Semi-aromatic bio-based polyamide and synthetic method thereof

By adding specific monomers and additives to semi-aromatic biobased polyamides, a crosslinking network structure is formed, which solves the problem of high water absorption rate of the material in humid environments and degraded mechanical properties in extreme environments, and achieves high performance resistance Thermal properties, mechanical properties and low water absorption rate are suitable for high-performance engineering plastics and other fields.

CN118994564AInactive Publication Date: 2024-11-22WEIFANG DONGSHENG PLASTIC TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411497403.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Semi-aromatic bio-based polyamide materials have high water absorption in humid environments and have deteriorated mechanical properties in extreme environments, making it difficult to meet high performance requirements.

Method used

By selecting suitable monomers and additives, the semiaromatic bio-based polyamides prepared include pentyldiamine, terephthalic acid, aliphatic dibasic acid, organic tribasic acid, low bromine epoxy resin modified butyldiamine and Bisphenol A diglycidyl ether modified nonediamine, etc., form a crosslinking network structure, improve the heat resistance, mechanical properties and impact resistance of the material, while reducing water absorption.

Benefits of technology

It achieves mechanical properties and low water absorption at extreme temperatures, improves the dimensional stability and chemical resistance of the material, and is suitable for high-performance engineering plastics and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses semi-aromatic bio-based polyamide and a synthesis method thereof, and belongs to the technical field of polymer organic materials. The semi-aromatic bio-based polyamide comprises the following raw materials in percentage by mass: 30-50% of pentamethylene diamine; 10-40% terephthalic acid and / or terephthalic acid derivatives; 15-30% of a first copolymerization raw material, wherein the first copolymerization raw material is aliphatic dibasic acid; 1-10% of a second copolymerization raw material, wherein the second copolymerization raw material is organic tribasic acid; 1-10% of a third copolymerization raw material, wherein the third copolymerization raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine according to a mass ratio of 1: (3-5); and 5-10% of a fourth copolymerization material, wherein the fourth copolymerization material is aliphatic diamine. The semi-aromatic bio-based polyamide prepared by elaborately selecting monomers and additives not only has excellent heat resistance and mechanical properties, but also has very excellent performance at extreme temperature, and also has lower water absorption and environmental friendliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer organic materials, and specifically relates to a semi-aromatic bio-based polyamide and a synthesis method thereof. Background Art

[0002] Polyamide material is a polymer containing repeated amide groups, which can be obtained by polycondensation of diamine and dibasic acid or ring-opening polymerization of amino acid or lactam. Polyamide material has high strength, stiffness, good heat resistance, wear resistance and chemical resistance. Due to its many advantages, it is used in engineering plastics, fibers, coatings and membrane materials.

[0003] With the improvement of sustainable development and environmental awareness, the use of bio-based raw materials to produce polyamide has become an important development direction. Semi-aromatic polyamides combine the good molding processability of aliphatic polyamides with the excellent properties of aromatic polyamides and have attracted widespread attention. As a high-performance engineering plastic, semi-aromatic bio-based polyamides do have some significant advantages, such as good heat resistance and chemical resistance. However, in actual applications, they may also have some disadvantages or limitations. For example: (1) Although semi-aromatic bio-based polyamides have lower water absorption than traditional aliphatic polyamides, they still have a certain tendency to absorb water, which may affect their dimensional stability and mechanical properties, especially in humid environments.

[0004] (2) Although these materials have good mechanical properties, their performance may deteriorate under extreme conditions (such as very high temperatures or long-term stress).

[0005] Therefore, there is an urgent need for a semi-aromatic bio-based polyamide material with low water absorption and almost no decrease in mechanical properties under extreme environments. Summary of the invention

[0006] The purpose of the present invention is to provide a semi-aromatic bio-based polyamide and a synthesis method thereof to solve the problems of high water absorption and decreased mechanical properties of the above-mentioned semi-aromatic bio-based polyamide under extreme environments. The semi-aromatic bio-based polyamide prepared by the present invention not only has excellent heat resistance and mechanical properties, but also has excellent performance under extreme temperatures, and also has low water absorption and environmental friendliness through carefully selected monomers and additives.

[0007] To achieve the above object, the present invention provides a semi-aromatic bio-based polyamide, which comprises the following raw materials in terms of mass percentage: 30~50% pentamethylenediamine; 10~40% terephthalic acid and / or terephthalic acid derivatives; 15-30% of the first copolymerization raw material, the first copolymerization raw material is an aliphatic dibasic acid; 1-10% of the second copolymerization raw material, the second copolymerization raw material is an organic tribasic acid; 1-10% of a third copolymer raw material, wherein the third copolymer raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:(3-5); 5-10% of the fourth copolymer raw material, the fourth copolymer raw material is an aliphatic diamine.

[0008] At present, the preparation of semi-aromatic bio-based polyamides is mostly formed by polycondensation of dibasic acids, terephthalic acid and diamines. The prepared polyamide materials have certain heat resistance and mechanical strength. However, with the continuous increase in the application fields of polyamide materials, higher requirements are put forward for their heat resistance, mechanical strength and environmental resistance. In the design of raw materials, the present invention not only adds ternary organic acids, but also adds the first copolymerization raw material, the third copolymerization raw material and the fourth copolymerization raw material to increase the types of dibasic acids and diamines. In the present invention, the organic ternary acid can form additional amide bonds with the amino groups in the polyamide chain, promote the formation of a cross-linked network, and contribute to the thermal stability of the material. The cross-linking points of the cross-linked network structure also increase the cohesion of the material, and improve the tensile strength and elastic modulus. In the raw materials of the present invention, a variety of dibasic acids and diamines are designed. The aromatic structure (such as terephthalic acid and its derivatives) itself has good chemical stability, which can improve the resistance of the material to various chemicals. The aliphatic dibasic acid and diamine provide flexible segments, giving the material good toughness. The invention can improve the impact resistance while maintaining a certain toughness by reasonably controlling the proportion of each component, and the prepared polyamide material has excellent mechanical properties.

[0009] Preferably, the terephthalic acid derivative is one or more of benzoyl chloride, dimethyl terephthalate, and diethyl terephthalate.

[0010] Preferably, the aliphatic dibasic acid is one or more of succinic acid, glutaric acid, adipic acid and pimelic acid.

[0011] Preferably, the organic tribasic acid is one or both of citric acid and benzene trimeric acid.

[0012] Preferably, the preparation process of low-bromine epoxy resin modified dibutyleneamine is: Add the composite low-bromine epoxy resin to diaminobutane in a mass ratio of (8-12):1, and mix at room temperature for 12-24 hours to obtain low-bromine epoxy resin modified diaminobutane; The composite low-brominated epoxy resin comprises a first low-brominated epoxy resin and a second low-brominated epoxy resin in a mass ratio of 1:(0.5-0.8); The first low-brominated epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 10-14%; The epoxy equivalent of the second low-brominated epoxy resin is 340-380 g / eq and the bromine content is 19-21%.

[0013] Preferably, the preparation process of bisphenol A diglycidyl ether modified nonanediamine is: Add the composite bisphenol A diglycidyl ether to nonanediamine in a mass ratio of (4-6):1, and mix at room temperature for 24-48 hours to obtain bisphenol A diglycidyl ether modified nonanediamine; The composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of (0.3-0.5): 1; The epoxy equivalent of the first bisphenol A diglycidyl ether is 210-240 g / eq; The epoxy equivalent of the second bisphenol A diglycidyl ether is 176-184 g / eq.

[0014] The present invention continues to develop and find that although the addition of organic tribasic acid and the design of multiple dibasic acids and diamines can further improve the heat resistance and mechanical properties of polyamide materials, the water absorption rate and tolerance of polyamide materials in extreme environments are still poor. Based on this, the present invention specifically modifies diaminobutane and diamine, specifically using epoxy resin to modify both, thereby improving the mechanical strength of polyamide materials in extremely hot and cold environments and reducing the water absorption rate of polyamide materials. Analysis of the reasons: Both the composite low-bromine epoxy resin and the composite bisphenol A diglycidyl ether contain epoxy groups. These groups react with diaminobutane and diamine to form a cross-linked structure during the modification process. The cross-linked network reduces the gaps between molecular chains and reduces the possibility of water penetrating into the material, thereby reducing the water absorption rate. Reducing the water absorption rate helps maintain the dimensional stability and long-term chemical resistance of the material, especially in a humid environment. The cross-linked network also limits the movement of the molecular chain, so that the material can still maintain its shape and performance at higher temperatures. By controlling the cross-linking density, the heat resistance can be improved without sacrificing other properties.

[0015] The present invention continues to develop and find that although the addition of low-bromine epoxy resin modified butylene diamine and bisphenol A diglycidyl ether modified nonane diamine to the reaction can increase the heat resistance of the polyamide material and reduce the water absorption rate, the crosslinking density is too high, which will increase the brittleness of the polyamide material and reduce the mechanical strength at low temperatures. Based on this, the present invention limits the mass ratio of low-bromine epoxy resin modified butylene diamine and bisphenol A diglycidyl ether modified nonane diamine. The modification of low-bromine epoxy resin and bisphenol A diglycidyl ether can improve the toughness of the material at low temperatures, and appropriate crosslinking can reduce the brittleness of the material at low temperatures and improve its impact resistance under low temperature conditions. Therefore, the present invention can balance the hardness and toughness of the material by adjusting the ratio of the modifier to meet the requirements of the low temperature environment.

[0016] Preferably, the aliphatic diamine is one or more of hexamethylenediamine, heptamethylenediamine and octanediamine.

[0017] A second aspect of the present invention provides a method for synthesizing a semi-aromatic bio-based polyamide, comprising the following steps: (1) under a nitrogen atmosphere, pentamethylenediamine and a first copolymerization raw material are dissolved in water, and then terephthalic acid and / or a terephthalic acid derivative and a fourth copolymerization raw material are added, and the mixture is continuously stirred to perform a salt-forming reaction to obtain a polyamide salt solution; (2) adding a second copolymerization raw material to the polyamide salt aqueous solution to carry out a prepolymerization reaction to obtain a prepolymer; (3) Adding a third copolymer raw material to the prepolymer to carry out a solid phase reaction. After the reaction is completed, the prepolymer is allowed to stand at room temperature to fully precipitate the product, which is then filtered, washed, and dried to obtain a semi-aromatic bio-based polyamide.

[0018] Preferably, the amount of water added in step (1) is 100-120% of the mass of pentamethylenediamine.

[0019] Preferably, the temperature of the salt-forming reaction in step (1) is 80-100° C. and the time is 5-10 h; The prepolymerization reaction temperature in step (2) is 220-250°C and the reaction time is 3-6 hours; The temperature of the solid phase reaction in step (3) is 300-320°C and the time is 6-8h.

[0020] Therefore, the present invention adopts the above-mentioned semi-aromatic bio-based polyamide and its synthesis method, which has the following beneficial effects: 1. The presence of terephthalic acid and its derivatives in the present invention increases the rigidity of polyamide, helps to increase the glass transition temperature and melting point of the material, thereby enhancing the heat resistance of the material.

[0021] 2. The present invention optimizes the arrangement of molecular chains and improves the thermal stability of the material by controlling the temperature and time of prepolymerization and solid phase reaction.

[0022] 3. The introduction of aromatic structure in the present invention enhances the material's ability to resist chemical corrosion. At the same time, the modifiers in the third copolymer raw material, such as low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine, help to further improve the material's chemical resistance due to their hydrophobicity.

[0023] 4. The aliphatic dibasic acid and diamine in the present invention provide flexible segments, giving the material good toughness and impact resistance. The addition of organic tribasic acid helps to form a cross-linked network, improve the strength and modulus of the material, and finally, by adjusting the proportion of each component, the hardness and toughness of the material can be balanced to achieve ideal comprehensive mechanical properties.

[0024] 5. The flexible segments in the present invention (such as those from aliphatic dibasic acids and diamines) maintain the toughness of the material at low temperatures and avoid embrittlement at low temperatures; the addition of the third copolymer raw material improves the dimensional stability and impact resistance of the material at different temperatures, making it more suitable for extreme temperature environments.

[0025] 6. The third copolymer raw material in the present invention, such as low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine, has hydrophobic properties and can significantly reduce the water absorption rate of the material. The hydrophobicity of the aromatic structure also helps to reduce water absorption and maintain the dimensional stability and long-term durability of the material.

[0026] 7. The present invention uses bio-based raw materials (such as pentamethylenediamine) to reduce dependence on fossil fuels and reduce carbon footprint. It also reduces the emission of harmful substances by adopting low-bromine epoxy resin modifiers, further improving the overall environmental performance of the material. DETAILED DESCRIPTION

[0027] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.

[0028] Example 1 This embodiment provides a semi-aromatic bio-based polyamide, which includes the following raw materials in terms of mass percentage: 45% pentamethylenediamine; 20% terephthalic acid and dimethyl terephthalate, the mass ratio of terephthalic acid to dimethyl terephthalate is 1:1.

[0029] 15% of the first copolymerization raw material, the first copolymerization raw material is an aliphatic dibasic acid; the aliphatic dibasic acid is succinic acid and glutaric acid, and the mass ratio of succinic acid to glutaric acid is 1:1.

[0030] 5% of the second copolymerization raw material, the second copolymerization raw material is an organic tribasic acid; the organic tribasic acid is citric acid.

[0031] 5% of a third copolymer raw material, wherein the third copolymer raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:4; 10% of the fourth copolymer raw material, the fourth copolymer raw material is an aliphatic diamine, the aliphatic diamine is hexamethylenediamine and heptamethylenediamine, and the mass ratio of hexamethylenediamine to heptamethylenediamine is 1:1.

[0032] The preparation process of low-bromine epoxy resin modified butanediamine is as follows: adding composite low-bromine epoxy resin to butanediamine at a mass ratio of 10:1, mixing at room temperature for 15 hours, and obtaining low-bromine epoxy resin modified butanediamine; The composite low-brominated epoxy resin comprises a first low-brominated epoxy resin and a second low-brominated epoxy resin in a mass ratio of 1:0.6; The first low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 10-14%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., and the model is YNBE3462A80; The second low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 19-21%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YNBE3465A75.

[0033] The preparation process of bisphenol A diglycidyl ether modified nonanediamine is as follows: adding composite bisphenol A diglycidyl ether to nonanediamine at a mass ratio of 5:1, mixing at room temperature for 30 hours, and obtaining bisphenol A diglycidyl ether modified nonanediamine; The composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of 0.4:1; The first bisphenol A diglycidyl ether has an epoxy equivalent of 210-240 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., model number YN1826; The second bisphenol A diglycidyl ether has an epoxy equivalent of 176-184 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YN1827.

[0034] A method for synthesizing a semi-aromatic bio-based polyamide comprises the following steps: (1) Under a nitrogen atmosphere, pentamethylenediamine and a first copolymer raw material are dissolved in water, and then terephthalic acid and / or a terephthalic acid derivative and a fourth copolymer raw material are added, and the mixture is continuously stirred to carry out a salt-forming reaction at a temperature of 90° C. for 6 hours to obtain a polyamide salt solution; the amount of water added is 110% of the mass of pentamethylenediamine.

[0035] (2) adding a second copolymerization raw material to the polyamide salt aqueous solution to carry out a prepolymerization reaction at a temperature of 230° C. for 4 hours to obtain a prepolymer; (3) Adding the third copolymer raw material to the prepolymer to carry out a solid phase reaction at a temperature of 310° C. for 7 hours. After the reaction is completed, the prepolymer is allowed to stand at room temperature to fully precipitate the product, which is then filtered, washed, and dried to obtain a semi-aromatic bio-based polyamide.

[0036] Example 2 This embodiment provides a semi-aromatic bio-based polyamide, which includes the following raw materials in terms of mass percentage: 30% pentamethylenediamine; 20% terephthalic acid and diethyl terephthalate, the mass ratio of terephthalic acid to diethyl terephthalate is 1:1.

[0037] 20% of the first copolymerization raw material, the first copolymerization raw material is an aliphatic dibasic acid; the aliphatic dibasic acid is adipic acid and pimelic acid, and the mass ratio of adipic acid to pimelic acid is 1:1.

[0038] 10% of the second copolymerization raw material, the second copolymerization raw material is an organic tribasic acid; the organic tribasic acid is benzene trimecchymic acid.

[0039] 10% of a third copolymer raw material, wherein the third copolymer raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:3; 10% of the fourth copolymer raw material, the fourth copolymer raw material is an aliphatic diamine, and the aliphatic diamine is octanediamine.

[0040] The preparation process of low-bromine epoxy resin modified butanediamine is as follows: adding composite low-bromine epoxy resin to butanediamine at a mass ratio of 8:1, mixing at room temperature for 12 hours, and obtaining low-bromine epoxy resin modified butanediamine; The composite low-brominated epoxy resin includes a first low-brominated epoxy resin and a second low-brominated epoxy resin in a mass ratio of 1:0.5; The first low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 10-14%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., and the model is YNBE3462A80; The second low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 19-21%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YNBE3465A75.

[0041] The preparation process of bisphenol A diglycidyl ether modified nonanediamine is as follows: adding composite bisphenol A diglycidyl ether to nonanediamine at a mass ratio of 4:1, mixing at room temperature for 24 hours, and obtaining bisphenol A diglycidyl ether modified nonanediamine; The composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of 0.3:1; The first bisphenol A diglycidyl ether has an epoxy equivalent of 210-240 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., model number YN1826; The second bisphenol A diglycidyl ether has an epoxy equivalent of 176-184 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YN1827.

[0042] A method for synthesizing a semi-aromatic bio-based polyamide, characterized in that it comprises the following steps: (1) Under a nitrogen atmosphere, pentamethylenediamine and a first copolymer raw material are dissolved in water, and then terephthalic acid and / or a terephthalic acid derivative and a fourth copolymer raw material are added, and the mixture is continuously stirred to carry out a salt-forming reaction. The temperature of the salt-forming reaction is 80° C. and the time is 10 hours to obtain a polyamide salt solution. The amount of water added is 100% of the mass of pentamethylenediamine.

[0043] (2) adding a second copolymerization raw material to the polyamide salt aqueous solution to carry out a prepolymerization reaction at a temperature of 220° C. for 6 hours to obtain a prepolymer; (3) Adding the third copolymer raw material to the prepolymer to carry out a solid phase reaction at a temperature of 320° C. for 8 hours. After the reaction is completed, the prepolymer is allowed to stand at room temperature to fully precipitate the product, which is then filtered, washed, and dried to obtain a semi-aromatic bio-based polyamide.

[0044] Example 3 This embodiment provides a semi-aromatic bio-based polyamide, which includes the following raw materials in terms of mass percentage: 50% pentamethylenediamine; 10% terephthalic acid and benzoyl chloride, the mass ratio of terephthalic acid to benzoyl chloride is 1:1.

[0045] 25% of the first copolymerization raw material, the first copolymerization raw material is an aliphatic dibasic acid; the aliphatic dibasic acid is succinic acid, glutaric acid and adipic acid, and the mass ratio of succinic acid, glutaric acid and adipic acid is 1:1:1.

[0046] 4% of the second copolymerization raw material, the second copolymerization raw material is an organic tribasic acid; the organic tribasic acid is citric acid and benzene trimecchymic acid, and the mass ratio of citric acid to benzene trimecchymic acid is 1:1.

[0047] 3% of a third copolymer raw material, wherein the third copolymer raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:5; 8% of the fourth copolymer raw material, the fourth copolymer raw material is an aliphatic diamine, and the aliphatic diamine is hexamethylenediamine.

[0048] The preparation process of low-bromine epoxy resin modified butanediamine is as follows: adding composite low-bromine epoxy resin to butanediamine at a mass ratio of 12:1, mixing at room temperature for 12 hours, and obtaining low-bromine epoxy resin modified butanediamine; The composite low-brominated epoxy resin comprises a first low-brominated epoxy resin and a second low-brominated epoxy resin in a mass ratio of 1:0.8; The first low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 10-14%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., and the model is YNBE3462A80; The second low-bromine epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 19-21%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YNBE3465A75.

[0049] The preparation process of bisphenol A diglycidyl ether modified nonanediamine is as follows: adding composite bisphenol A diglycidyl ether to nonanediamine at a mass ratio of 6:1, mixing at room temperature for 24 hours, and obtaining bisphenol A diglycidyl ether modified nonanediamine; The composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of 0.5:1; The first bisphenol A diglycidyl ether has an epoxy equivalent of 210-240 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd., model number YN1826; The second bisphenol A diglycidyl ether has an epoxy equivalent of 176-184 g / eq and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YN1827.

[0050] A method for synthesizing a semi-aromatic bio-based polyamide, characterized in that it comprises the following steps: (1) Under a nitrogen atmosphere, pentamethylenediamine and a first copolymer raw material are dissolved in water, and then terephthalic acid and / or a terephthalic acid derivative and a fourth copolymer raw material are added, and the mixture is continuously stirred to carry out a salt-forming reaction. The temperature of the salt-forming reaction is 100° C. and the time is 5 hours to obtain a polyamide salt solution. The amount of water added is 120% of the mass of pentamethylenediamine.

[0051] (2) adding a second copolymerization raw material to the polyamide salt aqueous solution to carry out a prepolymerization reaction at a temperature of 250° C. for 3 hours to obtain a prepolymer; (3) Adding the third copolymer raw material to the prepolymer to carry out a solid phase reaction at a temperature of 300° C. for 8 hours. After the reaction is completed, the prepolymer is allowed to stand at room temperature to fully precipitate the product, which is then filtered, washed, and dried to obtain a semi-aromatic bio-based polyamide.

[0052] Comparative Example 1 The difference between this comparative example and Example 1 is that no second copolymerization raw material is added in step (2).

[0053] Comparative Example 2 The difference between this comparative example and Example 1 is that the third copolymerization raw material includes low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:1.

[0054] Comparative Example 3 The difference between this comparative example and Example 1 is that the types of low-bromine epoxy resins used in the preparation process of low-bromine epoxy resin-modified butanediamine are different. The first low-bromine epoxy resin has an epoxy equivalent of 420-440 g / eq and a bromine content of 18.5-21.5%, and is purchased from Jiangsu Yangnong Chemical Group Co., Ltd. with a model number of YNBE3351A80.

[0055] Comparative Example 4 The difference between this comparative example and Example 1 is that the types of bisphenol A diglycidyl ether used in the preparation process of bisphenol A diglycidyl ether-modified nonanediamine are different. The epoxy equivalent of the first bisphenol A diglycidyl ether is 450-550 g / eq, purchased from Jiangsu Yangnong Chemical Group Co., Ltd., model number YN2301.

[0056] Comparative Example 5 The difference between this comparative example and Example 1 is that the third copolymerization raw material includes low-bromine epoxy resin modified butanediamine and nonanediamine in a mass ratio of 1:4.

[0057] Comparative Example 6 The difference between this comparative example and Example 1 is that the third copolymerization raw material includes butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:4.

[0058] Comparative Example 7 The difference between this comparative example and Example 1 is that the third copolymerization raw material added in step (3) is butanediamine and nonanediamine.

[0059] Comparative Example 8 The difference between this comparative example and Example 1 is that the polyamide salt solution, the second copolymer raw material and the third copolymer raw material are directly mixed, and solid phase reacted at 310° C. for 7 hours. After the reaction is completed, the mixture is allowed to stand at room temperature to fully precipitate the product, which is filtered, washed and dried to obtain a semi-aromatic bio-based polyamide.

[0060] Comparative Example 9 The difference between this comparative example and Example 1 is that the second copolymerization raw material is added into step (1).

[0061] Comparative Example 10 The difference between this comparative example and Example 1 is that the composite low-bromine epoxy resin includes a first low-bromine epoxy resin and a second low-bromine epoxy resin in a mass ratio of 1:2.

[0062] Comparative Example 11 The difference between this comparative example and Example 1 is that the composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of 1:1.

[0063] Performance Testing Tensile properties: measured according to GB / T 1040.1-2006, tensile rate 5mm / min, test temperature 23℃; Impact performance: measured according to GB / T 1843-2008, the test temperature is 23℃; Water absorption: Determined according to GB / T 1034-2008. Before testing, the sample is placed in air with a relative humidity of 50% and a temperature of 23°C for 24 hours.

[0064] Melting point: Refer to ASTM D3418-2003. The specific test method is to use DSC analyzer to test the melting point of the sample, nitrogen atmosphere, flow rate of 40mL / min, first increase the temperature to 340℃ at 10℃ / min, keep at 340℃ for 2min, then cool to 50℃ at 10℃ / min, and then increase the temperature to 340℃ at 10℃ / min. The endothermic peak temperature at this time is set as the melting point T m .

[0065] The semi-aromatic bio-based polyamide prepared in the example and the comparative example was placed at 250° C. for 7 days and at −60° C. for 30 days, respectively, and then restored to room temperature, and then the tensile property retention rate and impact property retention rate thereof were tested.

[0066] Tensile performance retention rate = (tensile strength after high and low temperature treatment - tensile strength before high and low temperature treatment) / tensile strength before high and low temperature treatment × 100%; Impact performance retention rate = (notched impact strength after high and low temperature treatment - notched impact strength before high and low temperature treatment) / notched impact strength before high and low temperature treatment × 100%.

[0067] Table 1 Mechanical properties and water absorption test results

[0068] Table 2 High and low temperature resistance test results

[0069] It can be seen from the above performance test results that the semi-aromatic bio-based polyamides of Examples 1-3 have excellent high temperature resistance, mechanical strength, high water absorption, and can maintain their mechanical strength basically unchanged at extremely high and extremely low temperatures. In particular, the comprehensive performance of Example 1 is the most outstanding. This is mainly because organic tribasic acids and modified butanediamine and nonanediamine are added during the preparation of the semi-aromatic bio-based polyamide, which increases the degree of cross-linking of the reaction, forms a denser cross-linking structure, and increases the mechanical strength and environmental resistance of the product.

[0070] The comparative example did not adopt the necessary technical solution, resulting in its performance test being significantly worse than that of the embodiment. In comparative example 1, the type of raw materials was changed, and the second copolymer raw material ternary organic acid was not added. From the results, it can be seen that the effects of mechanical properties, water absorption rate and environmental resistance all decreased, proving that the ternary organic acid has an important influence on the improvement of the comprehensive effect. Analysis of the reasons: In step (2), the ternary organic acid is added. The organic ternary acid can form additional amide bonds with the amino groups in the polyamide chain, promote the formation of a cross-linked network, and contribute to the thermal stability of the material. The cross-linking points of the cross-linked network structure also increase the cohesion of the material, and improve the tensile strength and elastic modulus.

[0071] In Comparative Example 2, the mass ratio of modified butanediamine and modified nonanediamine in the third copolymer raw material was changed. From the results, it can be seen that the mechanical properties and environmental resistance of the prepared semi-aromatic bio-based polyamide were significantly reduced, and the water absorption rate was also increased compared with the embodiment, indicating that the ratio of modified butanediamine and modified nonanediamine has a very important influence on the improvement of the comprehensive performance of the product.

[0072] Comparative Examples 3-4 changed the parameters of low-bromine epoxy resin and bisphenol A diglycidyl ether respectively. From the results, it can be seen that the mechanical properties and environmental resistance of the prepared semi-aromatic bio-based polyamide are significantly reduced, and the water absorption rate is also increased compared with the embodiment, indicating that the epoxy equivalent of low-bromine epoxy resin and bisphenol A diglycidyl ether has a very important influence on the improvement of the comprehensive performance of the product.

[0073] In Comparative Examples 5 and 6, one of the diamines is modified respectively. In Comparative Example 5, only butanediamine is modified with epoxy resin, and in Comparative Example 6, only nonanediamine is modified with epoxy resin. From the results, it can be seen that the comprehensive performance of the products prepared in Comparative Examples 5 and 6 is further reduced compared with Comparative Examples 3 to 4, indicating that the modification of butanediamine and nonanediamine at the same time plays an important role in improving the comprehensive performance of the product.

[0074] In Comparative Example 7, neither butanediamine nor nonanediamine was modified. From the results, it can be seen that the mechanical properties and high and low temperature environmental resistance of the semi-aromatic bio-based polyamide prepared therefrom further decreased compared with Comparative Examples 5-6, indicating the necessity of modifying butanediamine and nonanediamine in the present invention. The reasons are analyzed as follows: low-bromine epoxy resin and bisphenol A diglycidyl ether both contain epoxy groups, which react with butanediamine and nonanediamine to form a cross-linked structure during the modification process. The cross-linked network reduces the gaps between molecular chains, improves the mechanical properties and environmental resistance of the semi-aromatic bio-based polyamide, reduces the water absorption rate, and improves its comprehensive performance.

[0075] In Comparative Example 8, the reaction steps were changed, and the salt-forming step and the prepolymerization step were not carried out. All the raw materials were directly mixed, and a semi-aromatic bio-based polyamide product was prepared by solid phase reaction. It can be seen from the results that the comprehensive performance of the prepared product is significantly reduced compared with that of the embodiment, which shows the necessity of setting the reaction steps in the present invention.

[0076] In Comparative Example 9, the step of adding the second copolymer raw material was changed, and it was mixed together with the dibasic acid monomer in the first copolymer raw material. From the results, it can be seen that the comprehensive properties of the semi-aromatic bio-based polyamide prepared therefrom, such as mechanical properties and environmental resistance, decreased, and the water absorption rate also increased. This shows the necessity of limiting the step of adding the second copolymer raw material in the present invention.

[0077] Comparative Examples 10 and 11 respectively changed the ratio of the composite low-bromine epoxy resin and the ratio of the composite bisphenol A diglycidyl ether. From the results, it can be seen that the semi-aromatic bio-based polyamide prepared therefrom has decreased comprehensive properties such as mechanical properties and environmental resistance compared with the examples, and the water absorption rate has also increased, indicating that it is necessary to set the ratio of the modified resin in the present invention. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effect.

[0078] Therefore, the present invention adopts a semi-aromatic bio-based polyamide of the above structure and its synthesis method, and through carefully selected monomers and additives, the prepared semi-aromatic bio-based polyamide not only has excellent heat resistance, chemical resistance and mechanical properties, but also has excellent performance under extreme temperatures, and also has low water absorption and environmental friendliness. These characteristics make the material very suitable for use in fields with high performance requirements, such as high-end engineering plastic products, electronic and electrical components, automotive parts, coatings, etc.

[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A semi-aromatic bio-based polyamide, It is characterized in that The following raw materials are included in terms of mass percentage: 30~50% pentamethylenediamine; 10~40% terephthalic acid and / or terephthalic acid derivatives; 15-30% of the first copolymerization raw material, the first copolymerization raw material is an aliphatic dibasic acid; 1-10% of the second copolymerization raw material, the second copolymerization raw material is an organic tribasic acid; 1-10% of a third copolymer raw material, wherein the third copolymer raw material comprises low-bromine epoxy resin modified butanediamine and bisphenol A diglycidyl ether modified nonanediamine in a mass ratio of 1:(3-5); 5-10% of the fourth copolymer raw material, the fourth copolymer raw material is an aliphatic diamine.

2. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The terephthalic acid derivative is one or more of benzoyl chloride, dimethyl terephthalate and diethyl terephthalate.

3. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The aliphatic dibasic acid is one or more of succinic acid, glutaric acid, adipic acid and pimelic acid.

4. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The organic tribasic acid is one or two of citric acid and benzene trimeric acid.

5. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The preparation process of low-bromine epoxy resin modified diaminobutane is as follows: Add the composite low-bromine epoxy resin to diaminobutane in a mass ratio of (8-12):1, and mix at room temperature for 12-24 hours to obtain low-bromine epoxy resin modified diaminobutane; The composite low-brominated epoxy resin comprises a first low-brominated epoxy resin and a second low-brominated epoxy resin in a mass ratio of 1:(0.5-0.8); The first low-brominated epoxy resin has an epoxy equivalent of 340-380 g / eq and a bromine content of 10-14%; The epoxy equivalent of the second low-brominated epoxy resin is 340-380 g / eq and the bromine content is 19-21%.

6. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The preparation process of bisphenol A diglycidyl ether modified nonanediamine is as follows: Add the composite bisphenol A diglycidyl ether to nonanediamine in a mass ratio of (4-6):1, and mix at room temperature for 24-48 hours to obtain bisphenol A diglycidyl ether modified nonanediamine; The composite bisphenol A diglycidyl ether comprises a first bisphenol A diglycidyl ether and a second bisphenol A diglycidyl ether in a mass ratio of (0.3-0.5): 1; The epoxy equivalent of the first bisphenol A diglycidyl ether is 210-240 g / eq; The epoxy equivalent of the second bisphenol A diglycidyl ether is 176-184 g / eq.

7. A semi-aromatic bio-based polyamide according to claim 1, It is characterized in that The aliphatic diamine is one or more of hexamethylenediamine, heptamethylenediamine and octanediamine.

8. A method for synthesizing a semi-aromatic bio-based polyamide according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) under a nitrogen atmosphere, pentamethylenediamine and a first copolymerization raw material are dissolved in water, and then terephthalic acid and / or a terephthalic acid derivative and a fourth copolymerization raw material are added, and the mixture is continuously stirred to perform a salt-forming reaction to obtain a polyamide salt solution; (2) adding a second copolymerization raw material to the polyamide salt aqueous solution to carry out a prepolymerization reaction to obtain a prepolymer; (3) Adding a third copolymer raw material to the prepolymer to carry out a solid phase reaction. After the reaction is completed, the prepolymer is allowed to stand at room temperature to fully precipitate the product, which is then filtered, washed, and dried to obtain a semi-aromatic bio-based polyamide.

9. A method for synthesizing a semi-aromatic bio-based polyamide according to claim 8, It is characterized in that The amount of water added in step (1) is 100-120% of the mass of pentamethylenediamine.

10. The method for synthesizing a semi-aromatic bio-based polyamide according to claim 8, Features: The temperature of the salt-forming reaction in step (1) is 80-100°C and the time is 5-10h; The prepolymerization reaction temperature in step (2) is 220-250°C and the reaction time is 3-6 hours; The temperature of the solid phase reaction in step (3) is 300-320°C and the time is 6-8h.

Citation Information

Cited By

  • Bio-based polyamide with low water absorption and preparation method thereof

    CN120699248A