Flame-retardant durable 3D printing raw material and preparation method thereof

By adding anti-corrosion aids and flame retardant of mugwort fiber powder to 3D printing raw materials, corrosion-resistant and flame-retardant 3D printing consumables are prepared, which solves the problem of 3D printing products in acidic environments and combustion in high-temperature environments. Improves the durability and safety of the product.

CN118978778AInactive Publication Date: 2024-11-19ANHUI SUNLU IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411268729.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Common 3D printing consumables are susceptible to corrosion in acidic environments, affecting the durability and service life of the product.

Method used

Corrosion-resistant and flame-retardant 3D printing materials containing anti-corrosion additives and flame-retardant agents of mugwort fiber powder are prepared by stirring, mixing, extrusion and cooling.

Benefits of technology

Prevent corrosion in an acidic environment, improve the durability and convenience of the product, and prevent combustion in a high-temperature environment, enhancing flame retardant safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978778A_ABST
    Figure CN118978778A_ABST
Patent Text Reader

Abstract

The invention discloses a flame-retardant and durable 3D printing raw material and a preparation method thereof, and belongs to the technical field of 3D printing consumables, and in the flame-retardant and durable 3D printing raw material, an anti-corrosion auxiliary agent containing folium artemisiae argyi fiber powder is added into the raw material for preparing the 3D printing consumables, so that the prepared 3D printing consumables have good flame retardance in a printed finished product; according to the present invention, the product is not easily corroded even if the product is used in the acid environment, and the added folium artemisiae argyi fiber powder enables the prepared finished product to have a certain aromatic odor so as to improve the convenience and the durability during the use process. In the process of preparing the raw materials of the 3D printing consumable, the flame retardant is added into the preparation raw materials, so that after the prepared consumable is printed into a finished product, even if the consumable is used in a high-temperature environment, the consumable is not prone to combustion, and the flame-retardant safety of the consumable in the using process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of 3D printing consumables, and specifically relates to a flame-retardant and durable 3D printing raw material and a preparation method thereof. Background Art

[0002] The 3D printer is equipped with different "printing materials" such as metal, ceramic, plastic, sand, etc., which are real raw materials. After the printer is connected to the computer, the "printing materials" can be stacked layer by layer through computer control, and finally the blueprint on the computer can be turned into a physical object. In layman's terms, a 3D printer is a device that can "print" real 3D objects, such as printing a robot, printing a toy car, printing various models, and even food. The reason why it is commonly called a "printer" is based on the technical principles of ordinary printers, because the layered processing process is very similar to inkjet printing. This printing technology is called 3D stereoscopic printing technology. 3D printing consumables are needed in the 3D printing process.

[0003] However, when using common 3D printing consumables, when the printed products are used in a highly acidic environment, the corrosion rate of the finished products will be accelerated, thus affecting the durability and service life of the 3D printed products. Summary of the invention

[0004] The purpose of the present invention is to provide a flame retardant and durable 3D printing raw material and a preparation method thereof in order to solve the above-mentioned problems.

[0005] The technical solution adopted by the present invention is as follows: a flame retardant and durable 3D printing raw material and a preparation method thereof, which comprises the following steps:

[0006] S1: First, weigh the raw materials for preparing corrosion-resistant 3D printing consumables, and weigh: 600-800 parts by weight of carboxyl acrylic resin, 200-400 parts by weight of SAN resin, 25-35 parts by weight of anti-corrosion additive, 2-5 parts by weight of lubricant, 10-20 parts by weight of foaming agent, 10-18 parts by weight of organic antimony stabilizer, 20-30 parts by weight of flame retardant, 10-20 parts by weight of reinforcing modifier, 20-25 parts by weight of anti-aging agent and 100-300 parts by weight of color pigment;

[0007] S2: the carboxyl acrylic resin, SAN resin, anticorrosive agent, lubricant, foaming agent, organic antimony stabilizer, flame retardant, reinforcing modifier and color pigment weighed in step S1 are stirred and mixed uniformly to obtain a mixture at a stirring speed of 2800 rpm for 10 min;

[0008] S3: fully mixing the mixture obtained in step S2 in a high-speed mixer to obtain a dry mixture, wherein: the stirring speed is 2400 rpm, the stirring time is 5 min, and a mixed consumable raw material is obtained;

[0009] S4: The fully mixed raw materials obtained in step S3 are put into a twin-screw extruder, and the raw materials are pulled by a tractor and pelletized by a granulator to obtain wire masterbatch.

[0010] S5: putting the wire masterbatch obtained in step S4 into a single screw extruder, cooling the extruded filaments with water, and pulling them with a traction machine to make 3D printing consumables with a certain wire diameter, and rolling them into bundles;

[0011] S6: The 3D printing consumables obtained in step S5 are packaged, collected and stored, thereby completing the entire preparation process of the corrosion-resistant 3D printing consumables.

[0012] In a preferred embodiment, in step S1, the preparation method of the anti-corrosion additive is: mix the carboxyl acrylic resin and the nano-tin dioxide powder evenly, then add the silane coupling agent KH-570, stir at 38-46°C for 20-28h, cool to room temperature, then place in an ice water bath for crushing, and ultrasonically treat for 10-14min to obtain material a; disperse concentrated sulfuric acid in distilled water, stir evenly to obtain an acidic composite intercalation aqueous solution; place montmorillonite in a calcining furnace and calcine at 750-850°C for 1-5h, cool, soak in a hydrochloric acid solution for 2-4h, filter out, wash with clean water, and dry Dry, crush into 150-350 mesh powder, then add acidic composite intercalation aqueous solution and mix evenly, then heat to 85-95℃, keep warm for 1-3h, then add material a, calcium sulfate, silicon nitride, montmorillonite powder, barium sulfate, antimony trioxide, weathered coal, seaweed powder, zinc phosphate, bentonite, zeolite powder and zirconium oxide and mix evenly, disperse in 45-55℃ water bath with ultrasonic-mechanical stirring for 2-4h, stand for stratification, remove the upper clear liquid, filter the lower reaction product, wash, vacuum dry at 750-850℃ to constant weight, grind, pass through 150-250 mesh sieve, and obtain anticorrosive additive raw material A;

[0013] Add 10% by weight of nano mugwort fiber powder into the anti-corrosion agent raw material A, and mix thoroughly to obtain the anti-corrosion agent.

[0014] In a preferred embodiment, in step S1, the lubricant is one of calcium stearate, barium stearate, magnesium stearate and polyethylene glycol.

[0015] In a preferred embodiment, in step S1, the foaming agent is azodicarbonamide.

[0016] In a preferred embodiment, in step S1, the flame retardant is a mixture of resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), tributyl tin oxide, glass fiber powder, activated clay, and aluminum hydroxide, and the mixing ratio is: resorcinol bis(diphenyl phosphate): bisphenol A bis(diphenyl phosphate): tributyl tin oxide: molybdenum hydroxide: activated clay: aluminum hydroxide = 1:2:1:1:1:3.

[0017] In a preferred embodiment, in step S1, the reinforcing modifier is a mixture of ethylene-butyl acrylate-glycidyl methacrylate terpolymer and ethylene-vinyl acetate copolymer in a weight ratio of 1-5:1-5.

[0018] In a preferred embodiment, in step S1, the color pigment is at least one of mercuric oxide, basic lead carbonate, acid lead arsenate, acid lead phosphate and bismuth hydroxide.

[0019] In a preferred embodiment, in step S4, the parameters of the twin-screw extruder during the extrusion process are: zone one temperature 108-128°C, zone two temperature 118-138°C, zone three temperature 138-180°C, zone four temperature 150-170°C, zone five temperature 160-180°C, zone six temperature 168-188°C, zone seven temperature 170-190°C, zone eight temperature 168-188°C, zone nine temperature 170-180°C, die head temperature 180-190°C, and rotation speed 80-380rpm.

[0020] In a preferred embodiment, in step S1, the antioxidant is one or more of tea polyphenols, phytic acid, phenolic antioxidant 1076, antioxidant 1010 or phosphite antioxidant 168.

[0021] In a preferred embodiment, in step S5, the parameters of the single screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 168-178°C, zone 3 temperature 170-180°C, die head temperature 150-170°C, and rotation speed 200-230rpm.

[0022] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0023] 1. In the present invention, an anti-corrosion additive containing wormwood fiber powder is added to the raw materials for preparing 3D printing consumables, so that the 3D printing consumables will not be easily corroded in the printed finished products even when used in an acidic environment. At the same time, due to the addition of wormwood fiber powder, the finished products have a certain aromatic smell, thereby improving the convenience and durability during use.

[0024] 2. In the present invention, during the process of preparing the raw materials for 3D printing consumables, a flame retardant is added to the inside of the raw materials, so that after the consumables are printed into finished products, they will not easily burn even if used in a high temperature environment, thereby increasing the flame retardant safety of the consumables during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the process principle of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] Reference Figure 1 ,

[0028] Embodiment 1:

[0029] A flame retardant and durable 3D printing material and a preparation method thereof, comprising the following steps:

[0030] S1: First, weigh the raw materials for preparing corrosion-resistant 3D printing consumables, and weigh: 600 parts by weight of carboxyl acrylic resin, 200 parts by weight of SAN resin, 25 parts by weight of anti-corrosion additive, 2 parts by weight of lubricant, 10 parts by weight of foaming agent, 10 parts by weight of organic antimony stabilizer, 20 parts by weight of flame retardant, 10 parts by weight of reinforcing modifier, 20 parts by weight of anti-aging agent and 100 parts by weight of color pigment;

[0031] S2: the carboxyl acrylic resin, SAN resin, anticorrosive agent, lubricant, foaming agent, organic antimony stabilizer, flame retardant, reinforcing modifier and color pigment weighed in step S1 are stirred and mixed uniformly to obtain a mixture at a stirring speed of 2800 rpm for 10 min;

[0032] S3: fully mixing the mixture obtained in step S2 in a high-speed mixer to obtain a dry mixture, wherein: the stirring speed is 2400 rpm, the stirring time is 5 min, and a mixed consumable raw material is obtained;

[0033] S4: The fully mixed raw materials obtained in step S3 are put into a twin-screw extruder, and the raw materials are pulled by a tractor and pelletized by a granulator to obtain wire masterbatch.

[0034] S5: putting the wire masterbatch obtained in step S4 into a single screw extruder, cooling the extruded filaments with water, and pulling them with a traction machine to make 3D printing consumables with a certain wire diameter, and rolling them into bundles;

[0035] S6: The 3D printing consumables obtained in step S5 are packaged, collected and stored, thereby completing the entire preparation process of the corrosion-resistant 3D printing consumables.

[0036] In step S1, the preparation method of the anti-corrosion additive is as follows: carboxyl acrylic resin and nano-tin dioxide powder are mixed evenly, then silane coupling agent KH-570 is added, stirred at 38-46°C for 20-28h, cooled to room temperature, then placed in an ice water bath for crushing, and ultrasonically treated for 10-14min to obtain material a; concentrated sulfuric acid is dispersed in distilled water, and the acidic composite intercalation aqueous solution is stirred evenly; montmorillonite is placed in a calcining furnace and calcined at 750-850°C for 1-5h, cooled, placed in a hydrochloric acid solution for immersion for 2-4h, filtered out, washed with clean water, dried, and crushed into 1 50-350 mesh powder is then added to the acidic composite intercalation aqueous solution and mixed evenly, then heated to 85-95°C and kept warm for 1-3 hours, followed by adding material a, calcium sulfate, silicon nitride, montmorillonite powder, barium sulfate, antimony trioxide, weathered coal, seaweed powder, zinc phosphate, bentonite, zeolite powder and zirconium oxide and mixing evenly, and dispersed in a 45-55°C water bath by ultrasonic-mechanical stirring for 2-4 hours, allowed to stand for stratification, the upper clear liquid is removed, the lower reaction product is filtered, washed, vacuum dried at 750-850°C to constant weight, ground, and sieved through a 150-250 mesh sieve to obtain the preservative additive raw material A;

[0037] Add 10% by weight of nano mugwort fiber powder into the anti-corrosion agent raw material A, and mix thoroughly to obtain the anti-corrosion agent.

[0038] In step S1, the lubricant is one of calcium stearate, barium stearate, magnesium stearate and polyethylene glycol.

[0039] In step S1, the foaming agent is azodicarbonamide.

[0040] In step S1, the flame retardant is a mixture of resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), tributyl tin oxide, glass fiber powder, activated clay, and aluminum hydroxide, and the mixing ratio is: resorcinol bis(diphenyl phosphate): bisphenol A bis(diphenyl phosphate): tributyl tin oxide: molybdenum hydroxide: activated clay: aluminum hydroxide = 1:2:1:1:1:3.

[0041] In step S1, the reinforcing modifier is a mixture of ethylene-butyl acrylate-glycidyl methacrylate terpolymer and ethylene-vinyl acetate copolymer in a weight ratio of 1-5:1-5.

[0042] In step S1, the color pigment is at least one of mercuric oxide, basic lead carbonate, acid lead arsenate, acid lead phosphate and bismuth hydroxide.

[0043] In step S4, the parameters of the twin-screw extruder during the extrusion process are: zone one temperature 108-128°C, zone two temperature 118-138°C, zone three temperature 138-180°C, zone four temperature 150-170°C, zone five temperature 160-180°C, zone six temperature 168-188°C, zone seven temperature 170-190°C, zone eight temperature 168-188°C, zone nine temperature 170-180°C, die head temperature 180-190°C, and rotation speed 80-380rpm.

[0044] In step S1 , the anti-aging agent is one or more of tea polyphenols, phytic acid, phenolic antioxidant 1076 , antioxidant 1010 or phosphite antioxidant 168 .

[0045] In step S5, the parameters of the single screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 168-178°C, zone 3 temperature 170-180°C, die head temperature 150-170°C, and rotation speed 200-230rpm.

[0046] In the present invention, an anti-corrosion additive containing wormwood fiber powder is added to the raw materials for preparing 3D printing consumables, so that the 3D printing consumables will not be easily corroded in the printed finished products even when used in an acidic environment. At the same time, due to the addition of wormwood fiber powder, the finished products have a certain aromatic smell, thereby improving the convenience and durability during use.

[0047] In the present invention, during the process of preparing the raw materials for 3D printing consumables, a flame retardant is added to the inside of the raw materials, so that after the consumables are printed into finished products, they will not easily burn even if used in a high temperature environment, thereby increasing the flame retardant safety of the consumables during use.

[0048] Embodiment 2:

[0049] A flame retardant and durable 3D printing material and a preparation method thereof, comprising the following steps:

[0050] S1: First, weigh the raw materials for preparing corrosion-resistant 3D printing consumables, and weigh: 800 parts by weight of carboxyl acrylic resin, 400 parts by weight of SAN resin, 35 parts by weight of anti-corrosion additive, 5 parts by weight of lubricant, 20 parts by weight of foaming agent, 18 parts by weight of organic antimony stabilizer, 30 parts by weight of flame retardant, 20 parts by weight of reinforcing modifier, 25 parts by weight of anti-aging agent and 300 parts by weight of color pigment;

[0051] S2: the carboxyl acrylic resin, SAN resin, anticorrosive agent, lubricant, foaming agent, organic antimony stabilizer, flame retardant, reinforcing modifier and color pigment weighed in step S1 are stirred and mixed uniformly to obtain a mixture at a stirring speed of 2800 rpm for 10 min;

[0052] S3: fully mixing the mixture obtained in step S2 in a high-speed mixer to obtain a dry mixture, wherein: the stirring speed is 2400 rpm, the stirring time is 5 min, and a mixed consumable raw material is obtained;

[0053] S4: The fully mixed raw materials obtained in step S3 are put into a twin-screw extruder, and the raw materials are pulled by a tractor and pelletized by a granulator to obtain wire masterbatch.

[0054] S5: putting the wire masterbatch obtained in step S4 into a single screw extruder, cooling the extruded filaments with water, and pulling them with a traction machine to make 3D printing consumables with a certain wire diameter, and rolling them into bundles;

[0055] S6: The 3D printing consumables obtained in step S5 are packaged, collected and stored, thereby completing the entire preparation process of the corrosion-resistant 3D printing consumables.

[0056] In step S1, the preparation method of the anti-corrosion additive is as follows: carboxyl acrylic resin and nano-tin dioxide powder are mixed evenly, then silane coupling agent KH-570 is added, stirred at 38-46°C for 20-28h, cooled to room temperature, then placed in an ice water bath for crushing, and ultrasonically treated for 10-14min to obtain material a; concentrated sulfuric acid is dispersed in distilled water, and the acidic composite intercalation aqueous solution is stirred evenly; montmorillonite is placed in a calcining furnace and calcined at 750-850°C for 1-5h, cooled, placed in a hydrochloric acid solution for immersion for 2-4h, filtered out, washed with clean water, dried, and crushed into 1 50-350 mesh powder is then added to the acidic composite intercalation aqueous solution and mixed evenly, then heated to 85-95°C and kept warm for 1-3 hours, followed by adding material a, calcium sulfate, silicon nitride, montmorillonite powder, barium sulfate, antimony trioxide, weathered coal, seaweed powder, zinc phosphate, bentonite, zeolite powder and zirconium oxide and mixing evenly, and dispersed in a 45-55°C water bath by ultrasonic-mechanical stirring for 2-4 hours, allowed to stand for stratification, the upper clear liquid is removed, the lower reaction product is filtered, washed, vacuum dried at 750-850°C to constant weight, ground, and sieved through a 150-250 mesh sieve to obtain the preservative additive raw material A;

[0057] Add 10% by weight of nano mugwort fiber powder into the anti-corrosion agent raw material A, and mix thoroughly to obtain the anti-corrosion agent.

[0058] In step S1, the lubricant is one of calcium stearate, barium stearate, magnesium stearate and polyethylene glycol.

[0059] In step S1, the foaming agent is azodicarbonamide.

[0060] In step S1, the flame retardant is a mixture of resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), tributyl tin oxide, glass fiber powder, activated clay, and aluminum hydroxide, and the mixing ratio is: resorcinol bis(diphenyl phosphate): bisphenol A bis(diphenyl phosphate): tributyl tin oxide: molybdenum hydroxide: activated clay: aluminum hydroxide = 1:2:1:1:1:3.

[0061] In step S1, the reinforcing modifier is a mixture of ethylene-butyl acrylate-glycidyl methacrylate terpolymer and ethylene-vinyl acetate copolymer in a weight ratio of 1-5:1-5.

[0062] In step S1, the color pigment is at least one of mercuric oxide, basic lead carbonate, acid lead arsenate, acid lead phosphate and bismuth hydroxide.

[0063] In step S4, the parameters of the twin-screw extruder during the extrusion process are: zone one temperature 108-128°C, zone two temperature 118-138°C, zone three temperature 138-180°C, zone four temperature 150-170°C, zone five temperature 160-180°C, zone six temperature 168-188°C, zone seven temperature 170-190°C, zone eight temperature 168-188°C, zone nine temperature 170-180°C, die head temperature 180-190°C, and rotation speed 80-380rpm.

[0064] In step S1 , the anti-aging agent is one or more of tea polyphenols, phytic acid, phenolic antioxidant 1076 , antioxidant 1010 or phosphite antioxidant 168 .

[0065] In step S5, the parameters of the single screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 168-178°C, zone 3 temperature 170-180°C, die head temperature 150-170°C, and rotation speed 200-230rpm.

[0066] In the present invention, an anti-corrosion additive containing wormwood fiber powder is added to the raw materials for preparing 3D printing consumables, so that the 3D printing consumables will not be easily corroded in the printed finished products even when used in an acidic environment. At the same time, due to the addition of wormwood fiber powder, the finished products have a certain aromatic smell, thereby improving the convenience and durability during use.

[0067] In the present invention, during the process of preparing the raw materials for 3D printing consumables, a flame retardant is added to the inside of the raw materials, so that after the consumables are printed into finished products, they will not easily burn even if used in a high temperature environment, thereby increasing the flame retardant safety of the consumables during use.

[0068] Embodiment three:

[0069] A flame retardant and durable 3D printing material and a preparation method thereof, comprising the following steps:

[0070] S1: First, weigh the raw materials for preparing corrosion-resistant 3D printing consumables, and weigh: 700 parts by weight of carboxyl acrylic resin, 300 parts by weight of SAN resin, 28 parts by weight of anti-corrosion additive, 4 parts by weight of lubricant, 15 parts by weight of foaming agent, 15 parts by weight of organic antimony stabilizer, 25 parts by weight of flame retardant, 15 parts by weight of reinforcing modifier, 23 parts by weight of anti-aging agent and 200 parts by weight of color pigment;

[0071] S2: the carboxyl acrylic resin, SAN resin, anticorrosive agent, lubricant, foaming agent, organic antimony stabilizer, flame retardant, reinforcing modifier and color pigment weighed in step S1 are stirred and mixed uniformly to obtain a mixture at a stirring speed of 2800 rpm for 10 min;

[0072] S3: fully mixing the mixture obtained in step S2 in a high-speed mixer to obtain a dry mixture, wherein: the stirring speed is 2400 rpm, the stirring time is 5 min, and a mixed consumable raw material is obtained;

[0073] S4: The fully mixed raw materials obtained in step S3 are put into a twin-screw extruder, and the raw materials are pulled by a tractor and pelletized by a granulator to obtain wire masterbatch.

[0074] S5: putting the wire masterbatch obtained in step S4 into a single screw extruder, cooling the extruded filaments with water, and pulling them with a traction machine to make 3D printing consumables with a certain wire diameter, and rolling them into bundles;

[0075] S6: The 3D printing consumables obtained in step S5 are packaged, collected and stored, thereby completing the entire preparation process of the corrosion-resistant 3D printing consumables.

[0076] In step S1, the preparation method of the anti-corrosion additive is as follows: carboxyl acrylic resin and nano-tin dioxide powder are mixed evenly, then silane coupling agent KH-570 is added, stirred at 38-46°C for 20-28h, cooled to room temperature, then placed in an ice water bath for crushing, and ultrasonically treated for 10-14min to obtain material a; concentrated sulfuric acid is dispersed in distilled water, and the acidic composite intercalation aqueous solution is stirred evenly; montmorillonite is placed in a calcining furnace and calcined at 750-850°C for 1-5h, cooled, placed in a hydrochloric acid solution for immersion for 2-4h, filtered out, washed with clean water, dried, and crushed into 1 50-350 mesh powder is then added to the acidic composite intercalation aqueous solution and mixed evenly, then heated to 85-95°C and kept warm for 1-3 hours, followed by adding material a, calcium sulfate, silicon nitride, montmorillonite powder, barium sulfate, antimony trioxide, weathered coal, seaweed powder, zinc phosphate, bentonite, zeolite powder and zirconium oxide and mixing evenly, and dispersed in a 45-55°C water bath by ultrasonic-mechanical stirring for 2-4 hours, allowed to stand for stratification, the upper clear liquid is removed, the lower reaction product is filtered, washed, vacuum dried at 750-850°C to constant weight, ground, and sieved through a 150-250 mesh sieve to obtain the preservative additive raw material A;

[0077] Add 10% by weight of nano mugwort fiber powder into the anti-corrosion agent raw material A, and mix thoroughly to obtain the anti-corrosion agent.

[0078] In step S1, the lubricant is one of calcium stearate, barium stearate, magnesium stearate and polyethylene glycol.

[0079] In step S1, the foaming agent is azodicarbonamide.

[0080] In step S1, the flame retardant is a mixture of resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), tributyl tin oxide, glass fiber powder, activated clay, and aluminum hydroxide, and the mixing ratio is: resorcinol bis(diphenyl phosphate): bisphenol A bis(diphenyl phosphate): tributyl tin oxide: molybdenum hydroxide: activated clay: aluminum hydroxide = 1:2:1:1:1:3.

[0081] In step S1, the reinforcing modifier is a mixture of ethylene-butyl acrylate-glycidyl methacrylate terpolymer and ethylene-vinyl acetate copolymer in a weight ratio of 1-5:1-5.

[0082] In step S1, the color pigment is at least one of mercuric oxide, basic lead carbonate, acid lead arsenate, acid lead phosphate and bismuth hydroxide.

[0083] In step S4, the parameters of the twin-screw extruder during the extrusion process are: zone one temperature 108-128°C, zone two temperature 118-138°C, zone three temperature 138-180°C, zone four temperature 150-170°C, zone five temperature 160-180°C, zone six temperature 168-188°C, zone seven temperature 170-190°C, zone eight temperature 168-188°C, zone nine temperature 170-180°C, die head temperature 180-190°C, and rotation speed 80-380rpm.

[0084] In step S1 , the anti-aging agent is one or more of tea polyphenols, phytic acid, phenolic antioxidant 1076 , antioxidant 1010 or phosphite antioxidant 168 .

[0085] In step S5, the parameters of the single screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 168-178°C, zone 3 temperature 170-180°C, die head temperature 150-170°C, and rotation speed 200-230rpm.

[0086] In the present invention, an anti-corrosion additive containing wormwood fiber powder is added to the raw materials for preparing 3D printing consumables, so that the 3D printing consumables will not be easily corroded in the printed finished products even when used in an acidic environment. At the same time, due to the addition of wormwood fiber powder, the finished products have a certain aromatic smell, thereby improving the convenience and durability during use.

[0087] In the present invention, during the process of preparing the raw materials for 3D printing consumables, a flame retardant is added to the inside of the raw materials, so that after the consumables are printed into finished products, they will not easily burn even if used in a high temperature environment, thereby increasing the flame retardant safety of the consumables during use.

[0088] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0089] The above description enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A flame-retardant and durable 3D printing raw material and a preparation method thereof, characterized in that: The steps include: S1: First, weigh the raw materials for preparing corrosion-resistant 3D printing consumables, and weigh: 600-800 parts by weight of carboxyl acrylic resin, 200-400 parts by weight of SAN resin, 25-35 parts by weight of anti-corrosion additive, 2-5 parts by weight of lubricant, 10-20 parts by weight of foaming agent, 10-18 parts by weight of organic antimony stabilizer, 20-30 parts by weight of flame retardant, 10-20 parts by weight of reinforcing modifier, 20-25 parts by weight of anti-aging agent and 100-300 parts by weight of color pigment; S2: the carboxyl acrylic resin, SAN resin, anticorrosive agent, lubricant, foaming agent, organic antimony stabilizer, flame retardant, reinforcing modifier and color pigment weighed in step S1 are stirred and mixed uniformly to obtain a mixture at a stirring speed of 2800 rpm for 10 min; S3: fully mixing the mixture obtained in step S2 in a high-speed mixer to obtain a dry mixture, wherein: the stirring speed is 2400 rpm, the stirring time is 5 min, and a mixed consumable raw material is obtained; S4: The fully mixed raw materials obtained in step S3 are put into a twin-screw extruder, and the raw materials are pulled by a tractor and pelletized by a granulator to obtain wire masterbatch. S5: putting the wire masterbatch obtained in step S4 into a single screw extruder, cooling the extruded filaments with water, and pulling them with a traction machine to make 3D printing consumables with a certain wire diameter, and rolling them into bundles; S6: The 3D printing consumables obtained in step S5 are packaged, collected and stored, thereby completing the entire preparation process of the corrosion-resistant 3D printing consumables.

2. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In the step S1, the preparation method of the anti-corrosion additive is as follows: carboxyl acrylic resin and nano tin dioxide powder are mixed evenly, then silane coupling agent KH-570 is added, stirred at 38-46°C for 20-28h, cooled to room temperature, then placed in an ice water bath for crushing, and ultrasonically treated for 10-14min to obtain material a; concentrated sulfuric acid is dispersed in distilled water, and the acidic composite intercalation aqueous solution is stirred evenly; montmorillonite is placed in a calcining furnace and calcined at 750-850°C for 1-5h, cooled, placed in a hydrochloric acid solution for immersion for 2-4h, filtered out, washed with clean water, dried, and crushed into The 150-350 mesh powder is then added to the acidic composite intercalation aqueous solution and mixed evenly, then the temperature is raised to 85-95°C and kept warm for 1-3 hours, followed by adding material a, calcium sulfate, silicon nitride, montmorillonite powder, barium sulfate, antimony trioxide, weathered coal, seaweed powder, zinc phosphate, bentonite, zeolite powder and zirconium oxide and mixing evenly, and dispersed in a 45-55°C water bath by ultrasonic-mechanical stirring for 2-4 hours, and allowed to stand for stratification, the upper clear liquid is removed, the lower reaction product is filtered, washed, vacuum dried at 750-850°C to constant weight, ground, and sieved through a 150-250 mesh sieve to obtain the preservative additive raw material A; Add 10% by weight of nano mugwort fiber powder into the anti-corrosion agent raw material A, and mix thoroughly to obtain the anti-corrosion agent.

3. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In the step S1, the lubricant is one of calcium stearate, barium stearate, magnesium stearate and polyethylene glycol.

4. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In the step S1, the foaming agent is azodicarbonamide.

5. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In step S1, the flame retardant is a mixture of resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), tributyl tin oxide, glass fiber powder, activated clay, and aluminum hydroxide, and the mixing ratio is: resorcinol bis(diphenyl phosphate): bisphenol A bis(diphenyl phosphate): tributyl tin oxide: molybdenum hydroxide: activated clay: aluminum hydroxide = 1:2:1:1:1:

3.

6. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In the step S1, the reinforcing modifier is a mixture of ethylene-butyl acrylate-glycidyl methacrylate terpolymer and ethylene-vinyl acetate copolymer in a weight ratio of 1-5:1-5.

7. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In the step S1, the color pigment is at least one of mercuric oxide, basic lead carbonate, acid lead arsenate, acid lead phosphate and bismuth hydroxide.

8. The flame-retardant and durable 3D printing material and the preparation method thereof according to claim 1, characterized in that: In the step S4, the parameters of the twin-screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 118-138°C, zone 3 temperature 138-180°C, zone 4 temperature 150-170°C, zone 5 temperature 160-180°C, zone 6 temperature 168-188°C, zone 7 temperature 170-190°C, zone 8 temperature 168-188°C, zone 9 temperature 170-180°C, die head temperature 180-190°C, and rotation speed 80-380rpm.

9. A flame-retardant and durable 3D printing material and a preparation method thereof as claimed in claim 1, characterized in that: In step S1 , the anti-aging agent is one or more of tea polyphenols, phytic acid, phenolic antioxidant 1076 , antioxidant 1010 or phosphite antioxidant 168 .

10. The flame-retardant and durable 3D printing material and the preparation method thereof according to claim 1, characterized in that: In step S5, the parameters of the single screw extruder during the extrusion process are: zone 1 temperature 108-128°C, zone 2 temperature 168-178°C, zone 3 temperature 170-180°C, die head temperature 150-170°C, and rotation speed 200-230rpm.