Acrylic polyurethane environment-friendly floor paint and preparation method thereof

By using light reflective fillers, anti-aging agents coated with silica and grafted isocyanate functional groups in acrylic polyurethane floor paint, combined with end hydroxyl hyperbranched polyester, the problem of degradation of floor paint in outdoor light is solved, significantly Improves the anti-UV aging performance and construction performance, and extends the service life.

CN118978838APending Publication Date: 2024-11-19NINGBO XUANWEI COLOR WORLD PAINT CO LTD

Patent Information

Application Number
CN202411173923.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Acrylic polyurethane floor paint is prone to photodegradation when exposed to direct sunlight for a long time outdoors, causing the paint film to discolor, powder and peel, affecting the aesthetics and protective performance, and shortening its service life.

Method used

Using an anti-aging agent containing a light reflective filler, coated silica and grafted isocyanate functional groups, the photocatalytic activity is reduced by shielding the light reflective filler and coating the silica, combining isocyanate silane coupling agent and hydroxyl-containing di-di The grafting of benzophenone forms an efficient anti-UV aging agent, and the terminal hydroxyl hyperbranched polyester is added to compensate for the loss of curing rate.

Benefits of technology

It significantly improves the UV aging resistance and construction performance of the paint film, extends the service life of floor paint, and prevents photodegradation and peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010163160000101
    Figure BDA0005010163160000101
Patent Text Reader

Abstract

The invention relates to the field of floor paint, in particular to acrylic polyurethane environment-friendly floor paint and a preparation method thereof. The floor paint comprises 50-80 parts of acrylic resin, 15-25 parts of blocked polyurethane resin, 20-30 parts of pigment, 9-16 parts of an anti-aging agent, 1-2 parts of a wetting dispersant, 1-2 parts of an organic tin catalyst and 5-15 parts of a solvent. The anti-aging agent contains a light reflection filler, silicon dioxide coated on the surface of the light reflection filler and hydroxyl-containing benzophenone grafted on the surface of the silicon dioxide. The floor paint disclosed by the invention has excellent weather resistance and is suitable for field coating in an outdoor environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of floor paints, and in particular to an acrylic polyurethane environmentally friendly floor paint and a preparation method thereof. Background Art

[0002] Acrylic polyurethane floor paint combines the good weather resistance of acrylic resin and the high wear resistance of polyurethane resin, providing excellent resistance to chemical corrosion, wear and impact. In addition, this type of floor paint also has good stain resistance and easy cleaning, and can adapt to various harsh environmental conditions.

[0003] Acrylic polyurethane floor paint is not only suitable for indoor environments, but also performs well in outdoor facilities such as open-air parking lots and sports venues. However, when this type of floor paint is used in outdoor environments, especially when exposed to direct sunlight for a long time, it is prone to photodegradation, causing the paint film to discolor, powder, and even peel off. These changes not only affect the appearance, but also reduce the protective performance of the paint film and shorten the service life of the floor paint. Summary of the invention

[0004] In order to alleviate the problem that acrylic polyurethane floor paint is easily degraded and aged under outdoor lighting environment, the present application provides an acrylic polyurethane environmentally friendly floor paint and a preparation method thereof.

[0005] In a first aspect, the present application provides an acrylic polyurethane environmentally friendly floor paint, which includes the following components in parts by weight: 50 to 80 parts of acrylic resin, 15 to 25 parts of blocked polyurethane resin, 20 to 30 parts of pigment, 9 to 16 parts of anti-aging agent, 1 to 2 parts of wetting dispersant, 1 to 2 parts of organic tin catalyst, and 5 to 15 parts of solvent;

[0006] The anti-aging agent contains light-reflecting filler, silicon dioxide coated on the surface of the light-reflecting filler and hydroxy-containing benzophenone grafted on the surface of the silicon dioxide.

[0007] Preferably, the preparation method of the anti-aging agent is as follows:

[0008] The suspending agent is dissolved in anhydrous ethanol, and a light-reflecting filler is added and dispersed uniformly to obtain a dispersion liquid, and the pH value of the dispersion liquid is adjusted to 8-9 with an alkali solution; an anhydrous ethanol solution of orthosilicate is used as a precursor, and is dripped into the dispersion liquid under stirring conditions, and the temperature is increased to perform a sol-gel reaction to obtain a reaction liquid; the reaction liquid is cooled, the precipitate is filtered out, and it is washed with water until it is neutral, and dried to obtain a composite filler;

[0009] The composite filler is dispersed in anhydrous ethanol, an isocyanate silane coupling agent is added, the mixture is stirred for reaction, and then hydroxybenzophenone is added, the mixture is stirred for reaction, and the mixture is filtered, washed with water, and dried to obtain the product.

[0010] Preferably, the light reflecting filler is titanium dioxide and / or zinc oxide.

[0011] Preferably, the median particle size of the light reflecting filler is 5 to 20 microns.

[0012] Preferably, the suspending agent is selected from one or more of polyvinyl pyrrolidone, polyvinyl alcohol and hydroxyethyl cellulose.

[0013] Preferably, the hydroxy-containing benzophenone is selected from one or more of 2,4-dihydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, hydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 2-hydroxy-4-n-octyloxybenzophenone.

[0014] Preferably, the hydroxy-containing benzophenone contains at least two hydroxyl functional groups.

[0015] Preferably, the mass ratio of silicon dioxide to light reflective filler in the precursor is 0.5-1.5:10.

[0016] Preferably, in the precursor, the mass fraction of silicon dioxide is 15 to 35%.

[0017] Preferably, the mass ratio of the composite filler, the isocyanate silane coupling agent and the hydroxy-containing benzophenone is 10:0.5-0.8:0.5-1.

[0018] The isocyanate silane coupling agent is 3-isocyanate propyl trimethoxy silane and / or 3-isocyanate propyl triethoxy silane.

[0019] The anti-aging agent of the present application firstly uses a filler with a light-reflecting effect as a base material, and utilizes its shielding and reflecting effect on light to improve the anti-ultraviolet aging performance of the paint film. Secondly, by coating the surface of the light-reflecting filler with silica, on the one hand, the agglomeration of titanium dioxide can be reduced and its uniform dispersion can be promoted; on the other hand, since titanium dioxide has photocatalytic activity, it generates free radicals after absorbing ultraviolet light, which will cause the degradation of the paint film to a certain extent, and the coating of silica can inhibit its photocatalytic effect. Thirdly, by attaching an isocyanate-based silane coupling agent to silica, the reaction of isocyanate and hydroxyl groups is utilized to achieve the grafting of hydroxy-containing benzophenone, further absorbing ultraviolet rays and reducing the degradation and aging of the paint film.

[0020] In addition, the grafting process improves the utilization rate of hydroxybenzophenone. Specifically, the remaining isocyanate functional groups on the filler surface can react and bond with the acrylic resin, so that a strong chemical bond is formed between the base resin, the light-reflecting filler, and the hydroxybenzophenone, reducing the migration and precipitation of the antioxidant due to compatibility in the conventional process, and significantly improving the anti-ultraviolet aging performance of the paint film.

[0021] Preferably, the viscosity of the acrylic resin (25° C., Grignard) is 40 to 80S, the hydroxyl value is 50 to 60 mgKOH / g, and the acid value is 5 to 15 mgKOH / g. For example, BS-965 and BS-965H can be selected.

[0022] Preferably, the blocked polyurethane resin is a methanol or ethanol blocked polyurethane resin, and its viscosity is 150-450 mPa﹒s.

[0023] Preferably, the organotin catalyst is dibutyltin dilaurate.

[0024] Preferably, the wetting and dispersing agent can be selected from a type that is compatible with the pigment to ensure uniform dispersion of the pigment. For example, AFCONA-5207 is compatible with high molecular weight organic pigments, and EFKA-5207 is compatible with titanium dioxide.

[0025] Preferably, the solvent is selected from ethyl acetate, butyl acetate, toluene, xylene, ethylene glycol butyl ether, cyclohexanone or isobutanol.

[0026] Other additives may be added to the floor paint of the present application, such as defoaming agent, leveling agent, wear-resistant filler, anti-settling agent, and matting agent.

[0027] Preferably, the floor paint also comprises 5 to 10 parts of terminal hydroxyl hyperbranched polyester.

[0028] Exemplarily, the hydroxyl-terminated hyperbranched polyester is Boltorn H40.

[0029] Although the reaction of the isocyanate group on the surface of the above-mentioned anti-aging agent and the acrylic resin can improve the anti-ultraviolet aging performance of the paint film, it also reduces the curing rate of the polyurethane resin, which is unfavorable for the rapid curing of the floor paint and increases the construction difficulty. By adding the terminal hydroxyl hyperbranched polyester, the loss of its curing rate can be compensated to ensure construction performance. In addition, the addition of the terminal hydroxyl hyperbranched polyester has an enhanced toughening effect, and a paint film with a more balanced rigidity and toughness can be obtained, which improves the wear resistance of the paint film.

[0030] In a second aspect, the present application provides a method for preparing an acrylic polyurethane environmentally friendly floor paint, which comprises:

[0031] Adopting any of the above-mentioned floor paint component ratios; mixing acrylic resin, dispersant, anti-aging agent, pigment and 50-80wt% of solvent, and grinding to obtain slurry;

[0032] Add the blocked polyurethane resin, the organic tin catalyst and the remaining solvent into the slurry and mix them evenly to obtain the slurry.

[0033] The hydroxyl-terminated hyperbranched polyester can be added together with an acrylic resin or a blocked polyurethane resin, preferably added together with an acrylic resin.

[0034] In summary, this application has the following beneficial effects:

[0035] The anti-aging agent of the present application uses a light-reflecting filler as a base material, and through the coated silica, isocyanate functional groups and hydroxy-containing benzophenone are grafted to obtain a highly efficient migration-resistant anti-aging agent, which significantly improves the anti-ultraviolet aging performance of the paint film. Furthermore, by adding a terminal hydroxyl hyperbranched polyester, the curing rate of the floor paint is compensated to ensure its construction performance. DETAILED DESCRIPTION

[0036] Preparation Example

[0037] Preparation Example 1, an anti-aging agent, the preparation method is as follows:

[0038] Dissolve 10g of polyvinyl pyrrolidone in 500mL of anhydrous ethanol, add 100g of titanium dioxide (median particle size of 10 microns), disperse evenly to obtain a dispersion, and add ammonia water to adjust the pH of the dispersion to 9. Take methyl orthosilicate and anhydrous ethanol as raw materials, prepare a precursor solution with a mass fraction of SiO2 of 20%, and drip 50g of the precursor solution into the dispersion through a micropump under stirring conditions. The dripping is completed within 2h, and then the temperature is raised to 55°C for sol-gel reaction. After 2h, a reaction solution is obtained. The reaction solution is cooled to room temperature, the precipitate is filtered out and washed with deionized water until neutral, and dried to constant weight to obtain a composite filler.

[0039] Weigh 100g of the composite filler and disperse it in anhydrous ethanol, add 6.8g of 3-isocyanatepropyltrimethoxysilane, stir and react for 30min, then add 8.3g of 2,2',4,4'-tetrahydroxybenzophenone, stir and react for 1h, separate and filter, wash three times with deionized water, and dry to constant weight.

[0040] Preparation Example 2, an anti-aging agent, the preparation method is as follows:

[0041] 8g of polyvinyl pyrrolidone was dissolved in 500mL of anhydrous ethanol, 100g of titanium dioxide (median particle size of 10 microns) was added, and the mixture was evenly dispersed to obtain a dispersion, and ammonia water was added to adjust the pH of the dispersion to 9. A precursor solution with a mass fraction of SiO2 of 30% was prepared using methyl orthosilicate and anhydrous ethanol as raw materials. Under stirring conditions, 33g of the precursor solution was dripped into the dispersion through a micropump, and the addition was completed within 1h. The mixture was then heated to 50°C for sol-gel reaction, and a reaction solution was obtained after 2h. The reaction solution was cooled to room temperature, the precipitate was filtered out and washed with deionized water until neutral, and dried to constant weight to obtain a composite filler.

[0042] Weigh 100g of the composite filler and disperse it in anhydrous ethanol, add 5.2g of 3-isocyanatepropyltriethoxysilane, stir and react for 20min, then add 6.5g of 2,4-dihydroxybenzophenone, stir and react for 1h, separate and filter, wash three times with deionized water, and dry to constant weight.

[0043] Preparation Example 3, an anti-aging agent, the preparation method is as follows:

[0044] Dissolve 10g of polyvinyl pyrrolidone in 500mL of anhydrous ethanol, add 100g of zinc oxide (median particle size of 15 microns), disperse evenly to obtain a dispersion, and add ammonia water to adjust the pH of the dispersion to 8. Take methyl orthosilicate and anhydrous ethanol as raw materials, prepare a precursor solution with a mass fraction of SiO2 of 16%, and drip 31.5g of the precursor solution into the dispersion through a micropump under stirring conditions. The addition is completed within 1h, and then the temperature is raised to 55°C for sol-gel reaction. After 2h, a reaction solution is obtained. The reaction solution is cooled to room temperature, the precipitate is filtered out and washed with deionized water until neutral, and dried to constant weight to obtain a composite filler.

[0045] Weigh 100 g of the composite filler and disperse it in anhydrous ethanol, add 8.0 g of 3-isocyanatepropyltrimethoxysilane, stir and react for 30 minutes, then add 9.8 g of 2-hydroxy-4-methoxybenzophenone, stir and react for 1.5 hours, separate and filter, wash three times with deionized water, and dry to constant weight.

[0046] Preparation Example 4, an anti-aging agent, is different from Preparation Example 1 in that 2,2',4,4'-tetrahydroxybenzophenone is replaced by an equal amount of oxybenzophenone.

[0047] Preparation Example 5, an anti-aging agent, which differs from Preparation Example 1 in that hydroxy-containing benzophenone is not grafted, and the specific preparation method is as follows:

[0048] Dissolve 10g of polyvinyl pyrrolidone in 500mL of anhydrous ethanol, add 100g of titanium dioxide (median particle size of 10 microns), disperse evenly to obtain a dispersion, and add ammonia water to adjust the pH of the dispersion to 9. Take methyl orthosilicate and anhydrous ethanol as raw materials, prepare a precursor solution with a mass fraction of SiO2 of 20%, and drip 50g of the precursor solution into the dispersion through a micropump under stirring conditions. The dripping is completed within 2h, and then the temperature is raised to 55°C for sol-gel reaction. After 2h, a reaction solution is obtained. The reaction solution is cooled to room temperature, the precipitate is filtered out and washed with deionized water until neutral, and dried to constant weight to obtain a composite filler.

[0049] 100 g of the composite filler was weighed and dispersed in anhydrous ethanol, 6.8 g of 3-isocyanatepropyltrimethoxysilane was added, and the mixture was stirred for reaction for 30 min; the mixture was separated and filtered, washed three times with deionized water, and dried to constant weight.

[0050] Preparation Example 6, an anti-aging agent, which differs from Preparation Example 5 in that no isocyanate silane coupling agent is grafted, and the specific preparation method is as follows:

[0051] Dissolve 10g of polyvinyl pyrrolidone in 500mL of anhydrous ethanol, add 100g of titanium dioxide (median particle size of 10 microns), disperse evenly to obtain a dispersion, and add ammonia water to adjust the pH of the dispersion to 9. Take methyl orthosilicate and anhydrous ethanol as raw materials, prepare a precursor solution with a mass fraction of SiO2 of 20%, under stirring conditions, drop 50g of the precursor solution into the dispersion through a micropump, and complete the dropwise addition within 2h, then heat to 55°C for sol-gel reaction, and obtain a reaction solution after 2h. Cool the reaction solution to room temperature, filter out the precipitate and wash it with deionized water until neutral, dry it to constant weight, and obtain an anti-aging agent.

[0052] Preparation Example 7, an anti-aging agent, which differs from Preparation Example 1 in that it is not coated with silicon dioxide. The specific preparation method is as follows:

[0053] Weigh 100g of titanium dioxide (median particle size of 10 microns) and disperse it in anhydrous ethanol, add 6.8g of 3-isocyanatepropyltrimethoxysilane, stir and react for 30 minutes, then add 8.3g of 2,2',4,4'-tetrahydroxybenzophenone, stir and react for 1 hour, separate and filter, wash three times with deionized water, and dry to constant weight.

[0054] Example

[0055] In the following examples, the raw materials are selected as follows: BS-965H acrylic resin; ethanol blocked polyurethane resin with a viscosity of 300 mPa﹒s; Boltorn H40 terminal hydroxyl hyperbranched polyester; AFCONA-5207 wetting and dispersing agent; phthalocyanine green G pigment; and ethylene glycol butyl ether solvent.

[0056] Example 1, an acrylic polyurethane environmentally friendly floor paint, the preparation steps are as follows:

[0057] Weigh 670 g of acrylic resin, 75 g of terminal hydroxyl hyperbranched polyester, 15.8 g of wetting and dispersing agent, 10 g of leveling agent (BYK-361N), 20 g of anti-settling agent (bentonite), 8 g of defoaming agent (BYK-354), 136 g of the anti-aging agent obtained in Preparation Example 1, 265 g of pigment and 80 g of solvent, mix them, stir evenly at a speed of 500 rpm, and grind to obtain a slurry.

[0058] Add 210 g of blocked polyurethane resin, 13 g of dibutyltin dilaurate and 30 g of solvent into the slurry, and mix well to obtain the slurry.

[0059] Example 2, an acrylic polyurethane environmentally friendly floor paint, the preparation steps are as follows:

[0060] Weigh 530 g of acrylic resin, 100 g of terminal hydroxyl hyperbranched polyester, 11.5 g of wetting and dispersing agent, 15 g of leveling agent (BYK-361N), 25 g of anti-settling agent (bentonite), 10 g of defoaming agent (BYK-354), 90 g of the anti-aging agent obtained in Preparation Example 2, 300 g of pigment and 50 g of solvent, mix them, stir evenly at a speed of 500 rpm, and grind to obtain a slurry.

[0061] Add 150 g of blocked polyurethane resin, 10 g of dibutyltin dilaurate and 20 g of solvent into the slurry, and mix well to obtain the slurry.

[0062] Example 3, an acrylic polyurethane environmentally friendly floor paint, the preparation steps are as follows:

[0063] Weigh 800 g of acrylic resin, 50 g of terminal hydroxyl hyperbranched polyester, 18 g of wetting and dispersing agent, 15 g of leveling agent (BYK-361N), 25 g of anti-settling agent (bentonite), 12 g of defoaming agent (BYK-354), 160 g of the anti-aging agent obtained in Preparation Example 3, 300 g of pigment and 110 g of solvent, mix them, stir evenly at a speed of 500 rpm, and grind to obtain a slurry.

[0064] Add 240 g of blocked polyurethane resin, 18 g of dibutyltin dilaurate and 40 g of solvent into the slurry, and mix well to obtain the slurry.

[0065] Example 4, an acrylic polyurethane environmentally friendly floor paint, is different from Example 1 in that the anti-aging agent obtained in Preparation Example 3 is replaced by an equal amount of the anti-aging agent obtained in Preparation Example 4.

[0066] Example 5, an acrylic polyurethane environmentally friendly floor paint, differs from Example 1 in that no terminal hydroxyl hyperbranched polyester is added.

[0067] Comparative Example

[0068] Comparative Example 1, an acrylic polyurethane environmentally friendly floor paint, is different from Example 5 in that the anti-aging agent obtained in Preparation Example 1 is replaced by an equal amount of the anti-aging agent obtained in Preparation Example 5.

[0069] Comparative Example 2, an acrylic polyurethane environmentally friendly floor paint, is different from Example 5 in that the anti-aging agent obtained in Preparation Example 1 is replaced by an equal amount of the anti-aging agent obtained in Preparation Example 6.

[0070] Comparative Example 3, an acrylic polyurethane environmentally friendly floor paint, is different from Example 5 in that the anti-aging agent obtained in Preparation Example 1 is replaced by an equal amount of the anti-aging agent obtained in Preparation Example 7.

[0071] Comparative Example 4, an acrylic polyurethane environmentally friendly floor paint, is different from Example 5 in that the anti-aging agent obtained in Preparation Example 1 is replaced by a mixture of 70 g of the anti-aging agent obtained in Preparation Example 5 and 30 g of 2,2',4,4'-tetrahydroxybenzophenone.

[0072] Performance testing

[0073] Test 1: Anti-ultraviolet aging performance test

[0074] The floor paint was sprayed on the spray plate to make a test plate, with 5 test plates in each group. After the test plates were irradiated under a QUV xenon lamp for 500 hours, the Co1ourEye@XTS colorimeter was used to test the color value difference (△E) before and after irradiation under the test conditions of light source D65-10 and color measurement angle of 45°. The test results were taken as the average value, as shown in Table 1.

[0075] Test 2: Curing speed test

[0076] The test was carried out according to the finger touch method in GB / T 1728-1979 (89). The test temperature was 23±2℃ and the test was carried out every 10 minutes. The test results are shown in Table 1.

[0077] Test 3: Wear resistance test

[0078] The test was carried out in accordance with GB / T 1768-2006 "Determination of abrasion resistance of paints and varnishes - Rotating rubber grinding wheel method". The rubber grinding wheel was Cs-10, the counterweight was 1 kg, the specified number of revolutions was 2000, 5 specimens were prepared in each group, and the average mass loss of the specimens was calculated. The test results were accurate to 0.1 mg, as shown in Table 1.

[0079] Table 1. Floor paint performance test results

[0080]

[0081] Test results analysis

[0082] 1. Combining the values ​​of △E (500h) in Examples 1 to 5, Comparative Examples 1 to 4 and Table 1, it can be seen that the anti-ultraviolet aging performance of the paint film can be significantly improved by using the light-reflecting filler as the substrate, through the coated silica, and then grafting the isocyanate functional group and the hydroxy-containing benzophenone. And when the silica coating and the hydroxy-containing benzophenone grafting are not performed, the anti-ultraviolet aging performance of the paint film is reduced. The reason may be that the light-reflecting filler has good ultraviolet light reflection and absorption, and has a good anti-ultraviolet effect, and the coating of silica can inhibit the photocatalytic effect of the light-reflecting filler and reduce the degradation and damage of the paint film by free radicals. Hydroxy-containing benzophenone can cooperate with titanium dioxide to play a more excellent ultraviolet absorption effect through grafting, and it is not easy to migrate and precipitate in the paint film, which effectively guarantees the durability of its anti-ultraviolet performance.

[0083] Furthermore, in combination with the values ​​of surface drying time and average mass loss in Example 1 and Example 5 and Table 1, it can be seen that, based on the application of the above-mentioned anti-aging agent, the floor paint of the present application can compensate for the problem of decreased curing rate caused by the introduction of isocyanate in the anti-aging agent by adding terminal hydroxyl hyperbranched polyester, and improve the wear resistance of the paint film.

[0084] The embodiments of the present application are described above, but the present application is not limited to the above-mentioned specific implementation modes. The above-mentioned specific implementation modes are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. An acrylic polyurethane environmentally friendly floor paint, It is characterized in that The composition comprises the following components in parts by weight: 50-80 parts of acrylic resin, 15-25 parts of blocked polyurethane resin, 20-30 parts of pigment, 9-16 parts of anti-aging agent, 1-2 parts of wetting and dispersing agent, 1-2 parts of organic tin catalyst, 5-15 parts of solvent; The anti-aging agent contains light-reflecting filler, silicon dioxide coated on the surface of the light-reflecting filler and hydroxy-containing benzophenone grafted on the surface of the silicon dioxide.

2. The floor paint according to claim 1, It is characterized in that The preparation method of the anti-aging agent is as follows: The suspending agent is dissolved in anhydrous ethanol, and a light-reflecting filler is added and dispersed uniformly to obtain a dispersion liquid, and the pH value of the dispersion liquid is adjusted to 8-9 with an alkali solution; an anhydrous ethanol solution of orthosilicate is used as a precursor, and is dripped into the dispersion liquid under stirring conditions, and the temperature is increased to perform a sol-gel reaction to obtain a reaction liquid; the reaction liquid is cooled, the precipitate is filtered out, and it is washed with water until it is neutral, and dried to obtain a composite filler; The composite filler is dispersed in anhydrous ethanol, an isocyanate silane coupling agent is added, the mixture is stirred for reaction, and then hydroxybenzophenone is added, the mixture is stirred for reaction, and the mixture is filtered, washed with water, and dried to obtain the product.

3. The floor paint according to claim 1, It is characterized in that The light reflecting filler is titanium dioxide and / or zinc oxide.

4. The floor paint according to claim 1, It is characterized in that The hydroxy-containing benzophenone is selected from one or more of 2,4-dihydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, oxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 2-hydroxy-4-n-octyloxybenzophenone.

5. The floor paint according to claim 2, It is characterized in that The mass ratio of silicon dioxide to light-reflecting filler in the precursor is 0.5-1.5:

10.

6. The floor paint according to claim 2, It is characterized in that The mass ratio of the composite filler, the isocyanate silane coupling agent and the hydroxy-containing benzophenone is 10:0.5-0.8:0.5-1.

7. The floor paint according to claim 2, It is characterized in that The isocyanate silane coupling agent is 3-isocyanate propyl trimethoxy silane and / or 3-isocyanate propyl triethoxy silane.

8. The floor paint according to claim 1, It is characterized in that The floor paint also includes 5 to 10 parts of terminal hydroxyl hyperbranched polyester.

9. The floor paint according to claim 1, It is characterized in that The organic tin catalyst is dibutyltin dilaurate.

10. A method for preparing an acrylic polyurethane environmentally friendly floor paint, It is characterized in that include: Adopting the composition ratio of the floor paint described in any one of claims 1 to 9; Mixing acrylic resin, wetting and dispersing agent, anti-aging agent, pigment and 50-80 wt % of solvent, and grinding to obtain slurry; Add the blocked polyurethane resin, the organic tin catalyst and the remaining solvent into the slurry and mix them evenly to obtain the slurry.

Citation Information

Patent Citations

  • Preparation method of light-resistant MDI (diphenyl-methane-diisocyanate) polyurethane

    CN102924901A

  • Water-based nano antistatic epoxy floor paint and preparation method thereof

    CN108165076A

  • Waterborne terrace finish paint and preparation method thereof

    CN108997915A

  • Preparation method of modified waterborne polyurethane coating

    CN118359988A

  • Titanium dioxide coated with silica

    JP2013249229A

Cited By

  • Wear-resistant anti-aging polyurethane resin and preparation method thereof

    CN120059121A

  • High-filling super-curing floating coating in field of rail transit

    CN120484693A