Quantum dot-containing curable composition, quantum dot-containing cured product, method for producing optical member, and method for producing display device
By using a specific combination of solvents and curable binders in a quantum dot curing composition, the problems of quantum dot aggregation and unevenness in inkjet printing were solved, resulting in improved stability and uniformity.
Patent Information
- Application Number
- CN202411063255.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-06-08
- Filing Date
- 2018-06-06
- Publication Date
- 2024-11-19
AI Technical Summary
When forming a quantum dot layer using inkjet printing, quantum dots tend to agglomerate, leading to changes in luminescent color, inkjet head clogging, and surface unevenness, thus affecting luminescent characteristics and stability.
A quantum dot curable composition containing a solvent combination with a specific boiling point range is used to form a quantum dot layer on a substrate by inkjet printing. A curable adhesive component is used to fix the quantum dots, inhibiting agglomeration and improving dispersibility and discharge stability.
Excellent ejection stability was achieved in inkjet printing, quantum dot aggregation was suppressed, and a less unevenly formed quantum dot solidification layer was formed, improving the uniformity and stability of the light-emitting layer.
Smart Images

Figure CN118978832A_ABST
Abstract
Description
[0001] The present application is a divisional application of an application filed on June 6, 2018, with application number 201880037151.0, and invention name “Quantum dot-containing curable composition, quantum dot-containing cured product, method for manufacturing optical component, and method for manufacturing display device”. Technical Field
[0002] The present invention relates to a quantum dot-containing curable composition, a quantum dot-containing cured product, a method for producing an optical member, and a method for producing a display device. Background Art
[0003] In recent years, quantum dots (QDs), which have attracted attention as luminescent materials, are nanometer-sized particles of semiconductors (semiconductor nanocrystals). They exhibit unique optical and electrical properties through the quantum confinement effect (quantum size effect) of electrons and excitons confined in small nanometer-sized crystals. People expect their application in a wide range of fields, and their application as displays has also been proposed. The wavelength of light emitted from quantum dots depends on the particle size of the quantum dots, and light of various wavelengths can be obtained by controlling the particle size. In addition, the spectral width of the light emitted by quantum dots is narrow, so the color purity is excellent.
[0004] The quantum dot-containing layer can be formed by a wet method of applying a dispersion liquid in which the quantum dots are dispersed, or by a dry method of filmizing the quantum dot raw material by evaporation, sputtering, etc. From the perspective of simplicity of the device or process, smoothness of the obtained layer, etc., there is a tendency to adopt the wet method. For example, Patent Document 1 records that a layer containing quantum dots is formed on the surface of a substrate by screen printing, contact printing, or inkjet printing.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2010-533976 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, when the quantum dot layer is formed by a wet method, there is a problem that the quantum dots are easily condensed in the dispersion. Since the luminous color of quantum dots depends on their size, if the quantum dots condense and their crystal structure changes, there is a possibility that the luminous color changes and then causes extinction, which becomes one of the major reasons for reducing the luminous properties.
[0010] In addition, in order to match the ink to the correct pattern and blow it by inkjet method, straightness and stability are required when it is discharged from the discharge head. However, when forming a quantum dot layer by inkjet method, there is a problem that the inkjet head is easily clogged due to the aggregation of quantum dots. In addition, if the evaporation rate of the ink is too fast, the viscosity of the ink increases sharply at the front end of the nozzle of the discharge head, causing the flight of the ink drop to bend, or intermittent discharge at intervals will cause clogging and no longer be able to be discharged.
[0011] In addition, the ink layer formed by the inkjet method may have radial unevenness on the surface. If unevenness occurs on the surface of the quantum dot content layer, unevenness may occur in the luminescent color.
[0012] The present invention is made in view of the above-mentioned actual situation, and its purpose is to provide a quantum dot curable composition having excellent discharge stability in an inkjet method, suppressing the aggregation of quantum dots, and capable of forming a quantum dot-containing cured layer with reduced unevenness. In addition, the present invention aims to provide a quantum dot-containing cured product with reduced unevenness formed by using the above-mentioned quantum dot-containing curable composition. In addition, the present invention aims to provide a method for manufacturing an optical component having a quantum dot-containing cured layer with reduced unevenness formed by using the above-mentioned quantum dot-containing curable composition. In addition, the present invention aims to provide a method for manufacturing a display device using the above-mentioned method for manufacturing an optical component.
[0013] Technical means of solving problems
[0014] The quantum dot-containing curable composition of the present invention contains a curable binder component, quantum dots, and a solvent.
[0015] The solvent contains a solvent component having a boiling point of 165° C. or higher and 260° C. or lower as a first solvent, and further contains a solvent component having a boiling point of 100° C. or higher and lower than 165° C. as a second solvent.
[0016] The quantum dot-containing cured product of the present invention is a cured product of the quantum dot-containing curable composition of the present invention.
[0017] The method for manufacturing an optical component of the present invention comprises the following steps: a step of selectively attaching the above-mentioned quantum dot-containing curable composition of the present invention to a predetermined area on a substrate by inkjet method to form a quantum dot-containing layer; and a step of curing the above-mentioned quantum dot-containing layer to form a quantum dot-containing cured layer.
[0018] The method for manufacturing a display device of the present invention comprises the steps of: manufacturing an optical member by the method for manufacturing an optical member of the present invention; and mounting the manufactured optical member.
[0019] Effects of the Invention
[0020] According to the present invention, a quantum dot curable composition having excellent discharge stability in an inkjet method, in which quantum dot aggregation is suppressed and a quantum dot-containing cured layer with reduced unevenness can be formed can be provided. In addition, according to the present invention, a quantum dot-containing cured product with reduced unevenness formed using the above-mentioned quantum dot-containing curable composition can be provided. In addition, according to the present invention, a method for manufacturing an optical component having a quantum dot-containing cured layer with reduced unevenness formed using the above-mentioned quantum dot-containing curable composition can be provided. In addition, according to the present invention, a method for manufacturing a display device using the above-mentioned method for manufacturing an optical component can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram for explaining an example of the method for producing the optical member of the present invention.
[0022] Figure 2 This is a schematic diagram showing an example of a display device obtained by the manufacturing method of the present invention.
[0023] Figure 3 This is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention.
[0024] Figure 4 This is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention.
[0025] Figure 5 This is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention.
[0026] Figure 6 This is a diagram for explaining a method for evaluating the unevenness of a quantum dot-containing solidified layer. DETAILED DESCRIPTION
[0027] Hereinafter, the quantum dot-containing curable composition, the quantum dot-containing cured product, the method for producing an optical member, and the method for producing a display device of the present invention will be described in detail in this order.
[0028] It should be noted that the light in the present invention includes electromagnetic waves with wavelengths in the visible and non-visible regions, and also includes radiation, such as microwaves and electron beams. Specifically, it refers to electromagnetic waves with a wavelength of 5 μm or less, and electron beams.
[0029] In the present invention, (meth)acryloyl represents each of acryloyl and methacryloyl, (meth)acrylic acid represents each of acrylic acid and methacrylic acid, and (meth)acrylate represents each of acrylate and methacrylate.
[0030] I. Quantum-dot-containing curable composition
[0031] The quantum dot-containing curable composition of the present invention contains a curable binder component, quantum dots, and a solvent.
[0032] The solvent contains a solvent component having a boiling point of 165° C. or higher and 260° C. or lower as a first solvent, and further contains a solvent component having a boiling point of 100° C. or higher and lower than 165° C. as a second solvent.
[0033] The quantum dot-containing curable composition of the present invention is a composition suitable for forming a quantum dot-containing layer such as a light-emitting layer or a light conversion layer of an optical member by an inkjet method, and can be preferably used for inkjet.
[0034] The quantum dot-containing curable composition of the present invention can suppress the aggregation of quantum dots in the quantum dot-containing curable composition and improve dispersibility by using a solvent that combines a first solvent having a boiling point of 165°C or more and 260°C or less and a second solvent having a boiling point of 100°C or more and less than 165°C. It is speculated that this is because: the stability of the solvent composition in the ink, especially the ink in the inkjet device, is relatively high, which can suppress the aggregation of quantum dots and maintain dispersibility. In addition, by using the quantum dot-containing curable composition of the present invention, a quantum dot-containing cured layer in which the aggregation of quantum dots is suppressed can be formed. It is believed that this is because: the quantum dot-containing curable composition of the present invention has excellent dispersibility of quantum dots as described above, so the quantum dots can be uniformly dispersed, and since a curable adhesive component is used as an adhesive component, if the quantum dot-containing curable composition of the present invention is cured, while maintaining the state in which the quantum dots are uniformly dispersed, the curable adhesive component forms a cross-linked structure to fix the quantum dots.
[0035] In addition, the quantum dot curable composition of the present invention can form a quantum dot curable layer with reduced unevenness while having excellent discharge stability in the inkjet method by using a solvent containing the above-mentioned specific first solvent and the above-mentioned specific second solvent in combination. It is believed that the quantum dot curable composition of the present invention suppresses the rapid drying of the quantum dot curable composition due to the above-mentioned specific first solvent with a moderately slow drying speed, thereby improving the straightness and stability when the quantum dot curable composition is discharged from the discharge head, and also suppresses the clogging of the discharge head, thereby having excellent discharge stability. In addition, it is speculated that the use of the quantum dot curable composition of the present invention can form a quantum dot curable layer with reduced unevenness because: by combining the above-mentioned specific first solvent and the above-mentioned specific second solvent, it has a moderate drying speed, so that during the drying process when forming the quantum dot layer, the flow of the solute is suppressed, the generation of radial unevenness on the coating surface is suppressed, and the generation of unevenness caused by the aggregation of quantum dots is suppressed.
[0036] Hereinafter, each component used in the quantum dot-containing curable composition of the present invention will be described in order from the solvent. It should be noted that, hereinafter, the quantum dot-containing curable composition of the present invention may be referred to as ink.
[0037] <Solvent>
[0038] The solvent used in the quantum dot-containing curable composition of the present invention is characterized by containing a solvent component having a boiling point of 165°C to 260°C as a first solvent and a solvent component having a boiling point of 100°C to less than 165°C as a second solvent.
[0039] The solvent component having a boiling point of 165°C or more and 260°C or less has moderate drying properties, so the quantum dot curable composition of the present invention containing such a solvent component as the first solvent does not dry quickly in either the case of intermittent discharge or continuous discharge, and is therefore not prone to causing a sharp increase in viscosity and clogging at the nozzle tip of the inkjet head, and has excellent stability in the discharge direction and discharge amount. Therefore, the quantum dot curable composition of the present invention is discharged onto the substrate surface in a predetermined pattern by inkjet method, thereby accurately and uniformly forming a patterned quantum dot curable layer.
[0040] Furthermore, the quantum dot curable composition of the present invention, in addition to the above-mentioned specific first solvent, also appropriately combines a solvent component having a boiling point of 100°C or more and less than 165°C as a second solvent, thereby optimizing the drying speed and suppressing the aggregation of quantum dots. Since the front end of the nozzle of the inkjet head does not dry quickly, and the drying speed is moderate when the coating of the quantum dot curable composition is dried, the flow of solute can be suppressed. Therefore, after being discharged onto the substrate, it is fused with the surface of the substrate and fully leveled, and then it can be completely dried in a relatively short time by appropriate drying means. Therefore, if the quantum dot curable composition of the present invention is used, a pattern with a higher uniformity of film thickness with reduced unevenness can be obtained, and it can be dried efficiently.
[0041] The solvent component used as the first solvent may be one or a mixed solvent of two or more as long as it is a solvent having the above-mentioned boiling point. The proportion of the first solvent in the total amount of solvent in the quantum dot curable composition of the present invention is not particularly limited. From the perspective of easily obtaining drying properties suitable for inkjet, improving the initial discharge properties of inkjet and intermittent discharge stability, it is preferably 30% by mass or more, from the perspective of further improving the initial discharge properties, it is more preferably 40% by mass or more, and from the perspective of further improving the intermittent discharge stability, it is more preferably 50% by mass or more. On the other hand, from the perspective of being able to fully contain the second solvent and optimizing the drying speed of the composition, the proportion of the first solvent in the total amount of solvent in the quantum dot curable composition of the present invention is preferably 90% by mass or less, more preferably 80% by mass or less, more preferably 70% by mass or less, and particularly preferably 65% by mass or less.
[0042] The surface tension of the first solvent at 23° C. is preferably 24 mN / m or more from the viewpoint of suppressing outflow of the quantum dot-containing curable composition during patterning. When the first solvent is a mixed solvent of two or more, the mixed solvent as a whole preferably has the above surface tension.
[0043] In addition, when the following variable wettability layer is formed on the surface of the substrate and exposed, and an ink-affinity region is formed on the portion of the substrate where the quantum dot layer is to be formed, and the quantum dot curable composition of the present invention is selectively attached to the ink-affinity region by inkjet, the following solvent may be selected as the first solvent: the standard liquid shown in the wettability test specified in JIS K6768 is used to make the droplet contact and measure the contact angle (θ) after 30 seconds, and the contact angle relative to the surface of the test piece with a critical surface tension of 30mM / m obtained by the curve graph of Zisman Plot is 25° or more, preferably 30° or more, and the contact angle relative to the surface of the test piece with a critical surface tension of 70mN / m obtained by the same measurement method is 10° or less. When the first solvent is a mixed solvent of two or more, it is preferred that the mixed solvent as a whole has the above contact angle.
[0044] If a quantum dot-containing curable composition is prepared using a solvent that exhibits the above-mentioned behavior with respect to wettability, the composition exhibits a large repellency to the surface of the variable wettability layer described below before the wettability of the variable wettability layer is changed, and exhibits a large affinity to the surface of the variable wettability layer after the wettability of the variable wettability layer is changed and changed in a direction of increasing hydrophilicity. Therefore, the difference in wettability of the quantum dot-containing curable composition with respect to the ink-philic region formed by selectively exposing a portion of the surface of the variable wettability layer and the difference in wettability of the ink-repellent region with respect to the surrounding region can be increased, and the ink blown to the ink-philic region by the inkjet method can be uniformly wetted and diffused to every corner of the ink-philic region.
[0045] Here, the test piece having the above-mentioned characteristics regarding the critical surface tension may be formed of any material. As a test piece showing a critical surface tension of 30 mN / m, for example, a test piece obtained by actually performing the above test and meeting the requirements can be selected from polymethyl methacrylate, polyvinyl chloride, polyvinylidene chloride, polyethylene terephthalate, and a test piece obtained by coating a smooth glass surface with the above polymer or surface modifier, etc. In addition, as a test piece showing a critical surface tension of 70 mN / m, for example, a test piece obtained by actually performing the above test and meeting the requirements can be selected from nylon, a test piece obtained by coating a hydrophilized glass surface, etc.
[0046] As the above-mentioned first solvent, from the perspective of suppressing the aggregation of quantum dots and the discharge stability in the inkjet method, it is preferably selected from one or more of glycol ethers, glycol ether esters, aliphatic carboxylic acids, aliphatic esters, aromatic esters, dicarboxylic acid diesters, alkoxy carboxylic acid esters, keto carboxylic acid esters, halogenated carboxylic acids, alcohols, phenols, aliphatic ethers, alkoxy alcohols, glycol oligomers, amino alcohols, alkoxy alcohol esters, ketones, morpholines, aliphatic amines, aromatic amines, halogenated aromatic hydrocarbons and alkanes.
[0047] More specifically, as the first solvent, for example, the following solvents can be selected and used: glycol ethers such as ethylene glycol monohexyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, diethylene glycol methyl ethyl ether, and dipropylene glycol dimethyl ether; glycol ether esters such as ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate; aliphatic carboxylic acids such as 2-ethylhexanoic acid; aliphatic esters such as cyclohexyl acetate; aromatic esters such as propyl benzoate; dicarboxylic acid diesters such as diethyl carbonate; alkoxycarboxylic acid esters such as methyl 3-methoxypropionate and ethyl 3-ethoxypropionate; ketocarboxylic acid esters such as methyl acetoacetate and ethyl acetoacetate; chloroacetic acid, dichloroacetic acid, etc. halogenated carboxylic acids of the type; alcohols or phenols such as ethanol, isopropanol, phenol, 2-methylcyclohexanol, 2-octanol, n-heptanol, and diacetone alcohol; aliphatic ethers such as diethyl ether, diisoamyl ether, and 1,8-cineole; alkoxy alcohols such as 3-methoxy-3-methyl-1-butanol; glycol oligomers such as diethylene glycol and tripropylene glycol; amino alcohols such as 2-diethylaminoethanol; alkoxy alcohol esters such as 3-methoxy-3-methylbutyl acetate and 3-methoxybutyl acetate; ketones such as diisobutyl ketone, methylcyclohexanone, and methyl-n-hexanone; morpholines such as phenylmorpholine; aliphatic or aromatic amines such as aniline; halogenated aromatic hydrocarbons such as dichlorobenzene; alkanes such as decane, undecane, dodecane, tridecane, and tetradecane.
[0048] As the first solvent, from the perspective of the dispersibility of quantum dots and the discharge stability in the inkjet method, it is preferably selected from 3-methoxy-3-methyl-1-butanol, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, diethylene glycol dibutyl ether, ethylene glycol monobutyl ether, propylene glycol monobutyl ether, diethylene glycol methyl ethyl ether, dipropylene glycol dimethyl ether, diisoamyl ether, 1,8-cineole, diethyl adipate, dibutyl oxalate, malonic acid The invention relates to an aqueous solution of at least one of dimethyl ester, diethyl malonate, dimethyl succinate, diethyl succinate, 3-methoxybutyl acetate, methyl acetoacetate, cyclohexyl acetate, ethyl 3-ethoxypropionate, decane, undecane, dodecane, tridecane and tetradecane. From the perspective of improving the dispersibility of quantum dots, it is more preferably selected from ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, ethyl 3-ethoxypropionate and 3-methoxybutyl acetate.
[0049] Furthermore, from the viewpoint of improving the storage stability of the quantum dot-containing curable composition, the first solvent preferably does not have a hydroxyl group, and is particularly preferred from the viewpoint of improving the storage stability when used in combination with the blocked carboxylic acid curing agent described below.
[0050] The second solvent is a solvent component having a boiling point of 100°C or more and less than 165°C, and has a boiling point appropriately lower than that of the first solvent. Therefore, by combining the second solvent with the first solvent, the inkjet head nozzle tip does not dry quickly, and the solute flow can be suppressed when the quantum dot layer is dried, and the drying speed can be appropriately adjusted. The solvent component used as the second solvent can be used alone or in combination of two or more solvents as long as it has the above-mentioned boiling point.
[0051] The boiling point of each solvent component used as the second solvent is more preferably 105° C. to 160° C., particularly preferably 110° C. to 150° C., from the viewpoint of improving the dispersibility of quantum dots and easily obtaining a good coating film with reduced unevenness.
[0052] The proportion of the second solvent in the total amount of solvent in the quantum dot curable composition of the present invention is not particularly limited. From the perspective of improving the dispersibility of the quantum dots and suppressing the unevenness of the quantum dot cured layer, it is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 30% by mass or more, and particularly preferably 35% by mass or more. On the other hand, from the perspective of being able to fully contain the first solvent and improving the inkjet discharge properties, it is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less.
[0053] In addition, the viscosity of the second solvent at 23°C is preferably 0.5 to 6 mPa·s. In this case, by including the second solvent, the viscosity of the quantum dot curable composition can be appropriately reduced without hindering the effect of the first solvent, and the wettability and diffusion of the ink itself are improved. As a result, the sprayed ink droplets are easily wetted and diffused to the corners of the entire region where the quantum dot layer is formed. As a result, even for a variety of substrates, the sprayed ink can wet and diffuse to the edge of the partition wall, which can prevent the fading or brightness reduction of the pixel. In order to make the ink adhere to the corner of the region, there is also a method of spraying the ink to the end of the region, but if this method is used, there is a risk of the ink flowing out from the gap of the partition wall. In contrast, the situation where the ink itself wets and diffuses to the edge of the partition wall as in the present invention does not have the risk of ink flowing out, which is a more ideal method. The viscosity of the second solvent at 23°C is further preferably 0.5 to 3 mPa·s. In the case of using two or more second solvents in a mixed manner, even if the viscosity is outside the above range in the case of a single solvent, as long as the viscosity of the mixed solvent is in the above range, it can be preferably used. Here, the viscosity at 23° C. in the present invention can be measured by a rotational vibration type viscometer (for example, rotational vibration type viscometer VISCOMATE VM-1G manufactured by Yamaichi Electric Co., Ltd., etc.).
[0054] As long as the surface tension of the second solvent at 23°C is 35mN / m or less, it can be preferably used. Among them, when the surface tension of the second solvent at 23°C is 30mN / m or less, the surface tension can be appropriately reduced without hindering the effect of the first solvent, and the wettability and diffusivity of the ink itself are improved, so the sprayed ink droplets are easy to wet and diffuse to every corner of the entire quantum dot layer formation area. Here, the surface tension at 23°C in the present invention can be measured by a surface tensiometer (Wilhelmy method) (for example, manufactured by Kyowa Interface Science Co., Ltd., automatic surface tensiometer CBVP-Z, etc.).
[0055] The second solvent may be any solvent having the above-mentioned boiling point, and it is preferred to appropriately select and use a solvent having excellent compatibility with the first solvent.
[0056] Specific examples of the second solvent include glycol ethers such as ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, propylene glycol monopropyl ether, and diethylene glycol dimethyl ether; glycol esters including glycol ether esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; carboxylic acids such as isobutyric acid, propionic acid, and butyric acid; ethyl isovalerate, hexyl formate, amyl acetate, isopentyl acetate, ethyl lactate, methyl lactate, isopentyl propionate, Aliphatic esters such as butyl propionate, butyl butyrate, and dimethyl oxalate; aliphatic carboxylic acids and their anhydrides such as acetic acid and acetic anhydride; alcohols such as n-pentanol, isopentanol, 2-ethylbutanol, 1-butanol, n-hexanol, 4-methyl-2-pentanol, cyclohexanol, 2-heptanol, and 3-heptanol; ketones such as ethyl-n-butyl ketone, di-n-propyl ketone, and acetylacetone; alkanes such as octane and nonane; aromatic hydrocarbons such as toluene, xylene, and ethylbenzene; aromatic ethers such as anisole; aliphatic ethers such as 1,4-dioxane, etc.
[0057] As the second solvent, from the perspective of the dispersibility of quantum dots, it is preferred to use one or more selected from ethers including polyol ethers such as glycol ethers and glycerol ethers, and esters including polyol esters such as glycol esters and glycerol esters, aliphatic esters, alkoxycarboxylates, and ketocarboxylates. When using esters and ethers as described above, there is an advantage that it is easy to maintain the stability of the ink even when a highly reactive resin is used in the adhesive component, etc. In addition, when glycol ethers and glycol esters are used, the wettability of the second solvent to the glass substrate is improved, and it is easy to wet and diffuse to every corner of the entire region where the quantum dot layer is formed, which is effective in preventing the fading of pixels.
[0058] As the second solvent, in particular, from the perspective of the dispersibility of the quantum dots and the discharge stability in the inkjet method, preferably used is a solvent selected from ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, diethylene glycol dimethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, hexyl formate, ethyl lactate, isopentyl propionate, butyl propionate, butyl butyrate, dimethyl oxalate, 1-butanol, 1-butyl alcohol, , one or more solvents selected from 4-dioxane, octane, nonane, toluene, xylene, ethylbenzene and anisole, and from the aspect of improving the dispersibility of quantum dots, more preferably one or more selected from ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, toluene, and propylene glycol monomethyl ether acetate, and further preferably one or more selected from ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, and propylene glycol monomethyl ether acetate.
[0059] In addition, as the solvent used in the quantum dot-containing curable composition of the present invention, from the perspective of improving the dispersibility of the quantum dots, it is preferably a combination of one or more of the above-mentioned first solvent selected from ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, ethyl 3-ethoxypropionate, and 3-methoxybutyl acetate and one or more of the above-mentioned second solvent selected from ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, toluene, and propylene glycol monomethyl ether acetate.
[0060] The solvent used in the quantum dot curable composition of the present invention may further contain other solvents having a boiling point lower than 100° C., which are different from the first solvent and the second solvent, within the range that does not impair the effect of the present invention. The proportion of the other solvents in the total amount of the solvent used in the quantum dot curable composition of the present invention is preferably 30% by mass or less, more preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 2% by mass or less, and particularly preferably 0.5% by mass or less.
[0061] The total content of the above-mentioned solvents including the above-mentioned first solvent and the above-mentioned second solvent in the quantum dot-containing curable composition of the present invention is not particularly limited. From the perspective of the dispersibility of the quantum dots, the initial discharge property and intermittent discharge stability of the inkjet head, and the aspect of suppressing the unevenness generated on the surface of the cured film, it is preferably 50% by mass or more, more preferably 60% by mass or more, and further preferably 70% by mass or more. On the other hand, if the content ratio of the solvent is too much, it is difficult to make the quantum dot-containing cured layer contain a sufficient amount of quantum dots and binder components, etc., so it is preferably 98% by mass or less, more preferably 90% by mass or less, and further preferably 80% by mass or less.
[0062] <Curing Binder Component>
[0063] In order to impart film-forming properties, adhesion to the coated surface, and maintain the dispersibility of quantum dots in the film in a good state, the quantum dot-containing curable composition of the present invention contains a curable adhesive component. In the present invention, the curable adhesive component is a component contained in order to attach and fix the quantum dots to a predetermined position, and is usually a mixture.
[0064] The quantum dot-containing curable composition of the present invention contains a curable binder component, and in the quantum dot-containing cured product obtained by curing the quantum dot-containing curable composition, the aggregation of quantum dots can be suppressed during the production and the aggregation of quantum dots can be suppressed over time. In addition, the quantum dot-containing curable composition of the present invention contains a curable binder component, and can give the quantum dot-containing cured product sufficient strength, durability, and adhesion.
[0065] As the above-mentioned curable adhesive component, for example, a polymerizable adhesive component such as a photocurable adhesive component that can be polymerized and cured by light such as visible light, ultraviolet light, and electron beam, and a thermosetting adhesive component that can be polymerized and cured by heating can be used. As the curable adhesive component used in the quantum dot-containing curable composition of the present invention, it is preferred to contain at least one of a thermosetting adhesive component and a photocurable adhesive component from the aspects of easily suppressing the aggregation of quantum dots and the aspects of strength and durability. The curable adhesive component used in the quantum dot-containing curable composition of the present invention can be appropriately selected from the solvent solubility of the above-mentioned solvent and the component with high compatibility with quantum dots.
[0066] (1) Thermosetting adhesive component
[0067] As the thermosetting adhesive component, a combination of a compound having two or more thermosetting functional groups in one molecule and a curing agent is generally used, and a catalyst that can promote the thermosetting reaction may be further added. In addition, a polymer that itself has no polymerization reactivity may also be used.
[0068] As a compound having two or more thermosetting functional groups in one molecule, an epoxy compound can be preferably used. In addition, as a thermosetting functional group, in addition to an epoxy group, an oxetane group, an isocyanate group, a hydroxyl group, etc. can also be listed. From the aspect that the solvent solubility of the above-mentioned specific solvent and the compatibility with quantum dots are easily improved, a compound having two or more thermosetting functional groups selected from one or more of an epoxy group, an oxetane group, an isocyanate group and a hydroxyl group in one molecule can be preferably used.
[0069] The oxetane compound replaced with the oxetane group in the following epoxy compound can be used in the same manner as the epoxy compound. In addition, the combination of a compound having two or more isocyanate groups in one molecule (polyisocyanate compound) and a compound having two or more hydroxyl groups in one molecule (polyol compound) can form a polymer by forming a carbamate bond between molecules through the reaction of the isocyanate group and the hydroxyl group. At least one of the compound having two or more isocyanate groups in one molecule and the compound having two or more hydroxyl groups in one molecule can be a polymer compound, and at least one of them can be a carbamate prepolymer.
[0070] (Epoxides)
[0071] As the above-mentioned epoxy compound, an epoxy compound having two or more epoxy groups in one molecule can be preferably used. An epoxy compound having two or more epoxy groups in one molecule is an epoxy compound (including compounds called epoxy resins) having two or more, preferably 2 to 50, and more preferably 2 to 20 epoxy groups in one molecule. The epoxy group can be any structure having an oxirane ring structure, and examples thereof include glycidyl, ethylene oxide, and cyclohexyl oxide. As the epoxy compound, known polycyclic epoxy compounds that can be cured by carboxylic acids can be cited, and such epoxy compounds are widely disclosed in, for example, "Epoxy Resin Handbook" edited by Masaki Shinbo and published by Nikkan Kogyo Shimbun (1937), and these can be used.
[0072] Examples of the epoxy compound include epoxy group-containing (co)polymers and epoxy group-containing monomers, and commercially available epoxy resins may also be used.
[0073] The (co)polymer containing epoxy groups is a homopolymer of a monomer containing a carbon-carbon unsaturated bond and an epoxy group (hereinafter, sometimes referred to as a monomer containing epoxy groups), and a copolymer of the monomer and a monomer copolymerizable with the monomer containing epoxy groups. The molecular form of the copolymer may be linear, branched, or any form such as a random copolymer, a block copolymer, or a graft copolymer. The polymer containing epoxy groups may be obtained by a polymerization method selected from radical polymerization, ionic polymerization, and the like.
[0074] Examples of the epoxy group-containing monomer include glycidyl methacrylate (hereinafter referred to as GMA), 3,4-epoxycyclohexylmethyl methacrylate, neopentyl glycol glycidyl ether, etc. Examples of the monomer copolymerizable with the epoxy group-containing monomer include alkyl (meth)acrylates, styrene, N-alkylmaleimide, etc.
[0075] Examples of the epoxy resin include bisphenol A novolac epoxy resin, cresol novolac epoxy resin, bisphenol A epoxy resin, bisphenol F epoxy resin, brominated bisphenol A epoxy resin, bisphenol S epoxy resin, diphenyl ether epoxy resin, hydroquinone epoxy resin, naphthalene epoxy resin, biphenyl epoxy resin, fluorene epoxy resin, phenol novolac epoxy resin, o-cresol novolac epoxy resin, trihydroxyphenylmethane epoxy resin, trifunctional epoxy resin, tetrahydroxyphenylethane epoxy resin, dicyclopentadienol epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol A core-containing polyol epoxy resin, polypropylene glycol epoxy resin, glycidyl ester epoxy resin, glycidylamine epoxy resin, glyoxal epoxy resin, alicyclic epoxy resin, heterocyclic epoxy resin, and the like.
[0076] Commercial products of bisphenol A type epoxy resins include, for example, trade names jER828, jER157S70, and jER1001 [all manufactured by Mitsubishi Chemical Corporation]. Cresol novolac type epoxy resins include, for example, trade name YDCN-701 [manufactured by Tohto Kasei Corporation]. In addition, as a 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, trade name EHPE3150 [manufactured by Daicel Corporation] can also be used.
[0077] These epoxy compounds can be used alone or in combination of two or more.
[0078] (Curing agent)
[0079] The curing agent used for the thermosetting adhesive component is appropriately selected according to the type of the thermosetting functional group contained in the thermosetting adhesive component, and is not particularly limited.
[0080] For example, when the thermosetting adhesive component contains the epoxy compound, a conventionally known carboxylic acid compound can be used as a curing agent.
[0081] Specifically, examples include: acid anhydrides such as succinic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, trimellitic anhydride, 1,2,4-cyclohexanetricarboxylic anhydride, and methylhexahydrophthalic anhydride; aliphatic polycarboxylic acids such as succinic acid, adipic acid, 1,2,3,4-butanetetracarboxylic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid; aromatic polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, and pyromellitic acid; alicyclic polycarboxylic acids such as tetrahydrophthalic acid, hexahydrophthalic acid, and 1,2,4-cyclohexanetricarboxylic acid; polymer carboxylic acids such as polyester resins, acrylic resins, and maleated polybutadiene resins having two or more carboxyl groups in one molecule; and the following blocked carboxylic acid curing agents, etc.
[0082] Commercially available products may also be used, and examples thereof include RIKACID MH700, HNA-100, and MTA-15 [all manufactured by Shin Nippon Rika Co., Ltd.].
[0083] Among these, from the aspects of dischargeability, dispersibility of quantum dots, and storage stability of the quantum dot-containing curable composition, a blocked carboxylic acid curing agent in which the carboxyl group is blocked (latentized) is preferred. That is, as the above-mentioned curable adhesive component, a thermosetting adhesive component containing the above-mentioned epoxy compound and the above-mentioned blocked carboxylic acid curing agent can be preferably used.
[0084] The blocked carboxylic acid curing agent is heated to dissociate the vinyl ether compound and generate a carboxylic acid compound. The generated carboxylic acid compound reacts with the epoxy compound. Since the temperature of the blocked carboxylic acid curing agent is high, the storage stability of the composition can be improved, and the blocked carboxylic acid curing agent is a component that can coexist with epoxy groups at high concentrations and thus improve heat resistance and solvent resistance. In addition, when the blocked carboxylic acid curing agent is used in combination with quantum dots, it is not easily affected by the heat and light received during the manufacturing process or display, and the distance between the quantum dots can be kept fixed, and excitation suppression can be prevented, so it is preferred.
[0085] Examples of the blocked carboxylic acid curing agent include compounds obtained by blocking the carboxyl groups of polycarboxylic acid compounds with vinyl ether compounds. Examples of preferred polycarboxylic acid compounds include compounds represented by the following general formula (1).
[0086] [Chemical formula 1]
[0087] General formula (1)
[0088]
[0089] (In the general formula (1), m is an integer of 0 to 4, a is 0 or 1, and n is an integer of 1 to 4. When n is 1, R 1 is a hydrogen atom or a hydrocarbon group having 2 to 8 carbon atoms, and when n is 2 to 4, R 1 is a hydrocarbon group having 2 to 8 carbon atoms. 2 is an alkyl group having 1 or more and 5 or less carbon atoms. )
[0090] As the vinyl ether compound, for example, a compound represented by the following general formula (2) can be mentioned as a preferred compound.
[0091] [Chemical formula 2]
[0092] General formula (2)
[0093]
[0094] (In general formula (2), R 3 A hydrocarbon group having 1 to 10 carbon atoms.
[0095] Preferred examples of the blocked carboxylic acid curing agent include a curing agent having a structure in which the carboxyl groups in the general formula (1) are blocked as represented by the following general formula (3).
[0096] [Chemical formula 3]
[0097] General formula (3)
[0098]
[0099] (In general formula (3), R 3 Same as the above general formula (2).
[0100] In the compound represented by the above general formula (1), R 1 The compound other than a hydrogen atom may be a half ester obtained by the reaction of an alcohol compound with an acid anhydride. As the alcohol compound used in the reaction, the following may be cited as preferred examples: monohydric alcohol compounds such as ethanol, propanol, hexanol, octanol, and isopropanol; dihydric alcohol compounds such as ethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, and cyclohexanediol; trihydric alcohol compounds such as glycerol, pentanetriol, hexanetriol, cyclohexanetriol, benzenetriol, and trimethylolpropane; tetrahydric alcohol compounds such as pentaerythritol; more preferably, hexanol, isopropanol, 1,2-propylene glycol, 1,3-propylene glycol, 1,6-hexanediol, glycerol, trimethylolpropane, and pentaerythritol are cited.
[0101] Examples of the acid anhydride used in the above reaction include compounds represented by the following formula (4), and specific examples include 1,2-cyclohexanedicarboxylic acid anhydride and 1,3,4-cyclohexanetricarboxylic acid-3,4-anhydride as preferred examples.
[0102] [Chemical formula 4]
[0103] General formula (4)
[0104]
[0105] (In general formula (4), R 2 , a and m are the same as those in the above general formula (1).
[0106] From the viewpoint of compatibility, it is preferred to use a compound represented by the general formula (1) wherein R 1 A compound in which R 1 Examples of the compound having a hydrogen atom include alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; alicyclic tricarboxylic acids such as 1,2,4-cyclohexanetricarboxylic acid (CHTA); and alicyclic tetracarboxylic acids such as 1,2,4,5-cyclohexanetetracarboxylic acid. Among them, CHTA is preferred.
[0107] The acid equivalent of the polycarboxylic acid compound is preferably 55 g / mol or more, more preferably 60 g / mol or more, from the perspective of increasing the crosslinking density and the toughness of the cured film, and is preferably 600 g / mol or less, more preferably 500 g / mol or less from the perspective of compatibility. The above acid equivalent refers to the equivalent of the carboxyl group and is measured according to JIS K-0070-3 (1992).
[0108] In addition, the said polycarboxylic acid compound can be used individually by 1 type or in combination of 2 or more types.
[0109] Examples of the vinyl ether compound include alkyl vinyl ethers such as isopropyl vinyl ether, n-propyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, and cyclohexyl vinyl ether, among which n-propyl vinyl ether and isobutyl vinyl ether are preferred. The vinyl ether compounds may be used alone or in combination of two or more.
[0110] The blocked carboxylic acid curing agent can be obtained by reacting the polycarboxylic acid compound and the vinyl ether compound in the presence of an acid catalyst and a solvent as required at a temperature in the range of about 20° C. to 150° C.
[0111] From the aspects of reaction efficiency and yield, the molar equivalent ratio of the vinyl group of the vinyl ether compound to the carboxyl group of the polycarboxylic acid compound [(vinyl group / carboxyl group) molar equivalent ratio] is preferably 2 or less. The lower limit of the molar equivalent ratio is appropriately adjusted according to the application and is not particularly limited, and can be, for example, 0.5 or more, or 1 or more.
[0112] Moreover, as said acid catalyst, an acidic phosphate compound etc. are mentioned, for example.
[0113] In addition, the above-mentioned blocked carboxylic acid curing agent can be used individually by 1 type or in combination of 2 or more types.
[0114] From the perspective of heat resistance and hardness of the cured film, the molar equivalent ratio of the epoxy group in the above-mentioned epoxy compound to the carboxyl group and the blocked carboxyl group in the curing agent capable of reacting with the epoxy compound (carboxyl group and blocked carboxyl group / epoxy group) is preferably 0.2 or more, more preferably 0.5 or more, and from the perspective of adhesion of the cured film, it is preferably 1.6 or less, more preferably 1.2 or less.
[0115] In the quantum dot-containing curable composition of the present invention, when the above-mentioned thermosetting adhesive component is used as the above-mentioned curable adhesive component, from the perspective of suppressing the agglomeration of quantum dots in the cured product and the strength of the cured product, the total content of the compounds having two or more thermosetting functional groups in one molecule such as the above-mentioned epoxy compound is preferably 40% by mass or more, more preferably 50% by mass or more, relative to the total solid content of the above-mentioned quantum dot-containing curable composition. On the other hand, from the perspective of discharge stability and suppressing unevenness on the surface of the cured product, it is preferably 90% by mass or less, more preferably 80% by mass or less.
[0116] It should be noted that in the present invention, the solid content refers to all components other than the solvent.
[0117] In the quantum dot curable composition of the present invention, when the above-mentioned thermosetting adhesive component is used as the above-mentioned curable adhesive component, from the perspective of fully promoting the progress of the polymerization reaction and reducing the boiling and unevenness during the drying process, the content of the above-mentioned curing agent relative to the total solid content of the above-mentioned quantum dot curable composition is preferably 5 mass% or more, more preferably 10 mass% or more. On the other hand, from the perspective of discharge stability and suppression of unevenness on the surface of the cured product and storage stability, it is preferably 40 mass% or less, more preferably 30 mass% or less, and further preferably 25 mass% or less.
[0118] (2) Photocurable adhesive component
[0119] As a photocurable adhesive component, a combination of a photocurable resin and a photopolymerization initiator that can be polymerized and cured by light such as ultraviolet rays and electron beams is usually used. In the photocurable adhesive component, in order to impart film-forming properties and adhesion to the coated surface, it is preferred to include a polymer with a relatively high molecular weight. The so-called molecular weight is relatively high here, which means that the molecular weight is higher than the so-called monomer or oligomer, and the weight average molecular weight can be 3,000 or more as a standard. As a polymer with a relatively high molecular weight, any one of the polymers that do not have polymerization reactivity itself and the polymers that have polymerization reactivity itself can be used, in addition, more than two kinds can also be used in combination. And, the polymer with a relatively high molecular weight is used as the main body, and as required, a multifunctional monomer or oligomer with more than two photopolymerizable functional groups, a monofunctional monomer or oligomer with one photopolymerizable functional group, a photopolymerization initiator activated by light, and a sensitizer, etc. are used to form the photocurable adhesive component.
[0120] As polymers with relatively high molecular weight, for example, (meth)acrylic resins such as (meth)acrylic copolymers and styrene-(meth)acrylic copolymers, epoxy (meth)acrylate resins, etc. can be listed; among them, from the perspective of the dispersibility of quantum dots, (meth)acrylic resins such as (meth)acrylic copolymers and styrene-(meth)acrylic copolymers can be preferably used.
[0121] Examples of epoxy (meth)acrylate resins include epoxy (meth)acrylate compounds obtained by reacting a reaction product of an epoxy compound and a monocarboxylic acid containing an unsaturated group with an acid anhydride. The epoxy compound, the monocarboxylic acid containing an unsaturated group, and the acid anhydride can be appropriately selected from known compounds and used.
[0122] As the polymer having a relatively high molecular weight, in addition to (meth)acrylic resins such as (meth)acrylic copolymers and styrene-(meth)acrylic copolymers, and epoxy (meth)acrylate resins, thermoplastic resins such as polyester resins, maleic acid resins, polyolefin resins, polyamide resins, and polycarbonate resins may be used. Alternatively, a polymer used as a dispersant may be used.
[0123] From the viewpoint of improving the solubility in the above-mentioned specific solvent and the compatibility with the quantum dots, one or more resins selected from the above-mentioned (meth)acrylic resins, epoxy (meth)acrylate resins, polyester resins, and maleic acid resins can be preferably used.
[0124] As the polymer having a relatively high molecular weight, two or more kinds may be mixed and used, or one kind of resin may be used alone.
[0125] As the polymer having a relatively high molecular weight, a polymer having a photopolymerizable functional group such as an ethylenically unsaturated group in a side chain is preferred from the viewpoint of improving the film strength of the cured film.
[0126] In addition, from the perspective of the dispersibility of quantum dots, the acid value of the relatively high molecular weight polymer is preferably 200 mgKOH / g or less, more preferably 150 mgKOH / g or less, and further preferably 125 mgKOH / g or less.
[0127] The acid value refers to the mass (mg) of potassium hydroxide required to neutralize the acidic components contained in 1 g of the solid content of the polymer, and can be measured by the method defined in JIS K0070.
[0128] In addition, from the perspective of the dispersibility of quantum dots, the above-mentioned polymer with a relatively high molecular weight may also have an amine value. When having an amine value, the amine value is preferably greater than 40 mgKOH / g and less than 140 mgKOH / g, preferably less than 120 mgKOH / g, more preferably less than 100 mgKOH / g, and further preferably less than 80 mgKOH / g.
[0129] The amine value refers to the number of mg of potassium hydroxide equivalent to perchloric acid required to neutralize the amine component contained in 1 g of the solid content of the polymer, and can be measured by the method defined in JIS-K7237:1995.
[0130] The (meth)acrylic resin can be obtained, for example, by (co)polymerizing an ethylenically unsaturated monomer and, if necessary, other copolymerizable monomers by a known method.
[0131] As the ethylenically unsaturated monomer, for example, (meth)acrylate monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate can be preferably used. The structural unit derived from the ethylenically unsaturated monomer containing an ester group such as the (meth)acrylate monomer can function as a component that improves the solubility in the solvent and further improves the solvent re-solubility. It should be noted that the structural unit derived from the monomer means a structural unit in which the polymerizable carbon-carbon double bond (C=C) in the monomer becomes a single bond (CC).
[0132] In the (meth) acrylic resin, from the aspect of obtaining a good pattern, the content of the structural unit having an ester group is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of 100% by mass of the monomer components used in the synthesis of the copolymer. On the other hand, from the aspect of the dispersibility of the quantum dots, the content of the structural unit having an ester group is preferably 95% by mass or less, more preferably 80% by mass or less, relative to the total amount of 100% by mass of the monomer components used in the synthesis of the copolymer.
[0133] From the aspect of excellent adhesion of the cured film, the above-mentioned (meth) acrylic resin preferably has a hydrocarbon ring. By making the (meth) acrylic resin have a hydrocarbon ring with a bulky group, the solvent resistance of the obtained cured film, especially the swelling of the cured film, is suppressed. The effect is not yet clear, but it is speculated that by making the cured film contain a bulky hydrocarbon ring, the movement of molecules in the cured film is suppressed, and as a result, the strength of the coating film is increased and the swelling caused by the solvent is suppressed.
[0134] Examples of such hydrocarbon rings include cyclic aliphatic hydrocarbon rings which may have a substituent, aromatic rings which may have a substituent, and combinations thereof. The hydrocarbon ring may also have a substituent such as a carbonyl group, a carboxyl group, an oxycarbonyl group, an amide group, etc. Among them, when an aliphatic ring is included, the heat resistance and adhesion of the cured film are improved, and the transparency of the obtained cured film is improved.
[0135] Specific examples of hydrocarbon rings include: aliphatic hydrocarbon rings such as cyclopropane, cyclobutane, cyclopentane, cyclohexane, norbornane, tricyclo[5.2.1.0(2,6)]decane (dicyclopentane), and adamantane; aromatic rings such as benzene, naphthalene, anthracene, phenanthrene, and fluorene; chain polycyclic rings such as biphenyl, terphenyl, diphenylmethane, triphenylmethane, and isodiphenylethylene; and the Cardo structure shown in the following chemical formula (i).
[0136] [Chemical formula 5]
[0137] Chemical formula (i)
[0138]
[0139] Furthermore, the (meth)acrylic resin preferably has a maleimide structure represented by the following general formula (ii).
[0140] [Chemical formula 6]
[0141] Formula (ii)
[0142]
[0143] (In general formula (ii), R M is an optionally substituted hydrocarbon ring. )
[0144] As R in the above general formula (ii) M Specific examples of the optionally substituted hydrocarbon ring in include the same hydrocarbon rings as the specific examples of the hydrocarbon rings described above.
[0145] In the case of containing an aliphatic ring as the hydrocarbon ring, it is preferred from the viewpoint that the heat resistance and adhesion of the cured film are improved and the brightness of the obtained cured film is improved.
[0146] In addition, when the cardo structure represented by the above chemical formula (i) is included, it is particularly preferred from the viewpoint of improving the curability of the cured film and improving the solvent resistance.
[0147] As the ethylenically unsaturated monomer having the above-mentioned hydrocarbon ring, for example, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, styrene, etc. can be cited; from the perspective of improving the dispersibility of quantum dots, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, adamantyl (meth)acrylate, benzyl (meth)acrylate, and styrene are preferred, and cyclohexyl (meth)acrylate and styrene are particularly preferred.
[0148] In addition, as the above-mentioned (meth)acrylic resin, a (meth)acrylic resin containing a (meth)acrylic copolymer having a structural unit having an olefinic double bond in a side chain can be preferably used. That is, as the above-mentioned curable adhesive component, a photocurable adhesive component containing a (meth)acrylic resin containing a (meth)acrylic copolymer having a structural unit having an olefinic double bond in a side chain can be preferably used.
[0149] Moreover, as the said (meth)acrylic-type resin, the (meth)acrylic-type copolymer containing the structural unit which has a hydrocarbon ring and the structural unit which has an ethylenic double bond can be used more preferably.
[0150] In the case of a (meth)acrylic copolymer containing a structural unit having an ethylenic double bond in a side chain, crosslinking bonds can be formed between (meth)acrylic resins and between the (meth)acrylic resin and a photopolymerizable compound during the curing step of the composition, thereby improving the film strength of the cured film and fixing the quantum dots to maintain dispersibility.
[0151] In addition, when used in combination with quantum dots, a (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain is less susceptible to the effects of heat and light during the manufacturing process or display, can maintain a constant distance between quantum dots, and can prevent excitation suppression.
[0152] The method of introducing olefinic double bonds into the (meth)acrylic copolymer can be appropriately selected from conventionally known methods. Examples thereof include: a method of introducing a structural unit having a carboxyl group into the copolymer in advance, and adding a compound having both an epoxy group and an olefinic double bond in the molecule, such as glycidyl (meth)acrylate, to the carboxyl group to introduce an olefinic double bond into the side chain; and a method of introducing a structural unit having a hydroxyl group into the copolymer in advance, and adding a compound having an isocyanate group and an olefinic double bond in the molecule to introduce an olefinic double bond into the side chain.
[0153] As the ethylenically unsaturated monomer containing a carboxyl group from which the structural unit having a carboxyl group is derived, for example, (meth) acrylic acid, vinyl benzoic acid, maleic acid, maleic acid monoalkyl ester, fumaric acid, itaconic acid, crotonic acid, cinnamic acid, acrylic acid dimer, etc. can be cited. In addition, the addition reaction product of a monomer having a hydroxyl group such as (meth) 2-hydroxyethyl acrylate and a cyclic anhydride such as maleic anhydride or phthalic anhydride, cyclohexane dicarboxylic anhydride, ω-carboxyl-polycaprolactone mono(meth) acrylate, etc. can also be used. In addition, anhydride-containing monomers such as maleic anhydride, itaconic anhydride, citraconic anhydride, etc. can also be used as precursors of the carboxyl group. Among them, (meth) acrylic acid is particularly preferred from the aspects of copolymerizability, cost, solubility, glass transition temperature, etc.
[0154] In the (meth)acrylic copolymer having a structural unit having an olefinic double bond in a side chain, the content ratio of the structural unit having an olefinic double bond in a side chain is preferably 5% by mass or more, more preferably 10% by mass or more, relative to 100% by mass of the total amount of the monomer components, from the perspective of maintaining the dispersibility of the quantum dots. On the other hand, from the perspective of the storage stability of the composition, it is preferably 50% by mass or less, more preferably 40% by mass or less.
[0155] In the (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain, the acid value is preferably 120 mgKOH / g or less, more preferably 80 mgKOH / g or less, and even more preferably 70 mgKOH / g or less, from the viewpoint of dispersibility of quantum dots.
[0156] In addition, from the aspects of the dispersibility, storage stability, curability, solvent resistance, adhesion and heat resistance of the quantum dots, the above-mentioned (meth)acrylic resin preferably contains a thermally latent (meth)acrylic copolymer having a structural unit derived from a (meth)acrylate monomer containing a tertiary carbon and a structural unit having a hydroxyl group.
[0157] That is, as the above-mentioned curable adhesive component, a photocurable adhesive component containing a (meth)acrylic resin can be preferably used, and the (meth)acrylic resin contains a thermal latent (meth)acrylic copolymer having a structural unit derived from a (meth)acrylate monomer containing a tertiary carbon and a structural unit having a hydroxyl group.
[0158] By heat, the OC bond between the oxygen atom adjacent to the (meth)acryloyl group and the tertiary carbon atom adjacent to the structural unit derived from the (meth)acrylic acid ester monomer containing tertiary carbon of the above-mentioned heat-latent (meth)acrylic acid copolymer is cut, thereby easily decomposing into (meth)acrylic acid and a stable compound generated on the tertiary carbon atom side. Therefore, for example, when the quantum dot-containing curable composition of the present invention contains the above-mentioned heat-latent (meth)acrylic acid copolymer, after the polymerization reaction of the curable adhesive component in the quantum dot-containing curable composition is carried out, a heating treatment is further carried out, thereby decomposing the structural unit derived from the (meth)acrylic acid ester monomer containing tertiary carbon to generate a (meth)acrylic acid unit and a stable compound generated on the tertiary carbon atom side. In addition, the hydroxyl group in the above-mentioned heat-latent (meth)acrylic acid copolymer reacts with the carboxyl group of the generated (meth)acrylic acid unit to generate an ester crosslinking structure, thereby improving the curability of the curable composition and the solvent resistance and heat resistance after curing. In addition, it is believed that the above-mentioned heat-latent (meth) acrylic copolymer can improve the storage stability of the quantum dot-containing curable composition because the carboxyl group is blocked, and the film thickness of the cured film can be reduced, thereby improving the adhesion. Furthermore, when the above-mentioned heat-latent (meth) acrylic copolymer is used in combination with quantum dots, it is not easily affected by heat and light during the manufacturing process or display, and the distance between quantum dots can be kept fixed, and excitation suppression can be prevented, so it is preferred.
[0159] The (meth)acrylate monomer containing tertiary carbon preferably has a structure in which an oxygen atom adjacent to the (meth)acryloyl group is bonded to a tertiary carbon atom. That is, the (meth)acrylate monomer containing tertiary carbon preferably has a structure in which an oxygen atom adjacent to the (meth)acryloyl group is bonded to a tertiary carbon atom. It should be noted that the so-called tertiary carbon atom means a carbon atom having three other carbon atoms bonded to the carbon atom.
[0160] The tertiary carbon-containing (meth)acrylate monomer is preferably a compound having one (meth)acryloyl group in the molecule, and examples thereof include compounds represented by the following general formula (5).
[0161] CH2=C(R a )-C(=O)-OA (5)
[0162] (R a represents a hydrogen atom or a methyl group, and A represents a monovalent organic group having a structure having a tertiary carbon atom on the oxygen atom side.)
[0163] In the above general formula (5), the organic group represented by A can be, for example, -C(R b )(R c )(R d ) is represented by. In this case, R b , R c and R d Preferably, they are the same or different hydrocarbon groups having 1 to 30 carbon atoms, and the hydrocarbon groups may be saturated or unsaturated. In addition, they may have a cyclic structure and may have a substituent. b , R c and R d They may also be linked to each other at the end portions to form a ring structure.
[0164] It should be noted that in the present invention, as described below, from the perspective that the new compound generated by cutting the OC bond between the oxygen atom adjacent to the (meth)acryloyl group and the tertiary carbon atom in the above A adjacent thereto is easily volatile, the carbon number of the organic group represented by the above A is preferably 12 or less. Among them, the organic group represented by the above A is preferably a group derived from at least one selected from tert-butyl (meth)acrylate and tert-amyl (meth)acrylate. In addition, the organic group represented by the above A may also have a branched structure.
[0165] Here, in the above-mentioned tertiary carbon-containing (meth)acrylate monomer, the tertiary carbon atom bonded to the oxygen atom adjacent to the (meth)acryloyl group is preferably bonded to a hydrogen atom at least one of the adjacent carbon atoms. For example, in the case where the tertiary carbon-containing (meth)acrylate monomer is a compound represented by the above-mentioned general formula (5) and A is -C(R b )(Rc )(R d In the case of a group represented by b , R c and R d At least one of the carbon atoms contains one or more hydrogen atoms and the carbon atom is bonded to a tertiary carbon atom. In such a form, by heating, the OC bond between the oxygen atom adjacent to the (meth)acryloyl group and the tertiary carbon atom adjacent thereto is cut to generate (meth)acrylic acid, and a double bond (C=C) is formed between the tertiary carbon atom and the carbon atom adjacent thereto, thereby generating a new compound more stably.
[0166] Since the novel compound is easily volatilized and the thickness of the cured product (cured film) can be reduced while increasing the concentration of quantum dots in the cured product (cured film), the R b , R c and R d The hydrocarbon group in is preferably a saturated hydrocarbon group having 1 to 15 carbon atoms, more preferably a saturated hydrocarbon group having 1 to 10 carbon atoms, further preferably a saturated hydrocarbon group having 1 to 5 carbon atoms, and particularly preferably a saturated hydrocarbon group having 1 to 3 carbon atoms.
[0167] Among them, the organic group represented by A is preferably at least one selected from the group consisting of a tert-butyl group and a tert-amyl group.
[0168] In the above-mentioned thermal latent (meth) acrylate copolymer, from the aspect of further exerting the above-mentioned effect, the content ratio of the above-mentioned (meth) acrylate monomer unit containing tertiary carbon is preferably 5 mass % or more, more preferably 15 mass % or more, and particularly preferably 20 mass % or more, relative to the total amount of monomer components 100 mass %. From the viewpoint of further improving pattern characteristics, the upper limit of the above-mentioned content ratio is preferably 90 mass % or less, more preferably 75 mass % or less, and further preferably 60 mass % or less.
[0169] The structural unit having a hydroxyl group in the above-mentioned heat-latent (meth)acrylate polymer is preferably a structural unit having a hydroxyl group in a side chain. As the monomer from which the structural unit having a hydroxyl group is derived, for example, preferably hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2,3-hydroxypropyl (meth)acrylate can be cited.
[0170] In the above-mentioned thermal latent (meth)acrylate copolymer, the content ratio of the structural unit having a hydroxyl group is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more, based on 100% by mass of the total amount of the monomer components, from the viewpoint of curability and solvent resistance. On the other hand, from the viewpoint of suppressing whitening of the surface of the cured product, it is preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 35% by mass or less.
[0171] The thermally latent (meth)acrylate polymer preferably has a structural unit derived from (meth)acrylic acid from the viewpoints of copolymerizability, cost, solubility, glass transition temperature, and the like.
[0172] In the above-mentioned (meth)acrylate copolymer, from the perspective of maintaining the dispersibility of quantum dots, the content ratio of the structural unit derived from (meth)acrylic acid relative to 100% by mass of the total amount of the monomer components is preferably 5% by mass or more, more preferably 10% by mass or more, and from the perspective of stability, it is preferably 35% by mass or less, more preferably 25% by mass or less.
[0173] From the viewpoint of the dispersibility of the quantum dots, the acid value of the thermal latent (meth)acrylate polymer is preferably 120 mgKOH / g or less, more preferably 80 mgKOH / g or less, and even more preferably 70 mgKOH / g or less.
[0174] In addition, from the perspective of the dispersibility of quantum dots, the above-mentioned thermal latent (meth)acrylate polymer preferably contains a structural unit having a tertiary amine. As the monomer from which the above-mentioned structural unit having a tertiary amine is derived, for example, preferably exemplified are (meth)acrylates containing alkyl-substituted amino groups such as dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and diethylaminopropyl (meth)acrylate; and (meth)acrylamides containing alkyl-substituted amino groups such as dimethylaminoethyl (meth)acrylamide and dimethylaminopropyl (meth)acrylamide.
[0175] In the above-mentioned (meth)acrylate copolymer, from the perspective of maintaining the dispersibility of quantum dots, the content ratio of the structural unit having a tertiary amine relative to the total amount of 100 mass % of the monomer components is preferably 5 mass % or more, more preferably 10 mass % or more, and on the other hand, from the perspective of stability, it is preferably 35 mass % or less, more preferably 25 mass % or less.
[0176] From the perspective of quantum dot dispersibility, the amine value of the above-mentioned thermal latent (meth)acrylate polymer is preferably 40 mgKOH / g or more and 140 mgKOH / g or less, preferably 120 mgKOH / g or less, more preferably 100 mgKOH / g or less, and further preferably 80 mgKOH / g or less.
[0177] In addition, from the aspect of improving the film strength of the cured film, the above-mentioned heat-latent (meth)acrylate polymer preferably has a structural unit having an ethylenically unsaturated group in the side chain. The structural unit having an ethylenically unsaturated group in the side chain is obtained, for example, by introducing a structural unit derived from (meth)acrylic acid during the synthesis of the above-mentioned heat-latent (meth)acrylate polymer, and adding, for example, glycidyl (meth)acrylate to the carboxyl group of the structural unit and the hydroxyl group of the above-mentioned monomer unit having a hydroxyl group.
[0178] The thermally latent (meth)acrylate polymer can be obtained, for example, by polymerizing a (meth)acrylate monomer containing a tertiary carbon, a monomer having a hydroxyl group, and, if necessary, other monomer components.
[0179] Examples of the other monomer components include monomers from which the structural unit having a hydrocarbon ring is derived, (meth)acrylate monomers containing no tertiary carbon, and monomers from which a structural unit having an ethylenic double bond in a side chain is derived.
[0180] In the present invention, the (meth)acrylic resin preferably contains at least one selected from a (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain and the thermally latent (meth)acrylate polymer from the perspective of the dispersibility of the quantum dots.
[0181] In the case where the quantum dot curable composition of the present invention contains a (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain, from the perspective of fully exerting the effect of the (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain, the content ratio of the (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain relative to the total solid content of the quantum dot curable composition is preferably 10% by mass or more, more preferably 15% by mass or more, and on the other hand, from the perspective of sufficiently containing other components, it is preferably 35% by mass or less, more preferably 25% by mass or less.
[0182] In addition, when the quantum dot-curable composition of the present invention contains the above-mentioned thermally latent (meth)acrylate polymer, from the perspective of fully exerting the effect of the thermally latent (meth)acrylate polymer, the content ratio of the above-mentioned thermally latent (meth)acrylate polymer relative to the total solid content of the quantum dot-curable composition is preferably 10% by mass or more, more preferably 15% by mass or more. On the other hand, from the perspective of sufficiently containing other components, it is preferably 35% by mass or less, more preferably 25% by mass or less.
[0183] In addition, in the present invention, as the above-mentioned (meth) acrylic resin, from the aspect of the dispersibility of quantum dots, a block copolymer used as a dispersant can also be preferably used. The (meth) acrylic resin of the block copolymer used as a dispersant usually has a block portion containing a structural unit having an acidic group such as a carboxyl group, or a basic group such as a tertiary amine, a tertiary amine salt, a quaternary ammonium salt, and a block portion containing a structural unit having one or more ester groups as a block portion. The structural unit having a carboxyl group, the structural unit having a tertiary amine, and the structural unit having an ester group can be the same as above, and other structural units having an acidic group and the structural unit having a basic group can also appropriately use known structural units.
[0184] A commercially available (meth)acrylic resin may be appropriately selected and used as the dispersant.
[0185] From the perspective of the dispersibility of the quantum dots, the amine value of the (meth)acrylic resin of the block copolymer used as a dispersant is also preferably 40 mgKOH / g or more and 140 mgKOH / g or less, preferably 120 mgKOH / g or less, more preferably 100 mgKOH / g or less, and further preferably 80 mgKOH / g or less.
[0186] The preferred weight average molecular weight (Mw) of the (meth)acrylic copolymer contained in the (meth)acrylic resin is preferably in the range of 1,000 to 50,000, and more preferably 3,000 to 20,000. If the weight average molecular weight of the (meth)acrylic copolymer is 1,000 or more, it is preferred from the perspective of excellent adhesive function after curing, and if it is 50,000 or less, it is preferred from the perspective of improved discharge properties.
[0187] The weight average molecular weight (Mw) of the polymer can be measured by using polystyrene as a standard substance and THF as an eluent using Shodex GPC System-21H.
[0188] From the perspective of obtaining the effects of improved film strength of the cured film and excellent adhesion to the substrate, the ethylenically unsaturated bond equivalent when the side chain of the (meth) acrylic resin has an ethylenically unsaturated group is preferably in the range of 100 to 2000, and particularly preferably in the range of 140 to 1500. If the ethylenically unsaturated bond equivalent is 2000 or less, excellent adhesion is achieved. In addition, if it is 100 or more, the proportion of other structural units such as structural units having hydrocarbon rings can be relatively increased, thereby improving heat resistance, etc.
[0189] Here, the ethylenically unsaturated bond equivalent refers to the weight average molecular weight per 1 mol of the ethylenically unsaturated bonds in the (meth)acrylic resin, and is represented by the following formula (1).
[0190] Formula (1) Ethylenically unsaturated bond equivalent (g / mol) = W (g) / M (mol)
[0191] (In formula (1), W represents the mass (g) of the (meth)acrylic resin, and M represents the number of moles (mol) of ethylenic double bonds contained in the (meth)acrylic resin W (g).)
[0192] The ethylenically unsaturated bond equivalent can also be calculated by measuring the number of ethylenic double bonds contained per 1 g of the (meth)acrylic resin, for example, according to the test method for iodine value described in JIS K 0070:1992.
[0193] In the quantum dot curable composition of the present invention, the (meth) acrylic resin may be used alone or in combination of two or more, and its content is not particularly limited. The (meth) acrylic resin is preferably in the range of 5% to 60% by mass, and more preferably in the range of 10% to 40% by mass, relative to the total solid content of the quantum dot curable composition. If the content of the (meth) acrylic resin is above the above lower limit, it is preferred from the perspective of improving the dispersibility of the quantum dots. In addition, if the content of the (meth) acrylic resin is below the above upper limit, it is preferred from the perspective of improving the discharge property.
[0194] In addition, in the quantum dot curable composition of the present invention, the polymer with a relatively high molecular weight can be used alone or in combination of two or more. There is no particular restriction on its content. The polymer with a relatively high molecular weight is preferably in the range of 5% to 60% by mass, and more preferably in the range of 10% to 40% by mass, relative to the total solid content of the quantum dot curable composition. If the content of the polymer with a relatively high molecular weight is above the lower limit, it is preferred from the perspective of improving the dispersibility of the quantum dots. In addition, if the content of the polymer with a relatively high molecular weight is below the upper limit, it is preferred from the perspective of improving the discharge property.
[0195] (Multifunctional monomer)
[0196] The polyfunctional monomer is not particularly limited as long as it can be polymerized by the photoinitiator described below, but generally a compound having two or more ethylenically unsaturated double bonds is used, and polyfunctional (meth)acrylates having two or more acryloyl or methacryloyl groups are particularly preferred.
[0197] As such a polyfunctional (meth)acrylate, what is necessary is just to select suitably from conventionally well-known (meth)acrylates and use it.
[0198] The multifunctional (meth)acrylate can be used alone or in combination of two or more. In addition, when the quantum dot curable composition of the present invention is required to have excellent photocurability (high sensitivity), the multifunctional monomer preferably has three (trifunctional) or more polymerizable double bonds, preferably poly (meth)acrylates of trivalent or more polyols or their dicarboxylic acid modified substances, specifically, preferably trimethylolpropane tri (meth)acrylate, pentaerythritol tri (meth)acrylate, succinic acid modified substance of pentaerythritol tri (meth)acrylate, pentaerythritol tetra (meth)acrylate, dipentaerythritol tetra (meth)acrylate, dipentaerythritol penta (meth)acrylate, succinic acid modified substance of dipentaerythritol penta (meth)acrylate, dipentaerythritol hexa (meth)acrylate, etc.
[0199] The content of the above-mentioned multifunctional monomer used in the quantum dot curable composition is not particularly limited. The multifunctional monomer is preferably in the range of 5 to 60% by mass, and more preferably in the range of 10 to 40% by mass, relative to the total solid content of the quantum dot curable composition. If the content of the multifunctional monomer is above the above lower limit, it is preferred from the aspect that photocuring is easy to be fully performed. In addition, in order to fully contain other components, the content of the multifunctional monomer is preferably below the above upper limit.
[0200] (Photoinitiator)
[0201] The photoinitiator is not particularly limited, and one type or a combination of two or more types of conventionally known photoinitiators can be used.
[0202] Examples of the photoinitiator include aromatic ketones, benzoin ethers, halomethyl oxadiazole compounds, α-aminoketones, biimidazoles, N,N-dimethylaminobenzophenone, halomethyl-S-triazine compounds, thioxanthones, etc. Specific examples of the photoinitiator include aromatic ketones such as benzophenone, 4,4′-bisdiethylaminobenzophenone, and 4-methoxy-4′-dimethylaminobenzophenone; benzoin ethers such as benzoin methyl ether; benzoins such as ethylbenzoin; biimidazoles such as 2-(o-chlorophenyl)-4,5-phenylimidazole dimer; halomethyl oxadiazole compounds such as 2-trichloromethyl-5-(p-methoxyphenyl)-1,3,4-oxadiazole; 2-(4-Butoxy-naphthalen-1-yl)-4,6-bis-trichloromethyl-S-triazine and other halomethyl-S-triazine compounds; 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 1,2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone, 1-hydroxy-cyclohexyl-phenyl ketone, benzyl, Benzoylbenzoic acid, benzoylbenzoic acid methyl ester, 4-benzoyl-4′-methyl diphenyl sulfide, benzyl methyl ketal, dimethylaminobenzoate, isopentyl p-dimethylaminobenzoate, 2-n-butoxyethyl-4-dimethylaminobenzoate, 2-chlorothioxanthone, 2,4-diethylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 4-benzoyl-methyl diphenyl sulfide, 1-hydroxy-cyclohexyl-phenyl ketone, 2-benzyl -2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, α-dimethoxy-α-phenylacetophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, etc.
[0203] Among them, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone, 4,4′-bis(diethylamino)benzophenone, and diethylthioxanthone can be preferably used.
[0204] Particularly preferred are photoinitiators that do not interfere with the light absorption of quantum dots, and preferably photoinitiators that have less absorption at the excitation wavelength of quantum dots, i.e., 350 nm or more or 400 nm or more. As such photoinitiators, for example, α-hydroxyketone-based initiators having absorption near 250 nm can be cited. There are 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one (Irgacure 127), 1-hydroxy-cyclohexyl-phenyl-ketone (Irgacure 184), 2,2-dimethoxy-1,2-diphenylethane-1-one (Irgacure 651), 2-hydroxy-2-methyl-1-phenyl-propane-1-one (Irgacure 1173), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one (Irgacure 2959), etc. It should be noted that the above-mentioned Irgacure 127, 184, 651, 1173, and 2959 are trade names and are available from BASF.
[0205] The total content of the photoinitiators is preferably 5% by mass to 15% by mass based on the total solid content of the quantum dot-curable composition.
[0206] The content of the photoinitiator is generally about 0.01 to 100 parts by mass, and preferably 5 to 60 parts by mass, based on 100 parts by mass of the polyfunctional monomer.
[0207] When the content of the photoinitiator is at least the lower limit, photocuring can be easily and sufficiently performed. On the other hand, when it is at most the upper limit, it is preferable from the viewpoint that yellowing of the obtained cured film can be reduced and a decrease in transparency can be suppressed.
[0208] As for the binder components used in the quantum dot curable composition of the present invention, it is preferred that their total content is 35% by mass to 97% by mass relative to the total solid content of the quantum dot curable composition, and more preferably 40% by mass to 96% by mass. If it is above the above lower limit, it is preferred from the aspect of obtaining a cured film with excellent hardness and adhesion to the substrate. In addition, if it is below the above upper limit, it is preferred from the aspect of suppressing the generation of micro-wrinkles caused by heat shrinkage.
[0209] <Quantum dot>
[0210] The quantum dots used in the present invention are fine particles of compound semiconductors having a size of several nm to several tens of nm, and are not particularly limited as long as they are light-emitting materials that produce a quantum confinement effect (quantum size effect).
[0211] As the quantum dots, known quantum dots can be used, one kind can be used alone, or two or more kinds can be mixed and used. Known quantum dots include quantum dots (R) having a luminescent center wavelength in a wavelength band ranging from 600nm to 680nm, quantum dots (G) having a luminescent center wavelength in a wavelength band ranging from 500nm to 600nm, and quantum dots (B) having a luminescent center wavelength in a wavelength band ranging from 400nm to 500nm. The quantum dots (R) are excited by excitation light and emit red light, the quantum dots (G) emit green light, and the quantum dots (B) emit blue light.
[0212] Specifically, the quantum dots include II-VI semiconductor compounds such as MgS, MgSe, MgTe, CaS, CaSe, CaTe, SrS, SrSe, SrTe, BaS, BaSe, BaTe, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, HgS, HgSe and HgTe; III-V semiconductor compounds such as AlN, AlP, AlAs, AlSb, GaAs, GaP, GaN, GaSb, InN, InAs, InP, InSb, TiN, TiP, TiAs and TiSb; semiconductor crystals containing IV semiconductors such as Si, Ge and Pb, and semiconductor compounds containing three or more elements such as InGaP. Alternatively, the semiconductor compounds doped with Eu can be used. 3+ , Tb 3+ 、Ag + , Cu + A semiconductor crystal composed of cations of rare earth metals or transition metals.
[0213] In addition, the quantum dots may include one semiconductor compound or more than two semiconductor compounds, for example, a core-shell structure having a core including a semiconductor compound and a shell including a semiconductor compound different from the core. As core-shell quantum dots, materials with a band gap higher than the semiconductor compound forming the core are used as semiconductor compounds constituting the shell to enclose the excitons in the core, thereby improving the luminous efficiency of the quantum dots. As core-shell structures (core / shell) having such a band gap relationship, for example, CdSe / ZnS, CdSe / ZnSe, CdSe / CdS, CdTe / CdS, InP / ZnS, CuInS / ZnS, etc. can be cited.
[0214] The size of the quantum dot can be appropriately adjusted according to the material constituting the quantum dot in order to obtain light of the desired wavelength. The energy band gap of the quantum dot increases as the particle size decreases. That is, as the crystal size decreases, the emission of the quantum dot shifts to the blue side, that is, the high energy side. Therefore, by changing the size of the quantum dot, its emission wavelength can be adjusted over the wavelength range of the spectrum in the ultraviolet region, the visible region, and the infrared region.
[0215] In addition, as the above-mentioned quantum dots, quantum dots formed by the ligand with a coordination group coordinated to the surface can also be used. As the above-mentioned coordination group, there can be listed: amino, carboxyl, sulfhydryl, phosphino, and phosphine oxide groups. As the above-mentioned coordination group, for example: hexylamine, decylamine, hexadecylamine, octadecylamine, oleylamine, myristylamine, laurylamine, oleic acid, mercaptopropionic acid, trioctylphosphine, trioctylphosphine oxide and polyethylene glycol can be listed. Among them, from the aspect of preventing the extinction caused by surface defects, it is preferably a quantum dot formed by the ligand with at least one coordination group selected from trioctylphosphine, trioctylphosphine oxide, octadecylamine and oleylamine, and more preferably a quantum dot formed by the ligand with at least one coordination group selected from trioctylphosphine oxide, octadecylamine and oleylamine.
[0216] It should be noted that the quantum dots formed by the ligand having the above-mentioned coordinating group coordinated to the surface can be synthesized by the method described in, for example, J.Am.Chem.Soc., 115, pp8706-8715 (1993) or J.Phys.Chem., 101, pp9463-9475 (1997), and commercially available products can also be preferably used.
[0217] In addition, as the quantum dots, quantum dots whose surfaces are protected by protective materials can also be used. As the protective materials, for example, protective materials having one or more hydrophilic groups and hydrophobic groups in one molecule can be cited, and as the hydrophobic group, at least one residue selected from triphenylamine derivatives, arylamine derivatives, oxadiazole derivatives, dinaphthyl anthracene derivatives, distyryl arylene derivatives, carbazole derivatives, benzimidazole derivatives, and hydroxyquinoline aluminum complex derivatives can be included.
[0218] Examples of the hydrophilic group include a carboxyl group, an amine group, a hydroxyl group, a thiol group, an aldehyde group, a sulfonic acid group, an amide group, a sulfonamide group, a phosphoric acid group, a phosphine group, and a phosphine oxide group.
[0219] From the perspective of luminous intensity, the content of quantum dots contained in the total solid component of the quantum dot-containing curable composition of the present invention is preferably 0.1 mass % or more, more preferably 0.3 mass % or more. On the other hand, from the perspective of discharge stability and dispersibility of the inkjet method, it is preferably 40 mass % or less, more preferably 35 mass % or less.
[0220] <Optional Additives>
[0221] The quantum dot-containing curable composition of the present invention may also contain various additives as required, such as antioxidants, polymerization terminators, chain transfer agents, leveling agents, plasticizers, surfactants, defoamers, silane coupling agents, ultraviolet absorbers, adhesion promoters, etc.
[0222] <Method for producing a quantum dot-containing curable composition>
[0223] The quantum dot-containing curable composition of the present invention can be prepared by putting the above-mentioned components into the above-mentioned solvent and mixing them, so that the solid components are dissolved or dispersed. For example, the following method can be preferably used: pre-prepare a curable adhesive composition in which adhesive components such as a curable resin and a curing agent are dissolved or dispersed in a solvent, add the curable adhesive composition, quantum dots, and any additional components, and then add a solvent and mix them. As a solvent for preparing the above-mentioned curable adhesive composition, it is preferably selected from at least one of the above-mentioned first solvent and the above-mentioned second solvent. In addition, for example, it is preferred that after preparing the above-mentioned curable adhesive composition, at least one selected from the above-mentioned first solvent and the above-mentioned second solvent is further added, thereby making the solvent in the quantum dot-containing curable composition a solvent containing the above-mentioned first solvent and the above-mentioned second solvent.
[0224] That is, as a method for producing the quantum dot-containing curable composition of the present invention, for example, the following production method can be cited, and the production method has the following steps:
[0225] preparing a curable adhesive composition containing the curable adhesive component and at least one selected from the first solvent and the second solvent; and
[0226] The curable adhesive composition, the quantum dots, and at least one selected from the first solvent and the second solvent are mixed, and
[0227] The mixed solvent of the solvent in the curable adhesive composition and the solvent used in the mixing step contains the first solvent and the second solvent.
[0228] When a polymer that functions as a dispersant is used as the curable binder component, the following production method may be mentioned. The production method includes the following steps:
[0229] preparing a curable adhesive composition containing a curable adhesive component other than a polymer functioning as a dispersant and at least one selected from the first solvent and the second solvent;
[0230] Preparing a quantum dot dispersion by dispersing the quantum dots, a polymer functioning as a dispersant, and at least one selected from the first solvent and the second solvent; and
[0231] The curable adhesive composition, the dispersion, and, if necessary, at least one selected from the first solvent and the second solvent are mixed together, and
[0232] The mixed solvent of the solvent in the curable adhesive composition and the solvent used in the mixing step contains the first solvent and the second solvent.
[0233] <Applications>
[0234] The use of the quantum dot-containing curable composition of the present invention is not particularly limited, and it can be used, for example, to form a quantum dot-containing cured layer possessed by various optical components used in the following display devices, etc. In addition, the quantum dot-containing curable composition of the present invention is a composition suitable for forming a quantum dot-containing layer by inkjet, and can be preferably used for inkjet.
[0235] Examples of the optical member include semiconductor optical members such as a light conversion member and a light emitting member.
[0236] II. Quantum dot-containing solid
[0237] The quantum dot-containing cured product of the present invention is a cured product of the quantum dot-containing curable composition of the present invention.
[0238] The quantum dot-containing cured product of the present invention has less unevenness and the aggregation of quantum dots in the cured product is suppressed, so that a desired color can be obtained.
[0239] The quantum dot-containing cured product of the present invention can be obtained, for example, by forming a quantum dot-containing layer as a coating of the above-mentioned quantum dot-containing curable composition of the present invention by inkjet method, and curing the quantum dot-containing layer. The method for forming the quantum dot-containing layer and the method for curing can be, for example, the same method as used in the method for manufacturing the optical component described below.
[0240] When the quantum dot-containing cured product of the present invention is used as a quantum dot-containing cured layer of various optical members such as light conversion members and light-emitting members used in display devices described below, high brightness and a wide color reproduction range can be achieved.
[0241] The quantum dot-containing cured product of the present invention can be made into a quantum dot-containing cured product having desired light-emitting properties by appropriately adjusting the type and content of quantum dots.
[0242] The color reproduction area of the quantum dot-containing cured product of the present invention can realize the luminous colors of red, green, blue and white by using a blue light emitting diode (Blue LED) as a light source. More specifically, in the chromaticity coordinates (x, y), red with Rx=0.60-0.71, Ry=0.29-0.35, green with Gx=0.16-0.35, Gy=0.55-0.80, blue with Bx=0.13-0.16, By=0.03-0.10 can be realized.
[0243] It should be noted that the above chromaticity coordinates x and y are chromaticity coordinates in the XYZ colorimetric system of JIS Z8701:1931 obtained by color measurement using a blue LED light source.
[0244] III. Method for manufacturing optical component
[0245] The method for manufacturing an optical member of the present invention is characterized by comprising the following steps:
[0246] The quantum dot-containing curable composition of the present invention is selectively attached to a predetermined area on a substrate by inkjet method to form a quantum dot-containing layer; and
[0247] The quantum dot-containing layer is cured to form a quantum dot-containing cured layer.
[0248] In addition, the method for producing an optical member of the present invention may further include other steps in addition to the above-mentioned steps as necessary.
[0249] The method for producing an optical component of the present invention uses the quantum dot-containing curable composition of the present invention, so that a quantum dot-containing cured layer with reduced unevenness can be formed. In addition, since aggregation of quantum dots in the quantum dot-containing cured layer is suppressed, desired color development can be obtained.
[0250] It should be noted that the quantum dot-containing cured layer can be adjusted to have desired color development characteristics by appropriately selecting the type and content of quantum dots, and has the same color reproduction range as the above-mentioned quantum dot-containing cured product of the present invention.
[0251] In the method for producing an optical member of the present invention, it is preferable that the predetermined region on the substrate is a region surrounded by partition walls on the substrate.
[0252] The optical member obtained by the production method of the present invention is preferably used as various semiconductor optical members such as light conversion members and light emitting members used in display devices described below, because high brightness and a wide color reproduction range can be achieved.
[0253] An example of the method for producing the optical member of the present invention will be described below using the drawings.
[0254] Figure 1 This is a diagram for explaining an example of a method for manufacturing an optical member of the present invention. Figure 1 In the method shown, first, Figure 1 As shown in (A), a substrate 1 of an optical component is prepared. The substrate is not particularly limited as long as it is a substrate conventionally used for optical components, and examples thereof include a transparent substrate, a thin film transistor (TFT) substrate, etc. As the transparent substrate, for example, a non-flexible transparent hard material such as quartz glass, Pyrex (registered trademark) glass, and a synthetic quartz plate, or a flexible transparent flexible material such as a transparent resin film and an optical resin plate can be used.
[0255] The substrate may be a substrate subjected to surface treatment for the purpose of imparting gas barrier properties or the like, as necessary.
[0256] Then, if Figure 1 As shown in FIG. 2B , partition walls 2 are formed in the region that becomes the boundary between sub-pixels on one side of the substrate 1. The partition walls 2 can be formed to a thickness of 100 mm by sputtering, vacuum deposition, or the like. A metal thin film of chromium or the like is formed by patterning the thin film. As the patterning method, a common patterning method such as sputtering can be used.
[0257] In addition, as the partition wall 2, it can also be a layer containing light-shielding particles such as carbon particles, metal oxides, inorganic pigments, and organic pigments in a resin adhesive, for example, a black matrix can be used. As the resin adhesive used for the partition wall, one or more adhesives mixed with resins such as polyimide resins, acrylic resins, epoxy resins, polyacrylamide, polyvinyl alcohol, gelatin, casein, cellulose, etc., or photosensitive resins, and then O / W latex-type resin compositions, such as reactive silicone latex-formed adhesives, etc. can be used. As the thickness of such a resin partition wall, it can be set within the range of 0.5 to 15 μm. As the patterning method of such a resin partition wall, a method commonly used such as photolithography and printing can be used to form a specified pattern, and a method such as ionizing radiation irradiation is used to cure it, and a method of baking as needed.
[0258] The partition walls 2 may or may not have ink repellency, but preferably have ink repellency when not having the ink repellent projections 3 described below. The ink repellency can be imparted by the same method as that for the ink repellent projections 3 described below.
[0259] The height of the partition walls is not particularly limited, but is preferably 1.0 μm or more, more preferably 2.0 μm or more, from the perspective of color mixing (blocking of oblique light). On the other hand, from the perspective of productivity of the partition walls, it is preferably 15 μm or less, more preferably 10 μm or less.
[0260] You can also Figure 1 (C) As shown, an ink-repellent convex portion 3 is formed on the pattern of the partition wall 2. The composition of such an ink-repellent convex portion is not particularly limited as long as it is a resin composition with ink-repellent properties that has a low affinity with the quantum dot curable composition of the present invention and repels the quantum dot curable composition. In addition, it is not particularly required to be transparent, and it can also be colored. For example, a material used for the partition wall and not mixed with a black material can be used. Specifically, a composition obtained by mixing one or more of an aqueous resin such as polyacrylamide, polyvinyl alcohol, gelatin, casein, cellulose, an O / W latex-type resin composition, such as a composition obtained by latexing a reactive silicone, etc. can be cited. In the present invention, a photocurable resin can be preferably used for reasons such as operability and easy curing. In addition, the stronger the ink-repellent property of the ink-repellent convex portion, the more preferred it is, so its surface can also be treated with an ink-repellent treatment agent such as a silicone compound or a fluorine-containing compound.
[0261] The patterning of the ink-repellent convex portion can be performed by printing a coating liquid of the ink-repellent resin composition or by photolithography using a photocurable coating liquid. As described above, the height of the ink-repellent convex portion is provided to prevent the ink from mixing when the ink is coated by the inkjet method, so it can be adjusted appropriately. Specifically, it varies depending on the deposition amount of the blown ink, and is generally preferably within the range of 0.1 to 3.0 μm.
[0262] In addition, in the formation of the ink-repellent convex portion, surface treatments such as plasma treatment can also be used to impart ink-repellent properties. As surface treatments, for example, reduced pressure plasma treatment or atmospheric pressure plasma treatment in which a gas containing fluorine or a fluorine compound is used in the introduced gas and plasma irradiation is performed under a reduced pressure environment or an atmospheric pressure environment. If plasma treatment is performed in a gas containing a fluorine-based compound and oxygen, a phenomenon in which the fluorine-based compound enters the surface of the organic material occurs in parallel with the above-mentioned reaction in the organic material. Especially in the case where the fluorine-based compound is more than oxygen, for example, in a gas environment where the amount of the fluorine-based compound is too much such that the content of the fluorine-based compound relative to the total amount of the fluorine-based compound and oxygen is set to 60% or more, the fluorine-based compound mixing phenomenon is stronger than the oxidation reaction caused by oxygen, and therefore the surface of the organic material is non-polarized by the mixing phenomenon, thereby imparting ink-repellent properties.
[0263] exist Figure 1 Although not shown in the figure, after forming the partition wall 2 and the ink-repellent convex portion 3 as required, a functional layer for imparting various functions (for example, the following) may be formed as required on the surface of the substrate 1 in each quantum dot layer forming region 4 divided by the pattern of the partition wall 2. Figure 2 The functional layer 8) can be made into a layer that blocks or diffuses the desired light in the light from the light source or external light, or a layer that imparts these two properties, for example, by appropriately selecting the type and content of colorants or light scattering particles.
[0264] It should be noted that although the functional layer is not shown, it can also be provided on the quantum dot-containing solidified layer after the quantum dot-containing solidified layer is formed. Examples of the functional layer provided on the quantum dot-containing solidified layer include a gas barrier layer and the like.
[0265] The functional layer can be formed by appropriately selecting materials and forming methods according to the function. The functional layer can be obtained, for example, by forming a coating film of a resin composition containing a resin and, if necessary, a colorant, light scattering particles, etc., by a known method such as photolithography or inkjet, and curing the coating film.
[0266] Next, as ink for forming each sub-pixel, the above-mentioned quantum dot-containing composition of the present invention is prepared as inkjet ink of various colors. Figure 1As shown in (D), on the surface of the substrate 1, in each quantum dot layer forming area 4 divided by the pattern of the partition wall 2, the sub-pixel forming ink of the desired color is blown by the inkjet method to form a quantum dot layer. In the blowing process of the ink, the viscosity of the sub-pixel forming ink is not easy to increase at the front end of the discharge head 5, and good discharge performance can be continuously maintained. Therefore, the ink of the corresponding color can be accurately and evenly attached to the specified quantum dot layer forming area. In addition, when the second solvent has a specified surface tension and viscosity, it can be wetted and diffused to each corner to form sub-pixels without color unevenness or fading in a correct pattern. In addition, multiple inkjet heads can also be used to blow sub-pixel forming inks of various colors onto the substrate at the same time, so compared with the case of forming sub-pixels of various colors, the operating efficiency can be improved.
[0267] Then, if Figure 1 As shown in (E), after the quantum dot layer 6 of various colors is dried and pre-baked as needed, it is cured by appropriate exposure and / or heating. Among them, in the present invention, from the aspect of suppressing radial unevenness of the surface, it is preferred to further include a process of reducing pressure and drying the above-mentioned quantum dot layer before the usual pre-baking stage. For example, pre-baking is performed on a heating plate at 60 to 140°C for 3 to 20 minutes. In addition, heating and reduced pressure drying can also be performed simultaneously. Thereafter, if the quantum dot layer is appropriately exposed and / or heated, the cross-linking elements of the curable resin contained in the inkjet ink undergo a cross-linking reaction, and the quantum dot layer is cured to form a quantum dot cured layer 7.
[0268] It should be noted that the quantum dots contained in each quantum dot-containing solidified layer 7 may be of the same type or of different types.
[0269] It should be noted that the size of each sub-pixel is not particularly limited, and can be, for example, 5 μm×5 μm or more and 200 μm×200 μm or less. According to the manufacturing method of the present invention, a desired quantum dot content solidified layer can be accurately formed on such a small sub-pixel.
[0270] The thickness of the quantum dot-containing solidified layer can be set to about 0.01 μm to 10 μm, for example. The thickness of the solidified layer can be changed for each sub-pixel and set to an optimal thickness for each color.
[0271] In addition, in the present invention, in the manufactured optical component, the maximum value of the film thickness of the above-mentioned quantum dot-containing solidified layer, especially the maximum value of the film thickness at the end of the above-mentioned quantum dot-containing solidified layer is preferably less than 15μm, and more preferably less than 10μm. In addition, in the present invention, in the manufactured optical component, the maximum value of the film thickness of the above-mentioned quantum dot-containing solidified layer, especially the maximum value of the film thickness at the end of the above-mentioned quantum dot-containing solidified layer, and the difference between the average film thickness are preferably less than 5μm, and more preferably less than 2.5μm. In this case, the thick film portion becomes darker and display failures are reduced. It should be noted that the film thickness refers to the height from the substrate. In addition, the average film thickness of the solidified layer is calculated by dividing the coating volume in the sub-pixel by the area of the surface of the solidified layer. Furthermore, the so-called maximum value of the film thickness at the end refers to the value of the film thickness at the part with the highest film thickness in the end raised part.
[0272] In this manner, the optical member 101 is manufactured using the quantum dot-containing curable composition of the present invention.
[0273] In addition, the method for producing an optical member of the present invention may further include a step of forming an outer coating layer covering the partition walls 2 and the quantum dot-containing solidified layer 7. That is, the optical member obtained by the production method of the present invention is as follows: Figure 2 As shown, an outer coating layer 9 covering the partition walls 2 and the quantum dot-containing solidified layer 7 may also be provided.
[0274] The outer coating is used to flatten the optical component and prevent the components contained in the sub-pixel from dissolving or oxygen and water from penetrating. The thickness of the outer coating can be set in consideration of the transmittance of the material used, the surface state of the optical component, etc., and can be set, for example, in the range of 0.01 to 2.0 μm. The outer coating can be formed by using materials having the required transmittance and gas barrier properties as a protective layer, such as organic materials such as known photosensitive resins, two-liquid curing resins, metal oxides such as silicon oxide, aluminum oxide, tantalum oxide, yttrium oxide, hafnium oxide, zirconium oxide, titanium oxide, metal nitride oxides such as silicon nitride, metal alkoxides, silicon oxynitride, hafnium aluminate, and organic-inorganic hybrid materials. In addition, the method for forming the outer coating is appropriately selected from known methods according to the material used, and is not particularly limited. When using the above-mentioned inorganic materials, organic-inorganic hybrid materials, etc., for example, sol-gel method, evaporation method, sputtering method, etc. can be cited.
[0275] In the manufacturing method of the optical component of the present invention, before the process of forming the above-mentioned quantum dot layer, it further includes a process of selectively changing the wettability in a specified area of the above-mentioned substrate surface to form a quantum dot layer forming area having higher affinity with the above-mentioned quantum dot curable composition than the surrounding area. In the process of forming the above-mentioned quantum dot layer, a method of selectively attaching the above-mentioned quantum dot curable composition to the above-mentioned quantum dot layer forming area by inkjet method can be preferably used to form the above-mentioned quantum dot layer.
[0276] This is because if the ink is attached to the region where the quantum dot layer is formed, which has a higher affinity with the quantum dot curing composition, that is, has a greater affinity for ink, the wettability and diffusivity of the ink will be further improved, and fading and uneven film thickness can be more effectively prevented, thereby obtaining sub-pixels that do not produce bright spots or uneven colors.
[0277] As a process for selectively changing the wettability in a specified area of the substrate surface to form a region of quantum dot layer formation having a greater affinity for ink than the surrounding area, there is no particular limitation, and surface treatments such as plasma treatment as described above may also be used. For example, if plasma treatment is performed in a gas containing a fluorine-based compound and oxygen, unreacted groups are generated on the surface of the inorganic material by plasma discharge, and the unreacted groups are oxidized by oxygen to produce polar groups such as carbonyl or hydroxyl groups, thereby imparting affinity for ink. On the other hand, in organic materials, the phenomenon of fluorine-based compounds entering the surface of the organic material occurs in parallel with the above-mentioned reaction. Especially in the case where there is more fluorine-based compound than oxygen, for example, in a gas environment where the amount of fluorine-based compound is too much such as setting the content of fluorine-based compound relative to the total amount of fluorine-based compound and oxygen to more than 60%, the phenomenon of fluorine-based compound mixing becomes stronger than the oxidation reaction caused by oxygen, so the surface of the organic material is non-polarized by the mixing phenomenon, thereby imparting ink repellency. Therefore, if after forming the partition wall 2 or the convex portion on the glass substrate by an organic material, a plasma treatment is performed under the condition of excessive fluorine compounds as described above, the ink affinity becomes larger on the glass substrate corresponding to the region where the quantum dot layer is formed than the surrounding, the partition wall 2 and the convex portion become ink-repellent, and the convex portion becomes ink-repellent convex portion 3. For the region where the quantum dot layer is formed thus obtained, the ink is easily wetted and diffused, fading or uneven film thickness can be prevented, and the ink outflow from the convex portion corresponding to the boundary with other ink forming regions can be prevented. In addition, in this case, if the partition wall 2 is formed by an inorganic material and the convex portion is formed thereon by an organic material, the ink affinity of the glass substrate and the partition wall 2 becomes larger, and the convex portion becomes ink-repellent.
[0278] IV. Manufacturing Method of Display Device
[0279] The manufacturing method of the display device of the present invention is characterized by comprising the following steps:
[0280] a step of manufacturing an optical member by the method for manufacturing an optical member of the present invention; and
[0281] A step of mounting the optical member manufactured as described above.
[0282] As a display device manufactured by the manufacturing method of the display device of the present invention, as long as it is a display device having an optical component manufactured by the manufacturing method of the optical component of the present invention, its structure is not particularly limited, and it can be appropriately selected from conventionally known display devices, such as micro LED display devices, quantum dot light-emitting display devices, liquid crystal display devices, organic light-emitting display devices, etc. From the aspect of achieving high brightness and a wide color reproduction area, the manufacturing method of the present invention is particularly preferably a manufacturing method for micro LED display devices and quantum dot light-emitting display devices.
[0283] <Micro LED display devices>
[0284] When a micro LED display device is manufactured by the display device manufacturing method of the present invention, the step of mounting the above-manufactured optical component can be set as, for example, a step of assembling the above-manufactured optical component and a counter substrate including a micro LED substrate facing each other.
[0285] A micro LED display device obtained by the manufacturing method of the present invention will be described with reference to the drawings. Figure 2 1 is a schematic diagram showing an example of a display device obtained by the manufacturing method of the present invention, and is a schematic diagram showing an example of a micro LED display device. Figure 2 As illustrated, the micro-LED display device 200 has a structure in which the optical component (light conversion component) 100 of the present invention described above is bonded to an opposing substrate 11 having a micro-LED substrate. The optical component 100 of the micro-LED display device 200 has an outer coating 9, and the surface of the outer coating 9 side of the optical component 100 is assembled in an opposing manner to the opposing substrate 11. In addition, the optical component 100 of the micro-LED display device 200 has sub-pixels 10R, 10G, and 10B adjusted to red, green, or blue. The sub-pixel 10R adjusted to red has a quantum dot-containing solidified layer 7R containing quantum dots that display a red luminescent color, and a functional layer 8 for blocking blue light is provided between the substrate 1 and the quantum dot-containing solidified layer 7R. The sub-pixel 10G adjusted to green has a quantum dot-containing solidified layer 7G containing quantum dots that display a green luminescent color, and a functional layer 8 for blocking blue light is provided between the substrate 1 and the quantum dot-containing solidified layer 7G. The sub-pixel 10B adjusted to blue does not have a quantum dot-containing solidified layer, but has a functional layer 8 .
[0286] It should be noted that the micro LED display device obtained by the manufacturing method of the present invention is not limited to Figure 2 The structure shown can be generally set as a well-known structure of a micro LED display device using a semiconductor optical component (light conversion component).
[0287] In addition, the counter substrate can be appropriately selected and used according to the driving method of the micro LED display device of the present invention.
[0288] In addition, the micro LED display device obtained by the manufacturing method of the present invention is not limited to having Figure 2 The configuration shown may include, for example, a display device having a known configuration described in Japanese Patent Publication No. 2016-523450 and Japanese Patent Publication No. 2016-533030.
[0289] <Quantum dot light-emitting display device>
[0290] When a quantum dot light-emitting display device is manufactured by the manufacturing method of the display device of the present invention, a TFT substrate can be used as a substrate for manufacturing the above-mentioned optical component, and the process of mounting the above-mentioned optical component can be set to, for example, a process of assembling the light-emitting body including the above-mentioned optical component and the color filter opposite to each other.
[0291] The quantum dot light-emitting display device obtained by the manufacturing method of the present invention will be described with reference to the drawings. Figure 3 1 is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention, and is a schematic diagram showing an example of a quantum dot light-emitting display device. Figure 3 As shown in the example, the quantum dot light-emitting display device 300 includes a color filter 40 and a light-emitting body 80 including an optical member 74 of the present invention. An organic protective layer 50 and an inorganic oxide film 60 may be provided between the color filter 40 and the light-emitting body 80.
[0292] As a stacking method of the light-emitting body 80, for example, a method of sequentially forming a transparent anode 71, a hole injection layer 72, a hole transport layer 73, an optical component 74 of the present invention, an electron injection layer 75, and a cathode 76 on the upper surface of the color filter 40, or a method of bonding the light-emitting body 80 formed on another substrate to the inorganic oxide film 60, etc. The transparent anode 71, the hole injection layer 72, the hole transport layer 73, the electron injection layer 75, and the cathode 76 in the light-emitting body 80, and other structures can appropriately use known structures. The quantum dot light-emitting display device 300 manufactured in the above manner can also be applied to, for example, a quantum dot light-emitting diode (QLED) display of a passive drive mode or a QLED display of an active drive mode.
[0293] <Liquid Crystal Display Device>
[0294] When a liquid crystal display device is manufactured by the method for manufacturing a display device of the present invention, the step of mounting the manufactured optical member may be set as a step of assembling the manufactured optical member and a liquid crystal driving substrate facing each other, for example.
[0295] A liquid crystal display device obtained by the manufacturing method of the present invention will be described with reference to the drawings. Figure 4 1 is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention, and is a schematic diagram showing an example of a liquid crystal display device. Figure 4 As shown, the liquid crystal display device 400 has an optical component (light conversion component) 100, and a liquid crystal driving substrate having a liquid crystal layer 13 on one side of an opposing substrate 12 having a TFT array substrate, and has a liquid crystal layer 13 between the above-mentioned optical component (light conversion component) 100 and the above-mentioned opposing substrate 12.
[0296] It should be noted that the liquid crystal display device of the present invention is not limited to the Figure 4 The structure shown can be generally set as a well-known structure as a liquid crystal display device using a semiconductor optical member (light conversion member).
[0297] The driving method of the liquid crystal display device of the present invention is not particularly limited, and a driving method commonly used for liquid crystal display devices can be adopted. As such a driving method, for example, a TN (twisted nematic) method, an IPS (in-plane switching) method, an OCB (optically compensated bend) method, and an MVA (multi-domain vertical alignment) method can be cited. In the present invention, any of these methods can be preferably used.
[0298] In addition, the counter substrate can be appropriately selected and used according to the driving method of the liquid crystal display device of the present invention.
[0299] As a method for forming the liquid crystal layer, a method generally used as a method for producing a liquid crystal cell can be used, and examples thereof include a vacuum injection method and a liquid crystal dropping method.
[0300] <Organic light emitting display device>
[0301] When an organic light-emitting display device is manufactured by the display device manufacturing method of the present invention, the process of mounting the above-mentioned optical component can be set as, for example, a process of preparing an organic light-emitting body including the above-mentioned optical component, and a process of assembling the above-mentioned organic light-emitting body and the color filter opposite to each other.
[0302] The organic light-emitting display device obtained by the method for manufacturing a display device of the present invention has an organic light-emitting body including the optical member (light-emitting member) of the present invention described above.
[0303] Such an organic light emitting display device of the present invention will be described with reference to the drawings. Figure 5 1 is a schematic diagram showing another example of a display device obtained by the manufacturing method of the present invention, and is a schematic diagram showing an example of an organic light emitting display device. Figure 5 As shown, the organic light-emitting display device 500 has a color filter 40 and an organic light-emitting body 81 including an optical component (light-emitting component) 74' of the present invention. An organic protective layer 50 and an inorganic oxide film 60 may also be provided between the color filter 40 and the organic light-emitting body 81. In addition, the optical component (light-emitting component) of the present invention used in the organic light-emitting display device can be made into an optical component having a sub-pixel having a solidified layer containing quantum dots and a sub-pixel having a light-emitting layer containing an organic light-emitting compound. As the organic light-emitting compound, an organic light-emitting compound used in the light-emitting layer of a known organic light-emitting display device can be used.
[0304] As a stacking method of the organic light emitting body 81, for example, a method of sequentially forming a transparent anode 71, a hole injection layer 72, a hole transport layer 73, an optical component (light emitting component) 74' of the present invention which may have a light emitting layer containing an organic light emitting compound, an electron injection layer 75, and a cathode 76 on the upper surface of a color filter, or a method of bonding an organic light emitting body 180 formed on another substrate to an inorganic oxide film 60, etc. The transparent anode 71, the hole injection layer 72, the hole transport layer 73, the electron injection layer 75, and the cathode 76 in the organic light emitting body 81, and other structures can appropriately use known structures. The organic light emitting display device 500 manufactured in the above manner can be applied to, for example, a passively driven organic electroluminescence (EL) display and an actively driven organic EL display.
[0305] It should be noted that the organic light emitting display device of the present invention is not limited to the Figure 5 The structure shown can be a well-known structure of a general organic light emitting display device.
[0306] Example
[0307] The present invention will be described in detail below with reference to Examples, but the present invention is not limited to these descriptions.
[0308] The weight average molecular weight was measured by Shodex GPC System-21H using polystyrene as a standard substance and THF as an eluent. The acid value was measured in accordance with JIS K0070.
[0309] (Production Example 1-1: Synthesis of Epoxy Group-Containing Copolymer A)
[0310] In a four-necked flask equipped with a thermometer, a reflux condenser, a stirrer, and a dropping funnel, 40.7 parts by mass of propylene glycol monomethyl ether acetate (hereinafter, sometimes referred to as PGMEA) was added according to the mixing ratio shown in Table 1, and the mixture was heated to 140°C while stirring. Then, 54.7 parts by mass of a mixture of monomers and polymerization initiators (dropping components) of the composition described in Table 1 were dripped at a constant rate for 2 hours through a dropping funnel at a temperature of 140°C. After the dripping was completed, the temperature was lowered to 110°C and 4.6 parts by mass of a mixture of polymerization initiator and PGMEA (additional catalyst component) were added. When the temperature of 110°C was maintained for 2 hours, 37.5 parts by mass of PGMEA was added and the reaction was terminated, thereby obtaining an epoxy-containing copolymer A having the characteristics described in Table 1.
[0311] (Production Example 1-2: Synthesis of Epoxy Group-Containing Copolymer B)
[0312] In the above Production Example 1-1, except that diethylene glycol monobutyl ether acetate (also known as butyl carbitol acetate, hereinafter sometimes referred to as BCA) was used instead of PGMEA, the epoxy group-containing copolymer B having the properties described in Table 1 was obtained in the same manner as in the above Production Example 1-1.
[0313] [Table 1]
[0314] Table 1
[0315]
[0316] It should be noted that the abbreviations in the table are as follows.
[0317] PGMEA: Propylene glycol monomethyl ether acetate (boiling point: 146°C)
[0318] BCA: Diethylene glycol monobutyl ether acetate (boiling point: 247°C)
[0319] GMA: Glycidyl Methacrylate
[0320] CHMA: Cyclohexyl methacrylate
[0321] PERBUTYL O: tert-butyl peroxy(2-ethylhexanoate) (trade name manufactured by NOF Corporation)
[0322] (Production Example 2-1: Synthesis of Adhesive Acrylic Resin A)
[0323] A mixed solution of 30 parts by mass of cyclohexyl methacrylate (CHMA), 25 parts by mass of 2-hydroxyethyl methacrylate (HEMA), 25 parts by mass of tert-butyl methacrylate (t-BMA), and 20 parts by mass of methyl methacrylate (MMA) was prepared. 2 parts by mass of PERBUTYL O and 10 parts by mass of n-dodecyl mercaptan were added to the mixed solution, and the mixture was added dropwise to a polymerization tank to which 168 parts by mass of BCA were added at 100° C. for 3 hours under a nitrogen stream. After the addition was completed, the mixture was further heated at 100° C. for 3 hours to obtain a polymer solution containing an adhesive acrylic resin A as a polymer. The solid content in the polymer solution was 40% by mass, and the weight average molecular weight of the adhesive acrylic resin A was 13000.
[0324] (Production Example 3-1: Synthesis of Adhesive Acrylic Resin B)
[0325] A mixed solution of 48 parts by mass of cyclohexyl methacrylate (CHMA), 20 parts by mass of methyl methacrylate (MMA), 12 parts by mass of methacrylic acid (MAA), and 3 parts by mass of azobisisobutyronitrile (AIBN) was added dropwise to a polymerization tank to which 155 parts by mass of BCA was added under a nitrogen flow at 100° C. for 3 hours. After the addition was completed, the mixture was further heated at 100° C. for 3 hours to obtain a polymer solution. The mass average molecular weight of the polymer solution was 7000.
[0326] Next, 200 parts by mass of glycidyl methacrylate (GMA), 0.2 parts by mass of triethylamine, and 0.05 parts by mass of p-methoxyphenol were added to the obtained polymer solution, and the mixture was heated at 110° C. for 10 hours. Air was bubbled into the reaction solution to obtain a binder acrylic resin B solution. The obtained binder acrylic resin B is a resin obtained by introducing a side chain having an olefinic double bond into a main chain formed by copolymerization of CHMA, MMA, and MAA using GMA. The solid content of the binder acrylic resin B solution is 40% by mass, and the acid value is 3 mgKOH / g. In addition, the weight average molecular weight of the binder acrylic resin B is 12,000.
[0327] (Production Example 4-1: Synthesis of Adhesive Acrylic Resin C)
[0328] In the synthesis of the adhesive acrylic resin B of Manufacturing Example 3-1, except that CHMA was set to 40 parts by mass, MMA was set to 15 parts by mass, and MAA was set to 25 parts by mass, an adhesive acrylic resin C solution was obtained in the same manner. The obtained adhesive acrylic resin C is a resin in which a side chain having an olefinic double bond is introduced into a main chain formed by copolymerization of CHMA, MMA, and MAA using GMA, and the solid content of the adhesive acrylic resin C is 40% by mass and the acid value is 74 mgKOH / g. In addition, the weight average molecular weight of the adhesive acrylic resin C is 12500.
[0329] (Production Example 5-1: Synthesis of Adhesive Acrylic Resin D)
[0330] A mixed solution of 64 parts by mass of styrene, 6 parts by mass of methacrylic acid (MAA), and 3 parts by mass of azobisisobutyronitrile (AIBN) was added dropwise to a polymerization tank to which 125 parts by mass of BCA was added under a nitrogen flow at 100° C. for 3 hours. After the addition was completed, the mixture was further heated at 100° C. for 3 hours to obtain a polymer solution. The weight average molecular weight of the polymer solution was 7,000.
[0331] Next, 10 parts by mass of glycidyl methacrylate (GMA), 0.2 parts by mass of triethylamine, and 0.05 parts by mass of p-methoxyphenol were added to the obtained polymer solution, and the mixture was heated at 110° C. for 10 hours, and air was bubbled into the reaction solution to obtain a binder acrylic resin D solution. The obtained binder acrylic resin D is a resin obtained by introducing a side chain having an olefinic double bond into a main chain formed by copolymerization of styrene and MAA using GMA, and the solid content of the binder acrylic resin D solution is 40% by mass. In addition, the weight average molecular weight of the binder acrylic resin D is 10,000.
[0332] (Production Example 6-1: Synthesis of Adhesive Acrylic Resin E)
[0333] In the manufacture of the adhesive acrylic resin B of Manufacturing Example 3-1, CHMA was set to 34 parts by mass, MMA was set to 22 parts by mass, MAA was set to 22 parts by mass, and glycidyl methacrylate (GMA) was set to 22 parts by mass, and an adhesive acrylic resin E solution was obtained in the same manner. The obtained adhesive acrylic resin E is a resin in which a side chain having an olefinic double bond is introduced into a main chain formed by copolymerization of CHMA, MMA, and MAA using GMA, and the solid content of the adhesive acrylic resin E is 40% by mass and the acid value is 64 mgKOH / g. In addition, the weight average molecular weight of the adhesive acrylic resin E is 8700.
[0334] (Production Example 7-1: Synthesis of Adhesive Acrylic Resin F)
[0335] In the manufacture of the adhesive acrylic resin A of Manufacturing Example 2-1, a polymer solution containing an adhesive acrylic resin F as a polymer was obtained in the same manner except that 30 parts by mass of CHMA, 25 parts by mass of HEMA, 25 parts by mass of t-BMA, 8.7 parts by mass of MMA, and 11.3 parts by mass of methacrylic acid (MAA) were used. The solid content in the polymer solution was 40% by mass, and the acid value was 74 mgKOH / g. In addition, the weight average molecular weight of the adhesive acrylic resin F was 13,000.
[0336] (Production Example 8-1: Synthesis of Adhesive Acrylic Resin G)
[0337] In the manufacture of the adhesive acrylic resin A of Manufacturing Example 2-1, 9 parts by mass of CHMA, 21 parts by mass of dimethylaminoethyl methacrylate (DMMA), 25 parts by mass of HEMA, 25 parts by mass of t-BMA, and 20 parts by mass of MMA were used. A polymer solution containing an adhesive acrylic resin G as a polymer was obtained in the same manner. The solid content in the polymer solution was 40% by mass, and the amine value was 75 mgKOH / g. In addition, the weight average molecular weight of the adhesive acrylic resin G was 13,000.
[0338] (Production Examples 2-2 to 8-2: Synthesis of Adhesive Acrylic Resins H to N)
[0339] In the above-mentioned Production Examples 2-1 to 8-1, except having used PGMEA instead of BCA, it carried out similarly to the above-mentioned Production Examples 2-1 to 8-1, and obtained the adhesive acrylic resin H to N which have the characteristics described in Table 7.
[0340] (Production Example 9-1: Synthesis of Blocked Carboxylic Acid Curing Agent A)
[0341] In a four-necked flask equipped with a thermometer, a reflux condenser and a stirrer, each component was added according to the mixing ratio shown in Table 2, and the temperature was raised to 70° C. while stirring. Then, the temperature was maintained while stirring was continued, and the reaction was terminated when the acid value of the mixture became 3.0 mgKOH / g or less, thereby obtaining a blocked carboxylic acid curing agent A having the characteristics described in Table 2.
[0342] (Production Example 9-2: Synthesis of Blocked Carboxylic Acid Curing Agent B)
[0343] In the above Production Example 9-1, except that BCA was used instead of PGMEA, a blocked carboxylic acid curing agent B having the properties described in Table 2 was obtained in the same manner as in the above Production Example 9-1.
[0344] [Table 2]
[0345] Table 2
[0346]
[0347] (Example 1)
[0348] (1) Preparation of adhesive composition
[0349] A Teflon (registered trademark)-coated rotor was added to a sample bottle and placed on a magnetic stirrer. The epoxy-containing copolymer A and the multifunctional epoxy resin described in the above-mentioned manufacturing example 1-1 were added to the sample bottle according to the following ratios, and fully stirred and dissolved at room temperature. Then, a diluent was added in such a way that the solid content became 40% by mass in order to adjust the viscosity, and stirred and dissolved, and then filtered to obtain an adhesive composition.
[0350] [Blending ratio of adhesive composition]
[0351] · Epoxy-group-containing copolymer A of Production Example 1-1 (solid content in PGMEA: 40% by mass): 75 parts by mass
[0352] · Multifunctional epoxy resin (trade name jER154, manufactured by Mitsubishi Chemical Corporation): 20 parts by mass
[0353] Neopentyl glycol glycidyl ether: 10 parts by mass
[0354] Blocked carboxylic acid curing agent A of Production Example 9-1 (solid content in PGMEA: 70.8% by mass): 42 parts by mass
[0355] Dilution solvent (PGMEA): 77.3 parts by mass
[0356] (2) Preparation of Quantum-Containing Curable Composition
[0357] 0.2 parts by mass of quantum dots (748056-25MG manufactured by Merck), 49.51 parts by mass of the adhesive composition obtained above, and 50.29 parts by mass of the first solvent BCA were fully mixed to obtain a quantum dot-containing curable composition of Example 1 having the mixing ratio shown in Table 3.
[0358] (3) Fabrication of optical components
[0359] A black matrix pattern having a line width of 20 μm and a film thickness of 5.0 μm was formed by photolithography using the curable resin composition for black matrices on a 0.7 mm thick, 10 cm×10 cm glass substrate (manufactured by Asahi Glass Co., Ltd.).
[0360] The obtained quantum dot-containing curable composition was attached to the area formed by the black matrix on the substrate by an inkjet method.
[0361] Thereafter, the film was dried under reduced pressure at 10 Torr for 120 seconds, and then pre-baked on a hot plate at 80° C. for 10 minutes. Thereafter, the film was post-baked at 200° C. for 30 minutes in a dust-free oven, and then further at 230° C. for 30 minutes, thereby forming a quantum dot-containing cured layer (quantum dot-containing cured product) having an average film thickness of 2.0 μm after drying and curing on the substrate, thereby obtaining an optical component.
[0362] (Examples 2 to 6 and Comparative Examples 1 to 2, 4)
[0363] In the preparation of the quantum dot curable composition (2) of Example 1, each solvent shown in Table 3 was used instead of BCA in such a manner that the solvent in the quantum dot curable composition was formulated as shown in Table 3. Otherwise, the quantum dot curable compositions and optical components of Examples 2 to 6 and Comparative Examples 1 to 2 and 4 were obtained in the same manner as in Example 1.
[0364] (Examples 7 and 8)
[0365] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed in a manner such that the composition is as shown in Table 3, and a mixed solvent of PGMEA and BCA is used instead of PGMEA as the diluent solvent used in the adhesive composition in a manner such that the solvent in the quantum dot curing composition is as shown in Table 3. Otherwise, the quantum dot curing compositions and optical components of Examples 7 and 8 are obtained in the same manner as in Example 1.
[0366] (Comparative Example 3)
[0367] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed to be the same as the composition of the adhesive component of Example 7, and BCA is used instead of PGMEA as the diluent solvent used in the adhesive composition. Otherwise, the quantum dot-curable composition and optical component of Comparative Example 3 are obtained in the same manner as Example 1.
[0368] (Comparative Example 5)
[0369] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed to be the same as the composition of the adhesive component of Example 7, and BCA is used instead of PGMEA as the diluent solvent used in the adhesive composition. In the preparation of the (2) quantum dot-containing curable composition of Example 1, ethyl acetate is used instead of BCA. Otherwise, the quantum dot-containing curable composition and optical component of Comparative Example 5 are obtained in the same manner as in Example 1.
[0370] (Examples 9 to 11)
[0371] In the preparation of the quantum dot curable composition (2) of Example 1, a mixed solvent of PGMEA and BCA was used instead of BCA in such a manner that the solvent in the quantum dot curable composition was formulated as shown in Table 3. Otherwise, the quantum dot curable compositions and optical components of Examples 9 to 11 were obtained in the same manner as in Example 1.
[0372] (Example 12)
[0373] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed in a manner that is the same as the composition of the adhesive component of Example 7, and a mixed solvent of PGMEA and BCA is used instead of PGMEA as a dilution solvent in a manner that the solvent in the quantum dot curable composition is formulated as shown in Table 3. Otherwise, the quantum dot curable composition and optical component of Example 12 are obtained in the same manner as Example 1.
[0374] (Examples 13 to 16)
[0375] In the preparation of the adhesive composition (1) of Example 1, the composition of the adhesive component is changed to the composition shown in Table 4. In the preparation of the optical component (3) of Example 1, the method for forming the quantum dot-containing cured layer (quantum dot-containing curable composition) is changed to the following method. Otherwise, the quantum dot-containing curable compositions and optical components of Examples 13 to 16 are obtained in the same manner as in Example 1.
[0376] <Production of Optical Members in Examples 13 to 16>
[0377] A black matrix pattern having a line width of 20 μm and a film thickness of 5.0 μm was formed by photolithography using the curable resin composition for black matrices on a 0.7 mm thick, 10 cm×10 cm glass substrate (manufactured by Asahi Glass Co., Ltd.).
[0378] The obtained quantum dot-containing curable composition was attached to the area formed by the black matrix on the substrate by an inkjet method.
[0379] Thereafter, the film was dried under reduced pressure at 10 Torr for 120 seconds, and further pre-baked on a hot plate at 80° C. for 10 minutes. Thereafter, a conveyor-type UV irradiator (manufactured by GS Yuasa) was used to irradiate the film at 1000 mJ / cm at a conveying speed of 1000 mm / min using a high-power low-pressure mercury lamp. 2The irradiation is performed, and then the film is post-baked by heating at 200°C for 30 minutes in a dust-free oven, and further post-baked by heating at 230°C for 30 minutes, thereby forming a quantum dot-containing cured layer (quantum dot-containing cured product) with an average film thickness of 2.0 μm after drying and curing on the substrate to obtain an optical component.
[0380] (Examples 17 to 19, 24, 29)
[0381] In the preparation of (1) the adhesive composition of Example 1, the composition of the adhesive component is changed in such a manner that the composition becomes the composition shown in Table 4. In the preparation of (2) the quantum dot curing composition of Example 1, the various materials and their combinations are changed in such a manner that the composition of the quantum dot curing composition becomes the composition shown in Table 4. Otherwise, the quantum dot curing compositions and optical components of Examples 17 to 19, 24, and 29 are obtained in the same manner as in Example 1.
[0382] (Examples 20 to 23, 25 to 28, 30 to 33)
[0383] In the preparation of the adhesive composition (1) of Example 1, the composition of the adhesive component is changed in such a way that the composition becomes the composition shown in Table 4. In the preparation of the quantum dot curable composition (2) of Example 1, the materials and their combinations are changed in such a way that the composition of the quantum dot curable composition becomes the composition shown in Table 4. In the preparation of the optical component (3) of Example 1, the method for forming the quantum dot curing layer (quantum dot curable composition) is changed to the same method as Example 13. Otherwise, the quantum dot curable compositions and optical components of Examples 20 to 23, 25 to 28, and 30 to 33 are obtained in the same manner as Example 1.
[0384] (Examples 34 to 37)
[0385] In the preparation of the adhesive composition (1) of Example 1, the composition of the adhesive component was changed so that the composition was as shown in Table 5, and in the preparation of the quantum dot curable composition (2) of Example 1, each material and its combination were changed so that the composition of the quantum dot curable composition was as shown in Table 5. The quantum dot curable compositions and optical members of Examples 34 to 37 were obtained in the same manner as in Example 1. It should be noted that all MEK (methyl ethyl ketone) in Example 37 was contained in the urethane resin (Nipporane 5253).
[0386] (Examples 38 to 44)
[0387] In the preparation of the adhesive composition (1) of Example 1, the composition of the adhesive component is changed in such a way that the composition becomes the composition shown in Table 5. In the preparation of the quantum dot curable composition (2) of Example 1, the materials and their combinations are changed in such a way that the composition of the quantum dot curable composition becomes the composition shown in Table 5. In the preparation of the optical component (3) of Example 1, the method for forming the quantum dot curing layer (quantum dot curable composition) is changed to the same method as Example 13. Otherwise, the quantum dot curable compositions and optical components of Examples 38 to 44 are obtained in the same manner as Example 1.
[0388] (Example 45)
[0389] (1) Preparation of dispersion
[0390] 65 parts by mass of PGMEA and 33 parts by mass of acrylic block resin (trade name, BYK-LPN6919, amine value 120 mgKOH / g, BYK-Chemie Japan) (solid content 60%) were added to a 225 mL mayonnaise bottle and stirred. 2 parts by mass of quantum dots (748056-25MG manufactured by Merck) and 100 parts by mass of zirconia beads with a particle size of 2.0 mm were added thereto, and the mixture was shaken for 1 hour with a paint shaker (manufactured by Asada Iron Works Co., Ltd.) as preliminary crushing. Then, 200 parts of zirconia beads with a particle size of 0.1 mm were used and dispersed for 4 hours with a paint shaker as formal crushing to obtain a quantum dot dispersion.
[0391] (2) Preparation of Quantum-Containing Curable Composition
[0392] In the preparation of the adhesive composition (1) of Example 1, the adhesive composition was prepared in the same manner except that the composition of the adhesive component was changed to the composition shown in Table 5 except for the acrylic block resin. 10 parts by mass of the quantum dot dispersion, 4.95 parts by mass of the adhesive composition (solid content 40%) obtained above, 47.32 parts by mass of the first solvent BCA, 21.89 parts by mass of the second solvent PGMEA, 13.86 parts by mass of the multifunctional monomer DPHA, and 41.98 parts by mass of the photopolymerization initiator Irg 18 were fully mixed to obtain a quantum dot curable composition of Example 45 having the mixing ratio shown in Table 5.
[0393] (3) Fabrication of optical components
[0394] In the production of the optical element, the method for forming the quantum dot-containing cured layer (quantum dot-containing curable composition) was the same as that of Example 13, thereby obtaining an optical member of Example 45.
[0395] (Examples 46 to 49)
[0396] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed in such a manner that the composition becomes the composition shown in Table 6. Furthermore, in the preparation of the (2) quantum dot-containing curable composition of Example 1, ethyl 3-ethoxypropionate (EEP) is used instead of BCA in such a manner that the composition of the quantum dot-containing curable composition becomes the composition shown in Table 6. Except for this, the quantum dot-containing curable compositions of Examples 46 to 49 are obtained in the same manner as in Example 1.
[0397] Optical members were obtained in the same manner as in Example 1 except that the temperature of the post-bake was changed to 150°C using the obtained quantum dot-containing curable compositions.
[0398] (Examples 50 to 60)
[0399] In the preparation of the (1) adhesive composition of Example 1, the composition of the adhesive component is changed in such a manner that the composition becomes the composition shown in Table 6. Furthermore, in the preparation of the (2) quantum dot-containing curable composition of Example 1, EEP is changed in such a manner that the composition of the quantum dot-containing curable composition becomes the composition shown in Table 6 instead of BCA. Otherwise, the quantum dot-containing curable compositions of Examples 50 to 60 are obtained in the same manner as in Example 1.
[0400] In the production of the optical element, the method for forming the quantum dot-containing cured layer (quantum dot-containing curable composition) was the same as that of Example 13, thereby obtaining the optical members of Examples 50 to 60.
[0401] (Example 61)
[0402] In Example 45, except that BCA was replaced with EEP so as to have the composition shown in Table 6, a quantum dot-containing curable composition of Example 61 having the mixing ratio shown in Table 6 was obtained in the same manner as in Example 45.
[0403] In the production of the optical element, the method for forming the quantum dot-containing cured layer (quantum dot-containing curable composition) was the same as that of Example 13, thereby obtaining an optical member of Example 61.
[0404] [evaluate]
[0405] (1) Inkjet discharge performance
[0406] The inkjet discharge properties of the quantum dot-containing curable compositions of the respective Examples and Comparative Examples obtained above were evaluated by the following method. The evaluation results are shown in Tables 3 to 6.
[0407] The ink (a quantum dot curable composition) is filled in the inkjet head and discharged from the inkjet head. The ink is dripped with a droplet diameter of 30 μm to the center of the quantum dot curable layer forming area on the glass transparent substrate divided into a predetermined pattern by a partition wall. Then, after stopping the initial discharge and letting the inkjet head stand for 30 minutes, the ink is dripped from the same inkjet head with a droplet diameter of 30 μm to the center of another quantum dot curable layer forming area. In such intermittent discharge, the discharge property (initial discharge property) at the time of the initial discharge action and the discharge property (intermittent discharge stability) at the time of the subsequent re-discharge are observed and evaluated according to the following criteria.
[0408] [Evaluation criteria for initial discharge performance]
[0409] AA: Ink can be discharged from all holes of the inkjet head.
[0410] A: There are a small number of holes in the inkjet head from which ink cannot be discharged.
[0411] B: About half of the holes in the inkjet head cannot discharge ink.
[0412] C: Almost all holes of the inkjet head cannot discharge ink.
[0413] [Evaluation criteria for intermittent discharge stability]
[0414] AA: Ink can be discharged from all holes of the inkjet head.
[0415] A: There are a small number of holes in the inkjet head from which ink cannot be discharged.
[0416] B: About half of the holes in the inkjet head cannot discharge ink.
[0417] C: Almost all holes of the inkjet head cannot discharge ink.
[0418] (2) Uneven
[0419] The quantum dot-containing cured layer of the optical member obtained in each of the examples and comparative examples was photographed, and the unevenness was evaluated according to the following evaluation criteria. Figure 6 As shown, the Blue LED is arranged at a position (opposite position of the camera 20) where the imaging optical axis of the camera 20 passes through the imaging area of the optical component 100 and extends, and the entire surface of the optical component 100 is photographed by the camera 20 while the Blue LED is irradiated from the back side to the quantum dot-containing solidified layer. The camera 20 is tilted 70 to 80 degrees from the direction perpendicular to the substrate of the optical component for photographing. A Blue LED is used as a light source, and a monochrome line sensor camera is used as a camera. The evaluation results are shown in Tables 3 to 6.
[0420] [Uneven evaluation criteria]
[0421] AA: No unevenness at all
[0422] A: Mild unevenness is visible in some areas
[0423] B: Partially visible unevenness
[0424] C: Unevenness is visible on the entire surface
[0425] D: Obvious unevenness can be seen on the entire surface
[0426] (3) Quantum dot dispersion
[0427] The optical components of each embodiment and each comparative example obtained above were cut into slices with a width of 100 nm, and the cross-section containing the quantum dot solidified layer of the slice was observed at 50,000 times using a transmission electron microscope: TEM (transmission electron microscopy model Tecnai G2spirits, manufactured by FEI Company). The aggregation state of the quantum dots was observed in a field of view of 500 nm×500 nm, and evaluated according to the following evaluation criteria. The evaluation results are shown in Tables 3 to 6.
[0428] [Evaluation criteria for quantum dot dispersion]
[0429] AA: No aggregation observed
[0430] A: Slight condensation observed
[0431] B: Partial aggregation was observed
[0432] C: A large number of aggregates were observed
[0433]
[0434]
[0435]
[0436]
[0437]
[0438] In addition, in a table|surface, the numerical value of the content ratio (mass ratio) of each component other than a solvent shows the solid content conversion value.
[0439] In addition, the abbreviations in the table are as follows.
[0440] 748056-25MG: Quantum dots, manufactured by Merck
[0441] 776750-5ML: Quantum dot solution, manufactured by Merck
[0442] 790192-25MG: Quantum dots, manufactured by Merck
[0443] 776777-5ML: Quantum dot solution, manufactured by Merck
[0444] jER1001: Multifunctional epoxy resin, trade name, manufactured by Mitsubishi Chemical Corporation jER157S70: Multifunctional epoxy resin, trade name, manufactured by Mitsubishi Chemical Corporation
[0445] Nipporane 5253: Urethane resin, trade name, manufactured by Tosoh Corporation
[0446] Coronate L: isocyanate curing agent, trade name, manufactured by Tosoh Corporation
[0447] Vylon 200: Polyester resin, trade name, manufactured by Toyobo Co., Ltd.
[0448] Vylon 802: Polyester resin, trade name, manufactured by Toyobo Co., Ltd.
[0449] MALKYD No.1: Maleic acid resin, trade name, manufactured by Arakawa Chemical Co., Ltd.
[0450] MALKYD No.31: Maleic acid resin, trade name, manufactured by Arakawa Chemical Co., Ltd.
[0451] BYK6919: Acrylic block resin, trade name, BYK-LPN6919, BYK-Chemie Japan
[0452] DPPA: Dipentaerythritol pentaacrylate
[0453] Irg 184: 1-Hydroxy-cyclohexyl-phenyl-ketone, manufactured by BASF, Irgacure 184
[0454] BCA: Diethylene glycol monobutyl ether acetate
[0455] Solfit AC: 3-Methoxy-3-methylbutyl acetate
[0456] Solfit: 3-Methoxy-3-methyl-1-butanol
[0457] EEP: Ethyl 3-ethoxypropionate
[0458] PGMEA: Propylene glycol monomethyl ether acetate
[0459] MEK: Methyl Ethyl Ketone
[0460] [Results Summary]
[0461] According to the results shown in Tables 3 to 6, in Examples 1 to 61 using a mixed solvent containing a first solvent having a boiling point of greater than 165°C and less than 260°C and a second solvent having a boiling point of greater than 100°C and less than 165°C, the quantum dot-containing curable composition has excellent discharge stability in the inkjet method, so the aggregation of quantum dots in the formed quantum dot-containing cured layer is suppressed and the unevenness is reduced.
[0462] On the other hand, since only the second solvent was used as the solvent in Comparative Examples 1 and 2 without using the first solvent, the discharge stability in the inkjet method was poor, and aggregation and unevenness of quantum dots were observed in the cured layer.
[0463] In Comparative Example 3, since only the first solvent was used as the solvent without using the second solvent, aggregation and unevenness of quantum dots were observed in the solidified layer.
[0464] In Comparative Example 4, since a mixed solvent of the second solvent and a high boiling point solvent that does not correspond to either the first solvent or the second solvent was used, aggregation and unevenness of quantum dots were observed in the cured layer.
[0465] Since Comparative Example 5 used a mixed solvent of the first solvent and a low boiling point solvent that did not match either the first solvent or the second solvent, the ejection stability in the inkjet method was poor, and aggregation and unevenness of quantum dots were observed in the cured layer.
[0466] In addition, the comparison of Examples 1 to 6 shows that if one or more first solvents selected from diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, 3-methoxybutyl acetate and ethyl 3-ethoxypropionate are used as the first solvent, the dispersibility of the quantum dots is better; if one or more first solvents selected from diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate and 3-methoxybutyl acetate are used, the dispersibility of the quantum dots is further improved.
[0467] In addition, the comparison of Examples 1, 9 to 11, and the comparison of Examples 7, 8, and 12 show that if the proportion of the first solvent in the total solvent is greater than 30 mass % and less than 80 mass %, and the proportion of the second solvent is greater than 20 mass % and less than 70 mass %, the dispersibility of the quantum dots is better and the unevenness is reduced.
[0468] In addition, according to Examples 13 to 16, even when a photocurable adhesive component is used, the discharge stability in the inkjet method is excellent, the dispersibility of the quantum dots is excellent, and the unevenness is reduced. Among them, in Example 13 using a thermal latent (meth) acrylic copolymer and Example 16 using a styrene-(meth) acrylic copolymer, the dispersibility of the quantum dots is excellent.
[0469] In addition, Examples 17 and 18 show that even when the quantum dot content in the quantum dot curable composition is increased, the ejection stability in the inkjet method is excellent, the dispersibility of the quantum dots is excellent, and the unevenness is reduced.
[0470] In addition, Examples 19 to 33 show that even when the type of quantum dots in the quantum dot-containing curable composition and the type of the second solvent are changed, the ejection stability in the inkjet method is excellent, the dispersibility of the quantum dots is excellent, and the unevenness is reduced.
[0471] In addition, Examples 34 to 61 show that even if the type of the binder component and the type of the first solvent in the quantum dot curable composition are changed to a solvent (EEP) with a lower boiling point and capable of post-baking at a low temperature, the discharge stability in the inkjet method is excellent, the dispersibility of the quantum dots is excellent, and the unevenness is reduced. If the binder component contains a polymer having an amine value, it can be seen that the dispersibility of the quantum dots tends to be better.
[0472] Description of Reference Numerals
[0473] 1 substrate
[0474] 2. Next door
[0475] 3 Ink-repellent convex parts
[0476] 4. Quantum dot layer formation area
[0477] 5 Inkjet Head
[0478] 6. Quantum dot layer
[0479] 7. Quantum dot-containing solidified layer
[0480] 7G, 7R quantum dot-containing curing layer
[0481] 8 Functional Layer
[0482] 9 Outer coating
[0483] 10R, 10G, 10B sub-pixels
[0484] 11 Counter substrate
[0485] 12 Counter substrate
[0486] 13 Liquid crystal layer
[0487] 20 Camera
[0488] 21 Blue LED
[0489] 40 Color Filters
[0490] 50 Organic protective layer
[0491] 60 Inorganic oxide film
[0492] 71 Transparent Anode
[0493] 72 Hole injection layer
[0494] 73 Hole transport layer
[0495] 74, 74′ Optical components
[0496] 75 Electron injection layer
[0497] 76 cathode
[0498] 80 Luminous Body
[0499] 81 Organic light emitting body
[0500] 100, 101 Optical components
[0501] 200 Micro LED display devices
[0502] 300 Quantum dot light-emitting display device
[0503] 400 LCD display devices
[0504] 500 Organic light-emitting display devices
Claims
1. A quantum dot-containing curable composition comprising a curable adhesive component, quantum dots, and a solvent, The solvent contains ethylene glycol monohexyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monobutyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, dipropylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, 2-ethylhexanoic acid, cyclohexyl acetate, diethyl adipate, dibutyl oxalate, dimethyl malonate, diethyl malonate, dimethyl succinate, diethyl succinate, 3-ethoxy at least one of ethyl propionate, methyl acetoacetate, ethyl acetoacetate, chloroacetic acid, dichloroacetic acid, 2-methylcyclohexanol, 2-octanol, n-heptanol, diacetone alcohol, diisoamyl ether, 1,8-cineole, 3-methoxy-3-methyl-1-butanol, diethylene glycol, 3-methoxy-3-methylbutyl acetate, 3-methoxybutyl acetate, diisobutyl ketone, methylcyclohexanone, methyl-n-hexanone, decane, undecane, tridecane and tetradecane as the first solvent, The invention also contains one or more selected from the group consisting of ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, diethylene glycol dimethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, propylene glycol monomethyl ether acetate, isobutyric acid, propionic acid, butyric acid, ethyl isovalerate, amyl acetate, isopentyl acetate, ethyl lactate, methyl lactate, butyl propionate, butyl butyrate, dimethyl oxalate, acetic acid, acetic anhydride, n-pentanol, isopentanol, 2-ethylbutanol, 1-butanol, n-hexanol, 4-methyl-2-pentanol, cyclohexanol, 2-heptanol, 3-heptanol, ethyl-n-butyl ketone, di-n-propyl ketone, acetylacetone, 1,4-dioxane, octane, and nonane as a second solvent.
2. The quantum dot-containing curable composition according to claim 1, wherein: The solvent contains the first solvent at a ratio of 30% by mass or more and 80% by mass or less, and contains the second solvent at a ratio of 20% by mass or more and 70% by mass or less.
3. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The curable adhesive component contains at least one of a thermosetting adhesive component and a photocurable adhesive component.
4. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The curable adhesive component includes a photocurable adhesive component, the photocurable adhesive component includes a (meth)acrylic resin, a multifunctional (meth)acrylate having two or more acryloyl groups or methacryloyl groups, and a photopolymerization initiator, the (meth)acrylic resin containing at least one of a (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain and a thermally latent (meth)acrylic copolymer having a structural unit derived from a (meth)acrylate monomer containing a tertiary carbon and a structural unit having a hydroxyl group.
5. The quantum dot-containing curable composition according to claim 4, wherein: The thermally latent (meth)acrylate polymer has an acid value of 70 mgKOH / g or less and optionally has a structural unit containing a tertiary amine, and the (meth)acrylic copolymer having a structural unit having an ethylenic double bond in a side chain contains a styrene structural unit.
6. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The curable adhesive component includes a thermosetting adhesive component, and the thermosetting adhesive component contains an epoxy compound and a blocked carboxylic acid curing agent.
7. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The first solvent is selected from one or more of 3-methoxy-3-methyl-1-butanol, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, diethylene glycol dibutyl ether, ethylene glycol monobutyl ether, propylene glycol monobutyl ether, diethylene glycol methyl ethyl ether, dipropylene glycol dimethyl ether, diisoamyl ether, 1,8-cineole, diethyl adipate, dibutyl oxalate, dimethyl malonate, diethyl malonate, dimethyl succinate, diethyl succinate, 3-methoxybutyl acetate, methyl acetoacetate, cyclohexyl acetate, ethyl 3-ethoxypropionate, decane, undecane, tridecane and tetradecane.
8. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The second solvent is selected from one or more of ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, diethylene glycol dimethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, propylene glycol monomethyl ether acetate, ethyl lactate, butyl propionate, butyl butyrate, dimethyl oxalate, 1-butanol, 1,4-dioxane, octane and nonane.
9. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The first solvent is one or more selected from ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, 3-methoxy-3-methylbutyl acetate, ethyl 3-ethoxypropionate, and 3-methoxybutyl acetate, and the second solvent is one or more selected from ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, and propylene glycol monomethyl ether acetate.
10. The quantum dot-containing curable composition according to claim 1 or 2, wherein: The first solvent is one or more selected from the group consisting of 3-methoxy-3-methyl-1-butanol, ethyl 3-ethoxypropionate, and 3-methoxybutyl acetate. 11 . A quantum dot-containing cured product, which is a cured product of the quantum dot-containing curable composition according to claim 1 .
12. A method for manufacturing an optical component, comprising the following steps: A step of selectively attaching the quantum dot-containing curable composition according to any one of claims 1 to 10 to a predetermined area on a substrate by an inkjet method to form a quantum dot-containing layer; and The step of curing the quantum dot-containing layer to form a quantum dot-containing cured layer.
13. The method for manufacturing an optical component according to claim 12, further comprising the following step before the step of forming the quantum dot-containing layer: A step of selectively changing the wettability in a predetermined area of the substrate surface to form a quantum dot layer forming area having a higher affinity with the quantum dot-containing curable composition than the surrounding area; and In the step of forming the quantum dot layer, the quantum dot-containing curable composition is selectively attached to the quantum dot-containing layer formation region by an inkjet method to form the quantum dot layer. 14 . The method for producing an optical member according to claim 12 , further comprising a step of drying the quantum dot-containing layer under reduced pressure.
15. A method for manufacturing a display device, comprising the following steps: a step of manufacturing an optical member by the method for manufacturing an optical member according to any one of claims 12 to 14; and A step of mounting the optical component manufactured as described above.
Citation Information
Patent Citations
LED display having a wavelength conversion layer
JP2016523450A
Light-emitting die and related method incorporating wavelength conversion material
JP2016533030A