably, the at least one metallocene complex (i) comprises or consists of a metallocene complex of formula (I).

[0042]

[0043] Where M is Hf,

[0044] X is a σ ligand,

[0045] R can be the same or different and can be a saturated straight chain or branched C1-C 10 Alkyl, C6-C 10 Aryl, C4-C 10 Heteroaryl, C6-C 20 Alkyl aryl or C6-C 20 arylalkyl radicals, which may optionally contain up to 2 heteroatoms or silicon atoms,

[0046] R 1 C6-C 10 Aryl or C6-C 20 Alkyl aryl, optionally containing up to 2 heteroatoms or silicon atoms or C4-C 10 The heteroaryl group,

[0047] R 2 C4-C 20 Cycloalkyl, optionally carrying an alkyl substituent in the β position of formula (II)

[0048]

[0049] wherein R' may be the same or different from each other, and R may be hydrogen, or may be defined as R, and n is 1 to 17,

[0050] and / or

[0051] The metallocene complex (i) comprises or consists of a metallocene complex of formula (III):

[0052]

[0053] Where M is Hf,

[0054] X is a σ ligand,

[0055] R can be the same or different and can be a saturated straight chain or branched C1-C 10 Alkyl, C5-C 10Aryl, C6-C 20 Alkyl aryl or C6-C 20 arylalkyl groups which may optionally contain up to 2 heteroatoms or silicon atoms,

[0056] R 1 C6-C 20 Aryl, which may be unsubstituted or substituted with one or up to 5 straight or branched C1-C 10 Alkyl substitution,

[0057] R 2 It is an unsaturated straight chain or cyclic C3-C 20 Alkyl or branched CR 3 R 4 R 5 Group, where R 3 is hydrogen or C1-C 20 Alkyl, R 4 and R 5 Same or different, can be C1-C 20 alkyl.

[0058] Preferably, the at least one metallocene complex of formula (I) is a metallocene complex of formula (Ia).

[0059]

[0060] Preferably, the at least one metallocene complex of formula (III) is a metallocene complex of formula (IIIa).

[0061]

[0062] ((Phenyl)(3-buten-1-yl)methylene(cyclopentadienyl)(2,7-di-tert-butylfluoren-9-yl)hafnium dimethyl),

[0063] Most preferably, (Phenyl)(cyclohexyl)methylene(cyclopentadienyl)(2,7-di-tert-butylfluoren-9-yl)hafnium dimethyl is used as the metallocene complex (i).

[0064] The metallocene complexes of the above formula (I) and formula (III) and their preparation are described in more detail in WO2018108917 and WO2018108918.

[0065] As cocatalyst (ii), it is possible to use an aluminoxane-containing or boron-containing cocatalyst or a mixture thereof.

[0066] The aluminoxane cocatalyst is one of formula (IV)

[0067]

[0068] wherein n is 6 to 20, and R has the following meanings.

[0069] Aluminoxanes are formed by partial hydrolysis of organoaluminum compounds, such as those of the formulas AIR3, AIR2Y, and Al2R3Y3, where R can be, for example, C1-C 10 Alkyl, preferably C1-C5 alkyl, or C3-C 10 Cycloalkyl, C7-C 12 Arylalkyl or alkylaryl and / or phenyl or naphthyl, and wherein Y can be hydrogen, halogen (preferably chlorine or bromine) or C1-C 10 Alkoxy (preferably methoxy or ethoxy). The oxygen-containing aluminoxane obtained is generally not a pure compound but a mixture of oligomers of formula (IV).

[0070] A preferred aluminoxane is methylaluminoxane (MAO).

[0071] Since the aluminoxanes used as cocatalysts according to the invention are not pure compounds due to the way they are prepared, the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.

[0072] Since the aluminoxanes used as cocatalysts according to the invention are not pure compounds due to the way they are prepared, the molar concentrations of the aluminoxane solutions hereinafter are based on their aluminum content.

[0073] The molar ratio of Al in aluminoxane to the transition metal of the metallocene is in the range of 1:1 mol / mol to 2000:1 mol / mol, preferably 10:1 mol / mol to 1000:1 mol / mol, more preferably 50:1 mol / mol to 500:1 mol / mol.

[0074] Appropriate amounts of promoter are well known to those skilled in the art.

[0075] In the embodiment of the aluminoxane (ii) of the present invention, methylaluminoxane and the formula Al(R 7 ) 3 as a co-catalyst, wherein R7 It is a linear or branched C2-C8 alkyl group (iii).

[0076] In this case, the cocatalyst is preferably an aluminoxane (ii), preferably a reaction product of methylaluminoxane and an alkylaluminum compound (iii), such as triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum, triisooctylaluminum, etc. The ratio between methylaluminoxane and the alkylaluminum compound may be between 10:1 and 1:10, preferably 5:1 to 1:5, most preferably 3:1 to 1:3 of the mole ratio of aluminum in methylaluminoxane to the mole ratio of aluminum in the alkylaluminum compound. The reaction between methylaluminoxane and the alkylaluminum compound is carried out by mixing the two components in a suitable solvent, which may be aromatic or aliphatic, at a reaction temperature between -50°C and +80°C, preferably between 10°C and 50°C, and more preferably between 20°C and 40°C.

[0077] Related boron-based co-catalysts include boron compounds containing borate 3+ ions, i.e., borate compounds. These compounds generally contain anions of the formula:

[0078] (Z)4B - (V)

[0079] Wherein Z is an optionally substituted phenyl derivative, the substituent being a halogenated C 1-6 An alkyl or halogen group. Preferably, it is fluoro or trifluoromethyl. Most preferably, the phenyl group is perfluorinated.

[0080] Such ionic promoters preferably contain a non-coordinating anion, such as tetrakis(pentafluorophenyl)borate.

[0081] Suitable counterions are protonated amine or aniline derivatives or phosphonium ions. These may have the general formula (VI) or (VII):

[0082] NQ4 + (VI) or PQ4 + (VII)

[0083] Wherein Q is independently H, C1-6 alkyl, C3-8 cycloalkyl, phenyl C1-6 alkylene or optionally substituted phenyl. Optional substituents can be C1-6 alkyl, halogen or nitro. One or more such substituents can be present. Therefore, preferred substituted phenyl includes para-substituted phenyl, preferably tolyl or xylphenyl.

[0084] It is preferred if at least one Q group is H, and preferred compounds are therefore those of the formula:

[0085] NHQ3 + (VIII) or PHQ3 + (IX)

[0086] Preferred phenyl C1-6 alkyl groups include benzyl.

[0087] Thus, suitable counterions include: methylammonium, anilinium, dimethylammonium, diethylammonium, N-methylanilinium, diphenylammonium, N,N-dimethylaniline, trimethylammonium, triethylammonium, tri-n-butylammonium, methyldiphenylammonium, p-bromo-N,N-dimethylaniline or p-nitro-N,N-dimethylaniline, especially dimethylammonium or N,N-dimethylaniline. Using pyridinium salts as counterions is a further option.

[0088] Relevant phosphine ions include triphenylphosphine, triethylphosphine, diphenylphosphine, tri(methylphenyl)phosphine and tri(dimethylphenyl)phosphine.

[0089] A more preferred counterion is trityl (CPh3 + ) or its analogues, wherein the phenyl group is functionalized to carry one or more alkyl groups. Thus, highly preferred borates for use in the present invention comprise tetrakis(pentafluorophenyl)borate ions.

[0090] Preferred ionic compounds for use according to the present invention include:

[0091] Tributylammoniumtetra(pentafluorophenyl)borate,

[0092] Tributylammoniumtetra(trifluoromethylphenyl)borate, Tributylammoniumtetra-(4-fluorophenyl)borate,

[0093] N,N-dimethylcyclohexylammoniumtetrakis-(pentafluorophenyl)borate,

[0094] N,N-dimethylbenzylammoniumtetrakis(pentafluorophenyl)borate,

[0095] N,N-dimethylaniliniumtetrakis(pentafluorophenyl)borate,

[0096] N,N-di(propyl)ammoniumtetrakis(pentafluorophenyl)borate,

[0097] di(cyclohexyl)ammoniumtetrakis(pentafluorophenyl)borate,

[0098] Triphenylcarbeniumtetrakis(pentafluorophenyl)borate, ferroceniumtetrakis(pentafluorophenyl)borate.

[0099] Triphenylcarbonium tetrakis(pentafluorophenyl)borate,

[0100] N,N-dimethylcyclohexylammonium tetrakis(pentafluorophenyl)borate,

[0101] N,N-dimethylbenzylammonium tetrakis(pentafluorophenyl)borate or

[0102] N,N-Dimethylanilinium tetrakis(pentafluorophenyl)borate.

[0103] More preferred borates are triphenylcarbonium tetrakis(pentafluorophenyl)borate and N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate.

[0104] N,N-Dimethylanilinium tetrakis(pentafluorophenyl)borate is most preferred.

[0105] Alkyl aluminum compounds may be further added. Suitable alkyl aluminum compounds are compounds of formula (VIII) AlR3, where R is a linear or branched C2-C8 alkyl group.

[0106] Preferred alkylaluminum compounds are triethylaluminum, triisobutylaluminum, triisohexylaluminum, tri-n-octylaluminum and triisooctylaluminum.

[0107] Suitable levels of promoters are well known to those skilled in the art.

[0108] The molar ratio of boron to the metal ion of the metallocene may be in the range of 0.5:1 mol / mol to 10:1 mol / mol, preferably 1:1 mol / mol to 10:1 mol / mol, and particularly 1:1 mol / mol to 5:1 mol / mol.

[0109] More preferably, the molar ratio of boron to the metal ion of the metallocene is from 1:1 mol / mol to less than 2:1 mol / mol, such as from 1:1 mol / mol to 1.8:1 mol / mol or 1:1 mol / mol to 1.5:1 mol / mol.

[0110] According to the invention, preference is given to using boron-containing cocatalysts as described above.

[0111] Preferably, the density of the first ethylene copolymer measured according to ISO 1183 is between 895 kg / m 3 and 925kg / m 3 More preferably, between 900 kg / m 3 and 915kg / m 3 between.

[0112] Preferably, the density of the second ethylene copolymer measured according to ISO 1183 is between 840 kg / m 3 and 890kg / m 3 between 80kg / m 3 and 885kg / m 3 between.

[0113] The melting temperature T of the first ethylene copolymer measured according to ISO 11357-3 m Preferably between 90°C and 110°C.

[0114] The melting temperature T of the second ethylene copolymer measured according to ISO 11357-3 m Preferably it is between 30°C and 80°C, more preferably between 35°C and 75°C.

[0115] The MFR2 of the first ethylene copolymer measured according to ISO 1133 is preferably from 0.5 g / 10min to 8.0 g / 10min, more preferably from 0.7 g / 10min to 4.0 g / 10min, more preferably from 0.8 g / 10min to 3.0 g / 10min, most preferably from 0.9 g / 10min to 1.5 g / 10min, and / or the MFR2 of the second ethylene copolymer measured according to ISO 1133 is preferably from 0.5 g / 10min to 8.0 g / 10min, more preferably from 0.7 g / 10min to 4.0 g / 10min, more preferably from 0.8 g / 10min to 3.0 g / 10min, most preferably from 0.9 g / 10min to 1.5 g / 10min.

[0116] Preferably, the first ethylene copolymer and the second ethylene copolymer both have the same α-olefin as comonomer, more preferably, the α-olefin of the first ethylene copolymer and the second ethylene copolymer are both octene.

[0117] Preferably, the α-olefin is present in the first ethylene copolymer in an amount of 8 to 15 wt.%, more preferably in an amount of 10 to 14 wt.%.

[0118] Preferably, the α-olefin is present in the second ethylene copolymer in an amount of 20 wt.% to 45 wt.%, more preferably 22 wt.% to 43 wt.%.

[0119] The first ethylene copolymer and the second ethylene copolymer are mixed in a mixing ratio, and their respective amounts are given in wt.%. The mixing ratio of the first ethylene copolymer to the second ethylene copolymer is preferably from 65:35 wt.% to 85:15 wt.%, and more preferably from 69:31 wt.% to 83:27 wt.%.

[0120] The mixing of the first ethylene copolymer as described above with the second ethylene copolymer as described above can be performed in three ways.

[0121] First, the copolymer according to the present invention can be produced online in the device, that is, the first ethylene copolymer and the second ethylene copolymer are produced in a parallel reactor configuration, and then the first ethylene copolymer and the second ethylene copolymer are mixed online to obtain the ethylene copolymer according to the present invention. Suitable equipment and online mixing processes can be found in WO 2017 / 108951A1. In this process, two or more reactors are operated in a parallel configuration, and each reactor produces the same or different intermediate (co) polymers. Downstream of the reactor, the two intermediate (co) polymers are mixed online (preferably before extrusion) to obtain the final (co) polymer. The process disclosed in WO 2017 / 108951 A1 can also be used to produce the copolymer according to the present invention. In particular, the first ethylene copolymer is produced in the first reactor, the second ethylene copolymer is produced in the second reactor in parallel, and the first ethylene copolymer and the second ethylene copolymer are then mixed online according to the process of WO 2017 / 108951 A1. Through this online process, the first ethylene copolymer, the second ethylene copolymer and the final ethylene copolymer according to the present invention can be prepared in the device itself.

[0122] Second, the first ethylene copolymer or the second ethylene copolymer is produced in a suitable device (such as disclosed in WO 2017 / 108951 A1), and then the other of the first ethylene copolymer or the second ethylene copolymer is added, and then mixed (preferably before extrusion) to obtain the final ethylene copolymer according to the present invention. The other of the first ethylene copolymer or the second ethylene copolymer is not produced online, that is, it is not added from the polymerization reactor of the device, but can be pre-produced, for example.

[0123] The 3rd, the mixing of the first ethylene copolymer and the second ethylene copolymer can be completed off-line. The off-line refers to first mixing the first ethylene copolymer and the second ethylene copolymer, followed by compounding (compounding) (e.g., in an extruder). Off-line also means that neither the first ethylene copolymer nor the second ethylene copolymer is produced online, followed by online mixing. Mixing can be, for example, by dry mixing, such as dry mixing of particles of the first ethylene copolymer and the second ethylene copolymer. Alternatively, the first ethylene copolymer and the second ethylene copolymer can be directly fed into an extruder, where they are mixed and extruded. Preferred extruders are twin screw extruders, for example. DETAILED DESCRIPTION

[0124] 1. Test Method

[0125] a) Melt flow rate (MFR) and flow rate ratio (FRR)

[0126] Melt flow rate (MFR) is determined according to ISO1133 - Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics - Part 1: Standard method and is expressed in g / 10min. MFR is an indicator of polymer fluidity and processability. The higher the melt flow rate, the lower the viscosity of the polymer.

[0127] The MFR2 of polypropylene was measured at a temperature of 230°C and a load of 2.16 kg.

[0128] The MFR2 of polyethylene was measured at a temperature of 190°C and a load of 2.16 kg.

[0129] Flow Rate Ratio (FRR) to MFR 21 / MFR2.

[0130] b) Density

[0131] The density of the (co)polymers was measured according to ISO1183.

[0132] c) Comonomer content

[0133] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers.

[0134] A Bruker Avance III 500 NMR spectrometer was used to analyze 1 H and 13 For C, the operation was performed at 500.13 MHz and 125.76 MHz, respectively, and quantitative data were recorded in the molten state. 13 C{ 1 H} NMR spectroscopy. Nitrogen was used for all pneumatics and the temperature was 150 °C. 13 All spectra were recorded with a C-optimized 7 mm magic angle spinning (MAS) probe. Approximately 200 mg of material was packed into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification. Standard single pulse excitation was used, with a transient NOE and RS-HE PT decoupling scheme using a short recycle delay of 3 s. A total of 1024 (1k) transients were acquired for each spectrum.

[0135] Use custom spectral analysis automation procedures to 13 C{ 1 H} NMR spectra were processed, integrated and quantitatively determined. All chemical shifts were internally referenced to the bulk methylene group signal (d+) at 30.00 ppm.

[0136] A characteristic signal corresponding to 1-octene incorporation was observed and all comonomer contents were calculated relative to all other monomers present in the polymer.

[0137] The characteristic signal of isolated 1-octene incorporation, i.e., the EEOEE comonomer sequence, was observed. The isolated 1-octene incorporation was quantified using the signal integral at 38.3 ppm. The integrals were attributed to the unresolved signals of the *B6 and *bB6B6 sites corresponding to the isolated (EEOEE) and isolated di-non-continuous (EEOEOEE) 1-octene sequences, respectively. The integral of the bbb6B6 site at 24.6 ppm was used to compensate for the impact of the two *bB6B6 sites:

[0138] O=I *B6+*bB6B6 -2*I bbB6B6

[0139] A characteristic signal of continuous 1-octene incorporation, namely the EEOOEE comonomer sequence, was also observed. This continuous 1-octene incorporation was quantified using the signal integral at 40.4 ppm attributed to the number of aaB6B6 sites per comonomer reporter site:

[0140] OO=2*I aaB6B6

[0141] The characteristic signal of isolated non-continuous 1-octene incorporation, namely the EEOEOEE comonomer sequence, was also observed. This isolated non-continuous 1-octene incorporation was quantified using the integral of the signal at 24.6 ppm attributed to the number of bbB6B6 sites per comonomer reporter site:

[0142] OEO=2*I bbB6B6

[0143] A characteristic signal of isolated three-consecutive 1-octene incorporation, namely the EEOOOEE comonomer sequence, was also observed. This isolated three-consecutive 1-octene incorporation was quantified using the signal integral at 41.2 ppm attributed to the number of aagB6B6B6 sites per comonomer reporter site:

[0144] OOO=3 / 2*I aagB6B6B6

[0145] The total 1-octene comonomer content was calculated based only on the contents of isolated (EEOEE), isolated di-continuous (EEOOEE), isolated discontinuous (EEOEOEE) and isolated tri-continuous (EEOOOEE) 1-octene comonomer sequences, in the absence of observed signals representing other comonomer sequences:

[0146] O 总 =O+O+OEO+OOO

[0147] Observe the characteristic signals of saturated end groups. Use the average integral of two resolved signals at 22.9 and 32.23ppm to quantify this saturated end group. The integral of 22.84ppm is attributed to the 2B6 and 2S sites of 1-octene and the unresolved signals of the saturated chain ends. The integral of 32.2ppm is attributed to the 3B6 and 3S sites of 1-octene and the unresolved signals of the saturated chain ends. Use the total 1-octene content to compensate for the influence of 2B6 and 3B6 1-octene sites:

[0148] S=(1 / 2)*(I 2s+2B6 +I 3S+3B6 -2*O 总 )

[0149] The ethylene comonomer content was quantified using the integration of the bulk methylene (bulk) signal at 30.00 ppm. This integral includes the D and 4B6 sites from 1-octene as well as the D D The total ethylene copolymer content was calculated based on the bulk integration and compensation for the observed 1-octene sequences and end groups:

[0150] Total E=(1 / 2)*[I 主体 +2*O+1*OO+3*OEO+0*OOO+3*S]

[0151] It should be noted that no compensation for the host integral is required for the presence of isolated tri-incorporated (EEOOOEE) 1-octene sequences since the number of under- and over-counted ethylene units is equal.

[0152] The total mole fraction of 1-octene in the polymer is then calculated:

[0153] fO=O 总 / (E 总 +O 总 )

[0154] The total comonomer incorporation of 1-octene in weight percent was calculated from the mole fractions using standard methods:

[0155] O[wt%]=100*(fO*112.21) / ((fO*112.21)+((1-fO)*28.05))

[0156] More information can be found in the following references:

[0157] Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.

[0158] Parkinson,M.,Klimke,K.,Spiess,H.W.,Wilhelm,M.,Macromol.Chem.Phys.2007;208:2128.

[0159] NMR Spectroscopy of Polymers:Innovative Strategies for ComplexMacromolecules,Chapter24,401(2011)

[0160] Pollard,M.,Klimke,K.,Graf,R.,Spiess,H.W.,Wilhelm,M.,Sperber,O.,Piel,C.,Kaminsky,W.,Macromolecules 2004;37:813.

[0161] Filip,X.,Tripon,C.,Filip,C.,J.Mag.Resn.2005,176,239

[0162] Griffin,J.M.,Tripon,C.,Samoson,A.,Filip,C.,and Brown,S.P.,Mag.Res.inChem.2007 45,S1,S198

[0163] Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer50(2009)2373

[0164] Zhou,Z.,Kuemmerle,R.,Qiu,X.,Redwine,D.,Cong,R.,Taha,A.,Baugh,D.Winniford,B.,J.Mag.Reson.187(2007)225

[0165] Busico,V.,Carbonniere,P.,Cipullo,R.,Pellecchia,R.,Severn,J.,Talarico,G.,Macromol.Rapid Commun.2007,28,1128

[0166] J.Randall,Macromol.Sci.,Rev.Macromol.Chem.Phys.1989,C29,201.

[0167] Qiu,X.,Redwine,D.,Gobbi,G.,Nuamthanom,A.,Rinaldi,P.,Macromolecules2007,40,6879

[0168] Liu,W.,Rinaldi,P.,McIntosh,L.,Quirk,P.,Macromolecules 2001,34,4757

[0169] d) Unsaturation

[0170] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the amount of unsaturated groups in the polymer.

[0171] Quantitative measurements were recorded in solution using a Bruker Avance II 400 NMR spectrometer operating at 400.15 MHz. 1 H NMR spectroscopy. All aerosols were performed using nitrogen gas at 125 °C. 13 All spectra were recorded with a C optimized 10 mm selective excitation probe. Approximately 200 mg of material was dissolved in 1,2-tetrachloroethane-d2 (TCE-d2) using approximately 3 mg of Hostanox 03 (CAS 32509-66-3) as a stabilizer. Standard single pulse excitation with a 30 degree pulse, a 10 s relaxation delay and 10 Hz sample rotation was employed. A total of 128 transients were acquired per spectrum using 4 virtual scans. This setup was chosen primarily for the high resolution required for quantitative determination of unsaturation and vinylidene stability. All chemical shifts were indirectly referenced to TMS at 0.00 ppm using the signal formed by the remaining protonated solvent at 5.95 ppm.

[0172] A characteristic signal corresponding to the presence of a terminal aliphatic vinyl group (R-CH=CH2) was observed and the amount was quantified using the integration of the number of two coupled unequal terminal CH2 protons (Va and Vb) occupying each functional group reporter site at 4.95 ppm, 4.98 ppm, 5.00 ppm and 5.05 ppm:

[0173] Nvinyl=IVab / 2

[0174] When a characteristic signal corresponding to the presence of an internal vinylidene group (RR'C=CH2) is observed, the amount is quantified using the integration of the number of two CH2 protons (D) occupying each functional group reporter site at 4.74 ppm:

[0175] N vinylidene = ID / 2

[0176] When a characteristic signal corresponding to the presence of an internal cis-vinylene (E-RCH=CHR') or related structure is observed, the amount is quantified using the integration of the number of two CH protons (C) occupying each functional group reporter site at 5.39 ppm:

[0177] Ncis=IC / 2

[0178] When a characteristic signal corresponding to the presence of an internal trans-vinylene (Z-RCH=CHR') is observed, the amount is quantified using the integration of the number of two CH protons (T) occupying each functional group reporter site at 5.45 ppm:

[0179] Ntrans=IT / 2

[0180] When a characteristic signal corresponding to the presence of an internal trisubstituted vinylene (RCH=CHR'R") or related structures is observed, the amount is quantified using the integration of the number of CH protons (Tris) occupying each functional group reporter site at 5.14 ppm:

[0181] Ntris=ITris

[0182] Hostanox 03 stabilizer was quantified by using multiple integration of the number of reporting sites per molecule occupied by aromatic protons (A) at 6.92 ppm, 6.91 ppm, 6.69 ppm and 6.89 ppm:

[0183] H=IA / 4

[0184] Quantification of unsaturation in polyolefins Typically, the amount of unsaturation is determined based on total carbon atoms, even if 1 H NMR spectroscopy. This can be combined with other 13 C NMR spectra for direct comparison of microstructural quantities.

[0185] The total amount of carbon atoms was calculated from the integration of the bulk aliphatic signal between 2.85 ppm and -1.00 ppm, compensating for the methyl signal from the stabilizer and the carbon atoms associated with unsaturated functionality which were not included in this region:

[0186] NC total = (I host - 42*H) / 2 + 2*N vinyl + 2*N vinylidene + 2*Ncis + 2*Ntrans + 2*Ntris The content of unsaturated groups (U) is calculated as the number of unsaturated groups per thousand total carbons (kCHn) in the polymer:

[0187] U=1000*N / NC total

[0188] The total amount of unsaturated groups was calculated as the sum of each observed unsaturated group and is therefore also reported per thousand total carbons:

[0189] Utotal=Uvinyl+Uvinylidene+Ucis+Utrans+Utris

[0190] The relative content of a specific unsaturated group (U) is reported as the fraction or percentage of a given unsaturated group relative to the total number of unsaturated groups:

[0191] [U] = Ux / Utotal

[0192] More information can be found in the following references:

[0193] He,Y.,Qiu,X,and Zhou,Z.,Mag.Res.Chem.2010,48,537-542.

[0194] Busico,V.et.al.Macromolecules,2005,38(16),6988-6996

[0195] e) Determination of average molecular weight and molecular weight distribution

[0196] The average molecular weight (Mz, Mw and Mn), molecular weight distribution (MWD) and its breadth are determined by gel permeation chromatography (GPC) according to ISO 16014-1:2003, ISO 16014-2:2003, ISO 16014-4:2003 and ASTM D 6474-12 using the following formula, expressed as the polydispersity index, PDI = Mw / Mn (where Mn is the number average molecular weight and Mw is the weight average molecular weight):

[0197]

[0198]

[0199]

[0200] For a constant elution volume interval ΔVi, where A i and M i are respectively related to the elution volume V i The associated chromatographic peak slice area and the polyolefin molecular weight (MW), where N equals the number of data points obtained from the chromatogram between the integration limits.

[0201] A high temperature GPC instrument equipped with an IR5 multi-band infrared detector (PolymerChar, Valencia, Spain) and 3×Agilent-PLgel Olexis and 1×Agilent-PLgel Olexis guard columns was used. 1,2,4-Trichlorobenzene (TCB) stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol was used as solvent and mobile phase. The chromatographic system was operated at 160°C and a constant flow rate of 1 mL / min. 200 μL of sample solution was injected for each analysis. Data acquisition was performed using PolymerChar GPC-one software.

[0202] The column set was calibrated using a universal calibration method (according to ISO 16014-2:2003) of 19 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The PS standards were dissolved at room temperature for several hours. The conversion of polystyrene peak molecular weight to polyolefin molecular weight was accomplished using the Mark Houwink equation and the following Mark Houwink constants:

[0203] K PS =19×10 -3 mL / g,α PS =0.655

[0204] K PE =39×10 -3 mL / g,α PE =0.725

[0205] A third-order polynomial was used to fit the calibration data.

[0206] All samples were prepared in the concentration range of 0.5 mg / mL to 1 mg / mL and dissolved at 160 °C with constant gentle shaking for 3 h.

[0207] f) Melting temperature (T m ) and crystallization temperature (T c )

[0208] The experiments were performed on a TA Instruments Q200 calibrated with Indium, Zinc, and Tin and according to ISO 11357-3. Approximately 5 mg of material was placed in a pan and tested at 10 °C / min throughout the experiment at a nitrogen flow rate of 50 mL / min, a lower temperature of -30 °C and an upper temperature of 180 °C, respectively. Only the second heating run was considered in the analysis. Melting temperature T m is defined as the temperature of the main peak of the thermogram, while the melting enthalpy (ΔHm) ... mThe integral is calculated between +15°C and +25°C. The running integral is also calculated within this range.

[0209] g) Glass transition temperature (T g )

[0210] The glass transition temperature Tg was determined by dynamic mechanical analysis according to ISO 6721-7. Compression molded samples (40×10×1 mm 3 ) is measured in torsion mode.

[0211] h) Vicat temperature (T vicat )

[0212] The Vicat temperature is measured according to method A50 of ISO 306. As described in EN ISO 1873-2, a flat-bottomed needle with a load mass of 10 N and a diameter of 80 × 10 × 4 mm is used. 3 The injection molded specimen is placed in direct contact with the needle. The specimen and the needle are heated at 50°C / h. The temperature at which the needle penetrates to a depth of 1 mm is recorded as the Vicat softening temperature.

[0213] 2. Materials

[0214] a) Comparative Example 1 (CE1)

[0215] CE1 has MFR2 of 1.1g / 10min and density of 902kg / m 3 , melting temperature T m Vinyl octene-1 plastomer (octene content 15.7 wt.%) commercially available from Borealis at 97°C. CE1 was produced in a solution polymerization process using a metallocene catalyst.

[0216] b) Copolymer A has an MFR2 of 1.1 g / 10 min and a density of 910 kg / m 3 and melting temperature T m It is a vinyl octene-1 plastomer at 106°C (octene content 11.9 wt.%).

[0217] c) Copolymer B has an MFR2 of 1.1 g / 10 min and a density of 882.3 kg / m 3 and melting temperature T m It is a vinyl octene-1 plastomer at 73°C (octene content 25.8 wt.%).

[0218] d) Copolymer C has an MFR2 of 1.0 g / 10 min and a density of 862 kg / m 3 and melting temperature T mIt is a vinyl octene-1 plastomer at 35°C (octene content 37.1 wt.%).

[0219] e) Copolymer D has an MFR2 of 1.0 g / 10 min and a density of 870 kg / m 3 and melting temperature T m It is a vinyl octene-1 plastomer at 56°C (octene content 31.5 wt.%).

[0220] In the presence of the metallocene catalyst (phenyl)(cyclohexyl)methylene(cyclopentadienyl)(2,7-di-tert-butylfluorenyl)hafnium dimethyl, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate (AB) (CAS 118612-00-3) commercially available from Boulder was used as a cocatalyst. Copolymers A to D were prepared using Borceed TM Produced by solution polymerization technology.

[0221] The conditions for the polymerization reaction were chosen in such a way that the reaction system was a liquid phase (T between 150° C. and 200° C.; 60 bar to 150 bar).

[0222] 3. Results

[0223] The mixing of the respective materials was performed using a Prism TSE-16, a 16 mm co-rotating twin screw extruder with L / D 25 and a throughput of about 1.4 kg / h. The temperature profile was set to 180°C-200°C and the machine was operated at 250 rpm. The samples were produced by mixing a dry mixture of matrix resin particles and extruding the mixture. A batch of about 2.5 kg of dry mix was fed into the hopper and about 2.0 kg of the final extruded mixture was collected after stabilization.

[0224] Examples IE1-1 to IE1-3 of the present invention are mixtures of two copolymers at a specific mixing ratio. The results are shown in Table 1 below.

[0225] Table 1: Results

[0226]

[0227] The above results show that the existing product (CE1) is used as the target to mix two different copolymers to form copolymers (IE-1 to IE1-3), which have good density, melt flow rate, M w Significantly better melting temperature T m And improved T g 、T c and T vicat .

Claims

1. A copolymer of ethylene and a C3 to C8 alpha-olefin, wherein The density of the copolymer measured according to ISO 1183 is 890 kg / m 3 Up to 915kg / m 3 , and the MFR2 measured according to ISO 1133 is 0.5 g / l0min to 8.0 g / l0min, wherein the amount of the α-olefin present in the copolymer is 10 wt.% to 20 wt.%, wherein the melting temperature T of the copolymer measured according to ISO 11357-3 is m Vicat softening temperature T measured according to ISO 306 between 100°C and 120°C vicat 80℃ to 96℃.

2. The copolymer according to claim 1, wherein The copolymer is a copolymer of ethylene and octene.

3. A copolymer according to any one of the preceding claims, wherein The MFR2 of the copolymer measured according to ISO 1133 is from 0.6 g / 10 min to 4.0 g / 10 min.

4. A copolymer according to any one of the preceding claims, wherein The MFR of the copolymer measured according to ISO 1133 21 30g / 10min to 45g / 10min.

5. A copolymer according to any one of the preceding claims, wherein The MFR of the copolymer measured according to ISO 1133 21 The ratio of MFR / MFR2 is 30 to 45.

6. A copolymer according to any one of the preceding claims, wherein The Mw / Mn of the copolymer determined by gel permeation chromatography is 2.5 to 3.

0.

7. A copolymer according to any one of the preceding claims, wherein The Mw of the copolymer determined by gel permeation chromatography is 75,000 to 90,000 g / mol.

8. A copolymer according to any one of the preceding claims, wherein The crystallization temperature T of the copolymer measured according to ISO 11357-3 c 82℃ to 96℃.

9. A copolymer according to any one of the preceding claims, wherein The glass transition temperature T of the copolymer measured according to ISO 6721-7 is g -35℃ to -45℃.

10. A copolymer according to any one of the preceding claims, wherein use 1 The copolymer has a vinyl content of 4.0 to 8.0 vinyl groups per 100,000 carbon atoms as measured by H NMR.

11. A copolymer according to any one of the preceding claims, wherein use 1 The vinylidene content of the copolymer measured by H NMR is 9.0 to 14 vinylidene groups per 100,000 carbon atoms.

12. A copolymer according to any one of the preceding claims, wherein use 1 The trisubstituted vinylene content of the copolymer measured by H NMR is 15.0 to 24.0 trisubstituted vinylene groups per 100,000 carbon atoms.

13. A copolymer according to any one of the preceding claims, wherein use 1 The copolymer has a vinylene content of 10.0 to 16.0 vinylene groups per 100,000 carbon atoms as measured by H NMR.

14. A copolymer according to any preceding claim, wherein The copolymer is obtained by mixing a first ethylene copolymer and a second ethylene copolymer, wherein the first ethylene copolymer has a higher density than the second ethylene copolymer.

15. The copolymer according to claim 14, wherein The mixing ratio of the first ethylene copolymer to the second ethylene copolymer is 65:35 wt. % to 85:15 wt. %.