Anti-yellowing and anti-aging silicone sealant and preparation method thereof

By using PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate fillers, the challenges of yellowing and aging are addressed, achieving enhanced UV resistance and mechanical properties are addressed, the challenges of yellowing and aging are addressed, achieving enhanced UV resistance and mechanical properties are addressed, achieving enhanced UV resistance and mechanical effectiveness are achieved, achieving effective and effective and effective and effective, effective and effective, effective and effective, effective, effective, effective, effective, effective, effective, effective, effective, effective, effective, achieving enhanced UV resistance and mechanical effectiveness are achieved.

CN119081640AInactive Publication Date: 2024-12-06HUBEI JUNBANG NEW MATERIAL TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411456948.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicone sealants suffer from yellowing and aging issues due to long-term sunlight exposure and humidity, leading to reduced mechanical properties and stability.

Method used

Incorporation of PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate fillers, along with a specific preparation method, to enhance UV resistance and antioxidant capacity, improving dispersibility and mechanical strength.

Benefits of technology

The solution significantly enhances the sealant's UV resistance, reducing yellowing and aging effects while maintaining mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005090733630000141
    Figure BDA0005090733630000141
  • Figure BDA0005090733630000151
    Figure BDA0005090733630000151
  • Figure BDA0005090733630000171
    Figure BDA0005090733630000171
Patent Text Reader

Abstract

The invention relates to the field of silicone sealants, and particularly discloses an anti-yellowing and anti-aging silicone sealant and a preparation method thereof. The anti-yellowing and anti-aging silicone sealant is prepared from the following raw materials in parts by weight: 1000 parts of alpha-hydrogen-omega-hydroxyl-polydimethylsiloxane, 5 to 10 parts of a cross-linking agent, 0.05 to 5 parts of a catalyst, 1 to 10 parts of a plasticizer, 5 to 15 parts of phenyltriethoxysilane modified zinc oxide coated calcium carbonate, 0.5 to 2 parts of a mildew preventive, 1 to 3 parts of a light stabilizer, 0.5 to 5 parts of a coupling agent and 3 to 8 parts of PDMS modified flower-like copper sulfide. The silicone sealant provided by the invention has excellent and long-acting anti-aging and anti-ultraviolet effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of silicone sealants, and more specifically, to an anti-yellowing and aging silicone sealant and a preparation method thereof. Background Art

[0002] Silicone sealant is a paste made of polydimethylsiloxane as the main raw material, supplemented by cross-linking agent, filler, plasticizer, coupling agent, catalyst, etc., mixed under vacuum state, and solidified by condensation reaction with moisture in the air at room temperature to form elastic silicone rubber. Due to its high tensile strength, strong bonding force, excellent electrical properties and chemical inertness, and also has weather resistance, flame resistance, moisture resistance, breathability, vibration resistance and other properties, its application value is very large, and it is widely used in kitchens, bathrooms, toilets, sanitary ware and waterproof sealing of joints between countertops, walls, and furniture, and the amount is increasing. However, after long-term use, such as long-term sunlight exposure or mildew, silicone glue is prone to yellowing. In particular, the use environment is relatively humid all year round, and silicone glue is easily invaded by microorganisms such as bacteria and mold, resulting in moldy and yellowing of the rubber strips, and the ultraviolet rays in the environment will promote the aging of silicone glue, greatly affecting the appearance. Therefore, how to improve the anti-yellowing and anti-aging properties of silicone glue is a technical problem that technicians in this field need to solve.

[0003] In the prior art, application number CN112480860B discloses a one-component silicone sealant with excellent yellowing resistance and weather resistance and a preparation method thereof, comprising the following raw materials in parts by weight: 100 parts of α, ω-dihydroxypolydimethylsiloxane, 1-10 parts of a plasticizer, 80-150 parts of nano-calcium carbonate, 5-20 parts of titanium dioxide, 5-12 parts of a cross-linking agent, 0.5-2 parts of a coupling agent and 0.05-5 parts of a catalyst; the titanium dioxide is rutile titanium dioxide coated with cerium oxide.

[0004] Although the above silicone sealants have added rutile titanium dioxide, their aging resistance, powdering resistance and yellowing resistance have been improved, but there are still problems with the compatibility and poor dispersibility of the silicone glue matrix, which makes the anti-yellowing and anti-aging functions of the silicone sealant unstable and not lasting, and will affect the mechanical properties of the sealant. Summary of the invention

[0005] In order to improve the stability and durability of the anti-aging and anti-yellowing effects of silicone sealants and increase their mechanical properties, the present application provides an anti-yellowing and aging silicone sealant and a preparation method thereof.

[0006] In a first aspect, the present application provides an anti-yellowing and aging silicone sealant, which adopts the following technical solution:

[0007] The invention discloses an anti-yellowing and aging silicone sealant, comprising the following raw materials in parts by weight: 1000 parts of α-hydrogen-ω-hydroxy-polydimethylsiloxane, 5-10 parts of a cross-linking agent, 0.05-5 parts of a catalyst, 1-10 parts of a plasticizer, 5-15 parts of phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, 0.5-2 parts of a mildewproofing agent, 1-3 parts of a light stabilizer, 0.5-5 parts of a coupling agent, and 3-8 parts of PDMS-modified flower-shaped copper sulfide.

[0008] By adopting the above technical scheme, phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate and PDMS-modified flower-shaped copper sulfide are used as fillers, which can improve the mechanical strength of the sealant and increase the UV resistance and antioxidant capacity at the same time; the ultraviolet absorption of calcium carbonate is low, but after zinc oxide is coated on its surface, the ultraviolet absorption is significantly improved, and the zinc oxide coating can significantly improve the reinforcement effect. Phenyltriethoxysilane and polydimethylsiloxane are both organic silicon compounds, and they have certain similarities in structure, thereby improving the compatibility between zinc oxide-coated calcium carbonate and the base glue; zinc oxide-coated calcium carbonate uses calcium carbonate as a core layer and zinc oxide as a shell layer, and a chemical reaction occurs between zinc oxide and phenyltriethoxysilane. Chemical bonding occurs with the shell layer, and a silanization reaction occurs, thereby grafting on the surface of the zinc oxide-coated calcium carbonate. After phenyltriethoxysilane is coated on the surface of the zinc oxide-coated calcium carbonate, a chemical bond occurs between them, thereby improving the dispersibility of the zinc oxide-coated calcium carbonate in the silicone adhesive. In addition, the decomposition temperature of phenyltriethoxysilane is relatively high, which increases the heat stability of the silicone adhesive and improves the hydrophobicity of the surface of the zinc oxide-coated calcium carbonate, thereby improving its dispersibility in the polymer, thereby improving the UV resistance of the silicone adhesive, effectively resisting UV aging, and reducing the degree of yellowing. The flower-shaped copper sulfide nanomaterial, with its unique flower-shaped hierarchical porous structure and photoelectric effect, makes the seal have a good anti-ultraviolet yellowing effect.

[0009] Optionally, the preparation method of the PDMS-modified flower-shaped copper sulfide is as follows:

[0010] Tetrabutyl titanate is mixed with anhydrous ethanol and deionized water, hydrochloric acid is added, and the mixture is stirred to form a sol. Flower-shaped copper sulfide is evenly mixed with hydrochloric acid and sodium hexametaphosphate, and the mixture is added to the sol. The mixture is reacted at 110-120° C. for 12-14 hours, cooled to room temperature, centrifuged, washed, and dried to obtain a load. The mass ratio of tetrabutyl titanate to flower-shaped copper sulfide is 30-40:1.

[0011] The load is mixed with polydimethylsiloxane, a curing agent and isopropyl alcohol, stirred evenly and then dried at 100-180° C. for 10-80 minutes.

[0012] By adopting the above technical scheme, titanium dioxide has good anti-ultraviolet performance, can achieve the improvement of the anti-ultraviolet performance of organic polymers, can absorb ultraviolet rays, reduce the erosion of ultraviolet rays on sealants, reduce the possibility of yellowing under ultraviolet light, and also improve its overall mechanical properties. Flower-shaped copper sulfide is used to modify titanium dioxide to inhibit photocatalytic performance and improve anti-ultraviolet effect. The flower-shaped hierarchical porous structure of flower-shaped copper sulfide can load titanium dioxide therein, and prevent the formation of superoxide free radicals and hydroxyl free radicals by blocking oxygen, water vapor and the reaction of electrons-holes generated on the surface of titanium dioxide after absorbing ultraviolet rays, thereby inhibiting the excellent photocatalytic activity of titanium dioxide. Then, PMDS is compounded with flower-shaped copper sulfide loaded with titanium dioxide, and the load formed by flower-shaped copper sulfide loaded with titanium dioxide is P MDS polysiloxane wrapping, PMDS is a low surface energy material, which can form a thin film on the surface of flower-shaped copper sulfide and wrap the flower-shaped copper sulfide, mix more evenly with the base glue, increase the moisture and heat resistance of the sealant, improve the resistance to moisture and heat yellowing, and PDMS (polydimethylsiloxane) contains Si-O-Si bonds, and the bond energy of Si-O-Si bonds is large, and the energy required to destroy the PDMS molecular chain is high, so PDMS can also be lower than the decomposition of ultraviolet rays. The special structure of flower-shaped copper sulfide makes it anti-ultraviolet, and the clustering of nanosheets makes its specific surface area larger, and there are some holes inside. When ultraviolet rays are irradiated to the surface of flower-shaped copper sulfide, the ultraviolet rays are reflected multiple times inside the holes of the nanosheets, so that the energy is reduced or offset, and finally a relatively excellent anti-ultraviolet aging and yellowing effect is achieved.

[0013] Optionally, the preparation method of the flower-shaped copper sulfide is as follows: dissolve 3.4 g of cupric chloride dihydrate in 120 ml of ethylene glycol solution, heat to 120° C., stir for 20 min until completely dissolved, add 6.08 g of thiourea to 100 ml of ethylene glycol solution, stir for 30 min to mix evenly, add the two dissolved solutions into a 250 ml high-pressure reactor, react in a 170° C. forced drying oven for 5 h, cool naturally to room temperature, wash the product with deionized water and ethanol, vacuum dry at 50° C. for 10 h, and grind to obtain flower-shaped copper sulfide.

[0014] By adopting the above technical scheme, with copper sulfide as the copper source, thiourea as the sulfur source, and ethylene glycol as the solvent, the copper sulfide crystal nuclei generated under solvothermal conditions will first grow in a directional manner along the low surface energy direction to form nanosheets. The nanosheets have a large specific surface area and the electrical properties of the two sides are opposite. The side where Cu atoms are concentrated is positively charged, and the side where S atoms are enriched is negatively charged. Due to the difference in electronegativity, the nanosheet structure will be unstable. In order to balance the positive and negative energy system, the nanosheets will cross-self-assemble into a flower-like structure and stabilize, forming flower-shaped copper sulfide microspheres.

[0015] Optionally, the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate comprises phenyltriethoxysilane and zinc oxide-coated calcium carbonate in a mass ratio of 1:2-3.

[0016] By adopting the above technical scheme, phenyltriethoxysilane (PETS) is a silane coupling agent, which can chemically bond with zinc oxide-coated calcium carbonate and undergo silanization reaction with the surface of zinc oxide, thereby being grafted on the surface of the zinc oxide shell, which is beneficial to improving the dispersibility of zinc oxide-coated calcium carbonate in the matrix glue. Moreover, the modified PTES can realize the conversion of ultraviolet light into thermal energy or low-energy light waves, and has an inhibitory effect on the photocatalytic activity of zinc oxide itself. Water molecules are difficult to adsorb on the surface of nanoparticles, thereby preventing the generation of hydroxyl radicals and eliminating ultraviolet light degradation or ultraviolet light aging.

[0017] Optionally, the preparation method of the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is as follows:

[0018] The zinc oxide coated calcium carbonate is dispersed in a mixture of anhydrous ethanol and an ammonia solution, phenyltriethoxysilane is added after uniform dispersion, ultrasonicated for 30-40 minutes, heated at 50-55° C. and stirred for 20-24 hours, washed with anhydrous ethanol, vacuum dried at 60-80° C. for 20-24 hours, and ground to obtain phenyltriethoxysilane-modified zinc oxide coated calcium carbonate.

[0019] By adopting the above technical scheme, phenyltriethoxysilane can be hydrolyzed to produce silanol, which undergoes a silanization reaction with the surface of zinc oxide-coated calcium carbonate, thereby being grafted onto the zinc oxide-coated calcium carbonate, thereby improving the dispersibility and compatibility of the zinc oxide-coated calcium carbonate in the matrix glue, and improving the mechanical strength and anti-ultraviolet aging effect.

[0020] Optionally, the preparation method of the zinc oxide coated calcium carbonate is as follows:

[0021] In parts by weight, 30-35 parts of expanded vermiculite are dispersed in 600-700 parts of deionized water to form a suspension, 9-10.5 parts of hydrochloric acid and 9-10.5 parts of sodium chloride are added, and after stirring evenly, suction filtration and washing are repeated until no chloride ions remain, drying to constant weight, grinding through a 300-mesh sieve, and obtaining an acidified sodium powder;

[0022] 5.4-5.5 parts of sodium acidified powder and 162-165 parts of deionized water are mixed to form a suspension, an ethanol solution and a zinc acetate solution with a concentration of 1-1.5 mol / l are added, and the mixture is ultrasonically dispersed for 15-20 min, and a zinc acetate solution with a concentration of 3-4.5 mol / l is added, and the mixture is heated in a water bath at 85-90° C. and stirred for 2.5-3 h, washed and filtered until there is no acetate ion, dried to constant weight, calcined at 350-360° C. for 2 h, and ground through a 300 mesh sieve to obtain expanded vermiculite-loaded zinc oxide powder;

[0023] The expanded vermiculite loaded zinc oxide powder is added to silica sol with a concentration of 20-30wt%, and after being evenly dispersed by ultrasonic, it is sprayed on calcium carbonate particles and dried to obtain zinc oxide coated calcium carbonate. The mass ratio of expanded vermiculite to silica sol is 0.05-0.1:1.

[0024] By adopting the above technical solution, the zinc oxide particles are smaller and have higher surface energy. In addition, under the influence of van der Waals force, the particles are easily adsorbed and agglomerated with lithium ions. The aluminum oxide octahedron and silicon oxide tetrahedron in the expanded vermiculite are combined in different proportions, giving it a unique two-dimensional layered structure, so that it has a greater potential for loading zinc oxide particles. Acidification of the expanded vermiculite can create more attachment points for the zinc oxide particle precursor, while sodiumization creates more ion exchange potential for the synthesized zinc oxide / expanded vermiculite. After treatment, the surface of the expanded vermiculite is flat and The smooth surface becomes rough, which is convenient for the loading of zinc oxide, indicating that the sodium acid treatment can promote the loading effect of expanded vermiculite on zinc oxide particles; when expanded vermiculite is used as a carrier and introduced into the preparation process of zinc oxide, zinc oxide particles can be embedded or loaded in the carrier layer, which reduces the agglomeration of zinc oxide particles to a certain extent. Zinc oxide particles are evenly distributed on the surface of expanded vermiculite. On the one hand, the integrity of the two-dimensional layered structure of layered expanded vermiculite is maintained, which is conducive to the formation of intercalation or exfoliation structure of zinc oxide / expanded vermiculite in silicone sealant. In addition, when heat and oxygen are combined with silicon When the ketone sealant interacts with the expanded vermiculite, the two-dimensional layered structure of the expanded vermiculite loaded with zinc oxide can inhibit the volatilization of components, block the penetration of heat and oxygen, and extend the transmission distance in the seal after some oxygen and heat penetrate into the seal. On the other hand, the expanded vermiculite loaded with zinc oxide improves the ultraviolet light absorption capacity of the expanded vermiculite. When exposed to ultraviolet radiation, zinc oxide can absorb, reflect or scatter ultraviolet light, reduce the adverse effects of ultraviolet light on the sealant, and delay the ultraviolet aging of the sealant. Finally, the expanded vermiculite loaded with zinc oxide is sprayed with silica sol. Coated on calcium carbonate to obtain zinc oxide-coated calcium carbonate, silica sol has good adhesion strength and can firmly adhere expanded vermiculite to the outer surface of calcium carbonate. Silica sol has excellent UV resistance and can improve the color stability of the material and delay the yellowing of the sealant. The zinc oxide-coated calcium carbonate prepared in this way can inhibit the volatilization rate of silicone sealant in the short-term aging process, enhance the anti-aging ability, delay the rate of thermal oxygen aging and ultraviolet aging, reduce the sensitivity of performance changes after aging, and improve the resistance to long-term thermal oxygen aging and long-term ultraviolet aging.

[0025] Optionally, the amount of expanded vermiculite loaded with zinc oxide in the zinc oxide-coated calcium carbonate is 3-4% of the mass of the calcium carbonate particles.

[0026] By adopting the above technical solution, the amount of expanded vermiculite loaded with zinc oxide is appropriate, which can better play a reinforcing role and improve the ultraviolet protection effect without affecting the tensile strength of the seal.

[0027] The inventors found through experiments that selecting a specific content of phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate and PDMS-modified flower-shaped copper sulfide as components to prepare a silicone sealant has better yellowing and aging resistance than using either one alone. This may be because the two work together to improve the aging resistance of the silicone sealant through the above-mentioned different anti-ultraviolet and aging resistance principles.

[0028] Optionally, the light stabilizer includes a benzotriazole ultraviolet light absorber and a hindered amine light stabilizer in a mass ratio of 1-2:5.

[0029] By adopting the above technical scheme, the benzotriazole ultraviolet light absorber can absorb ultraviolet light through the rapid tautomerism of excited hydrogen bonds and release energy in the form of heat energy, while the hindered amine light stabilizer is a free radical scavenger, which can capture the free radicals generated by the polymer to reduce the photodegradation rate of the polymer, thereby improving the polymer's resistance to ultraviolet aging. The combination of the two can increase the resistance to ultraviolet aging.

[0030] Optionally, the plasticizer is polydimethylsiloxane;

[0031] The crosslinking agent is selected from at least one of methyltriacetoxysilane, methyltributylidene oxime silane, methyltrimethoxysilane or methylisopropenyloxysilane;

[0032] The catalyst is selected from stannous octoate, dibutyltin dilaurate, dibutyltin dioctoate, dibutyltin diacetate, dibutyltin dimethoxide, dibutyltin oxide, and a compound of tetraisopropyl titanate, tetra-n-butyl titanate, diisopropoxy-bis(acetylacetonato) titanium, and diisopropoxy-bis(ethyl acetoacetate) titanium.

[0033] The coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane.

[0034] In a second aspect, the present application provides a method for preparing a yellowing-resistant and aging-resistant silicone sealant, which adopts the following technical solution:

[0035] A method for preparing an anti-yellowing and aging silicone sealant comprises the following steps:

[0036] Mix α-hydrogen-ω-hydroxy-polydimethylsiloxane, a plasticizer, a mildew preventer, a light stabilizer, a coupling agent, 3-8 parts of PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, heat to 120-130° C., stir in vacuum to obtain a base material, cool to below 50° C., add a crosslinking agent and a catalyst under nitrogen protection, mix well, and obtain a silicone sealant.

[0037] By adopting the above technical solution, the raw materials are mixed to obtain the product. The preparation method is simple and easy to operate, and industrial production can be realized.

[0038] Optionally, during the vacuum stirring, the vacuum degree is -(0.05-0.12) MPa, the stirring time is 3-4 h, and the stirring speed is 300-400 rpm.

[0039] By adopting the above technical solution, using a lower vacuum degree can help remove bubbles and volatile substances in the mixture, improve the quality and stability of the product, and the longer stirring time can fully ensure that the raw materials are mixed evenly, while avoiding overheating of the materials or causing unnecessary chemical reactions. The moderate stirring speed can promote the uniform dispersion of the barrier and avoid excessive shear heat.

[0040] In summary, this application has the following beneficial effects:

[0041] 1. Since the present application adopts α-hydrogen-ω-hydroxy-polydimethylsiloxane as the base glue, and adds PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, the flower-shaped copper sulfide and zinc oxide-coated calcium carbonate both have good anti-ultraviolet effects, and PDMS and phenyltriethoxysilane can respectively improve the dispersibility of flower-shaped copper sulfide and zinc oxide-coated calcium carbonate with the base glue, while increasing the moisture and heat resistance effect, reducing moisture penetration, improving the moisture and mildew resistance effect, and also increasing the anti-ultraviolet aging and heat-resistant yellowing effects.

[0042] 2. In the present application, flower-shaped copper sulfide is preferably used to load titanium dioxide, and PMDS is used for hydrophobic coating. Titanium dioxide has good resistance to ultraviolet aging. In addition, flower-shaped copper sulfide as a carrier and PMDS as a hydrophobic modifier can synergistically inhibit the self-photocatalytic activity of titanium dioxide, thereby reducing ultraviolet light degradation or ultraviolet light aging.

[0043] 3. In the present application, it is preferred to use acidified and sodiumized expanded vermiculite and zinc acetate to prepare expanded vermiculite-loaded zinc oxide, and then use silica sol to evenly adhere only the expanded vermiculite-loaded zinc oxide to calcium carbonate. Expanded vermiculite is used as a carrier, and zinc acetate is used to synthesize zinc oxide, which can improve the dispersion uniformity of zinc oxide on the expanded vermiculite and reduce the agglomeration of zinc oxide. At the same time, the multilayer structure of expanded vermiculite is used to improve the anti-ultraviolet effect. DETAILED DESCRIPTION

[0044] The following examples further illustrate the present application in detail.

[0045] Preparation Example 1-3 of PDMS-modified flower-shaped copper sulfide

[0046] Preparation Example 1: (1) Dissolve 3.4 g of cupric chloride dihydrate in 120 ml of ethylene glycol solution, heat to 120° C., and stir for 20 min until completely dissolved. Add 6.08 g of thiourea to 100 ml of ethylene glycol solution, stir for 30 min to mix evenly, add the two portions of the solution into a 250 ml autoclave, react in a 170° C. forced air drying oven for 5 h, cool naturally to room temperature, wash the product with deionized water and ethanol, vacuum dry at 50° C. for 10 h, and grind to obtain flower-like copper sulfide;

[0047] (2) 40 g of tetrabutyl titanate was added to 200 ml of anhydrous ethanol, mixed and stirred evenly, 40 ml of deionized water was added, stirred for 1 h, a white precipitate was obtained, 40 ml of 1 mol / l hydrochloric acid was added, and stirred to form a sol; 1 g of flower-shaped copper sulfide was mixed with 10 ml of 1 mol / l hydrochloric acid and sodium hexametaphosphate, added to the sol, stirred and reacted at 120° C. for 12 h, cooled to room temperature, centrifuged, washed, and dried at 80° C. for 24 h to obtain a load;

[0048] (3) 2 g of the load was mixed with 1 g of polydimethylsiloxane, 0.1 g of a curing agent and 10 g of isopropyl alcohol, stirred evenly, and dried at 100° C. for 80 min. The PDMS and the curing agent were selected from Dow Corning DC184.

[0049] Preparation Example 2: (1) Dissolve 3.4 g of cupric chloride dihydrate in 120 ml of ethylene glycol solution, heat to 120° C., and stir for 20 min until completely dissolved. Add 6.08 g of thiourea to 100 ml of ethylene glycol solution, stir for 30 min to mix evenly, add the two portions of the solution into a 250 ml autoclave, react in a 170° C. forced air drying oven for 5 h, cool naturally to room temperature, wash the product with deionized water and ethanol, vacuum dry at 50° C. for 10 h, and grind to obtain flower-like copper sulfide;

[0050] (2) 30 g of tetrabutyl titanate was added to 150 ml of anhydrous ethanol, mixed and stirred evenly, 30 ml of deionized water was added, stirred for 1 h, a white precipitate was obtained, 30 ml of 1 mol / l hydrochloric acid was added, and stirred to form a sol; 1 g of flower-shaped copper sulfide was mixed with 10 ml of 1 mol / l hydrochloric acid and sodium hexametaphosphate, added to the sol, stirred and reacted at 110° C. for 14 h, cooled to room temperature, centrifuged, washed, and dried at 80° C. for 24 h to obtain a load;

[0051] (3) 2 g of the load was mixed with 1 g of polydimethylsiloxane, 0.1 g of a curing agent and 10 g of isopropyl alcohol, stirred evenly, and dried at 180° C. for 10 min. The PDMS and the curing agent were selected from Dow Corning DC184.

[0052] Preparation Example 3: (1) Dissolve 3.4 g of cupric chloride dihydrate in 120 ml of ethylene glycol solution, heat to 120° C., and stir for 20 min until completely dissolved. Add 6.08 g of thiourea to 100 ml of ethylene glycol solution, stir for 30 min to mix evenly, add the two portions of the solution into a 250 ml autoclave, react in a 170° C. forced air drying oven for 5 h, cool naturally to room temperature, wash the product with deionized water and ethanol, vacuum dry at 50° C. for 10 h, and grind to obtain flower-like copper sulfide;

[0053] (2) 2 g of flower-shaped copper sulfide was mixed with 1 g of polydimethylsiloxane, 0.1 g of a curing agent and 10 g of isopropyl alcohol, stirred evenly, and dried at 100° C. for 80 min. The PDMS and the curing agent were selected from Dow Corning DC184.

[0054] Preparation Example 4-10 of Phenyltriethoxysilane Modified Zinc Oxide Coated Calcium Carbonate

[0055] Preparation Example 4: (1) 30 g of expanded vermiculite was dispersed in 600 g of deionized water to form a suspension, 9 g of hydrochloric acid and 9 g of sodium chloride were added, and after stirring, the mixture was filtered and washed repeatedly until no chloride ions remained (tested with a silver nitrate solution), dried to constant weight, and ground through a 300-mesh sieve to obtain a sodium acid powder;

[0056] (2) 5.4 g of sodium acid powder was mixed with 162 g of deionized water to form a suspension, 106 g of ethanol solution and 200 g of 1 mol / l zinc acetate solution were added, ultrasonic dispersion was performed for 15 min, 200 g of 3 mol / l zinc acetate solution was added, the mixture was heated in a water bath at 85° C. and stirred for 3 h, washed and filtered until there was no acetate ion, dried to constant weight, calcined at 350° C. for 2 h, and ground through a 300 mesh sieve to obtain expanded vermiculite-loaded zinc oxide powder;

[0057] (3) adding expanded vermiculite-loaded zinc oxide powder to 40 wt % silica sol, uniformly dispersing by ultrasonication, spraying on calcium carbonate particles, and drying to obtain zinc oxide-coated calcium carbonate, wherein the mass ratio of expanded vermiculite to silica sol is 0.1:1, the amount of expanded vermiculite-loaded zinc oxide is 4% of the mass of calcium carbonate particles, and the silica sol is selected from Guangdong Huierte Nanotechnology Co., Ltd., model HS-40;

[0058] (4) Disperse 10 g of zinc oxide-coated calcium carbonate in a mixture of 600 ml of anhydrous ethanol and an ammonia solution (the volume ratio of anhydrous ethanol to ammonia solution is 1:1), add phenyltriethoxysilane after uniform dispersion, ultrasonicate for 30 min, heat to 55 ° C, stir for 24 h, wash with anhydrous ethanol, dry at 60 ° C for 24 h, and grind to obtain phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate. The mass ratio of phenyltriethoxysilane to zinc oxide-coated calcium carbonate is 1:3. Phenyltriethoxysilane is selected from Wuhan Chengtian Fine Chemicals, model CT11996.

[0059] Preparation Example 5: (1) 35 g of expanded vermiculite was dispersed in 700 g of deionized water to form a suspension, 10.5 g of hydrochloric acid and 10.5 g of sodium chloride were added, and after stirring, the mixture was filtered and washed repeatedly until no chloride ions remained (tested with a silver nitrate solution), dried to constant weight, and ground through a 300-mesh sieve to obtain a sodium acid powder;

[0060] (2) 5.5 g of sodium acidified powder was mixed with 165 g of deionized water to form a suspension, 106 g of ethanol solution and 200 g of 1.5 mol / l zinc acetate solution were added, ultrasonic dispersion was performed for 20 min, 200 g of 4.5 mol / l zinc acetate solution was added, the mixture was heated in a water bath at 90° C. and stirred for 2.5 h, washed and filtered until there was no acetate ion, dried to constant weight, calcined at 360° C. for 2 h, and ground through a 300 mesh sieve to obtain expanded vermiculite-loaded zinc oxide powder;

[0061] (3) adding expanded vermiculite-loaded zinc oxide powder to 40 wt % silica sol, uniformly dispersing by ultrasonication, spraying on calcium carbonate particles, and drying to obtain zinc oxide-coated calcium carbonate, wherein the mass ratio of expanded vermiculite to silica sol is 0.05:1, the amount of expanded vermiculite-loaded zinc oxide is 3% of the mass of calcium carbonate particles, and the silica sol is selected from Guangdong Huierte Nanotechnology Co., Ltd., model HS-40;

[0062] (4) Disperse 10 g of zinc oxide-coated calcium carbonate in a mixture of 600 ml of anhydrous ethanol and an ammonia solution (the volume ratio of anhydrous ethanol to ammonia solution is 1:1), add phenyltriethoxysilane after uniform dispersion, ultrasonicate for 40 min, heat to 50 ° C, stir for 20 h, wash with anhydrous ethanol, dry at 80 ° C for 20 h, and grind to obtain phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate. The mass ratio of phenyltriethoxysilane to zinc oxide-coated calcium carbonate is 1:2. Phenyltriethoxysilane is selected from Wuhan Chengtian Fine Chemicals, model CT11996.

[0063] Preparation Example 6: The difference from Preparation Example 4 is that in step (3), the amount of expanded vermiculite loaded with zinc oxide is 1% of the mass of the calcium carbonate particles.

[0064] Preparation Example 7: The difference from Preparation Example 4 is that in step (3), the amount of expanded vermiculite loaded with zinc oxide is 6% of the mass of the calcium carbonate particles.

[0065] Preparation Example 8: The difference from Preparation Example 4 is that zinc acetate is not used to prepare zinc oxide, 35 g of expanded vermiculite and 35 g of zinc oxide are evenly mixed to obtain expanded vermiculite-loaded zinc oxide powder, and the rest is the same as Preparation Example 4.

[0066] Preparation Example 9: The difference from Preparation Example 4 is that an equal amount of deionized water is used instead of silica sol.

[0067] Preparation Example 10: The difference from Preparation Example 4 is that the zinc oxide is not treated with expanded vermiculite. The zinc oxide is added to a silica sol with a concentration of 40wt%, ultrasonicated for 20 minutes, and after uniform dispersion, it is sprayed on calcium carbonate particles and dried at 80°C to obtain zinc oxide-coated calcium carbonate. The mass ratio of zinc oxide to silica sol is 0.1:1, and the amount of zinc oxide is 4% of the mass of the calcium carbonate particles. The rest is the same as Preparation Example 4.

[0068] Example

[0069] Example 1: A yellowing-resistant aging silicone sealant, the raw material dosage is as shown in Table 1, wherein α-hydrogen-ω-hydroxy-polydimethylsiloxane is selected from Hubei Wande Chemical, with a product number of WD1207, the plasticizer is polydimethylsiloxane, the cross-linker is methyltriacetoxysilane, the catalyst is stannous octoate, the coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane, the light stabilizer includes a benzotriazole ultraviolet light absorber and a hindered amine light stabilizer in a mass ratio of 1:5, the benzotriazole light stabilizer is BASF Tinuvin326, the hindered amine light stabilizer is BASF Tinuvin770, the PDMS-modified flower-shaped copper sulfide is prepared from Preparation Example 1, and the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 4.

[0070] The method for preparing the above-mentioned anti-yellowing and aging silicone sealant comprises the following steps:

[0071] α-Hydrogen-ω-hydroxy-polydimethylsiloxane, plasticizer, mildewproof agent, light stabilizer, coupling agent, PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate are mixed, the temperature is raised to 120°C, and vacuum stirred to obtain a base material, which is cooled to below 50°C. Under nitrogen protection, a cross-linking agent and a catalyst are added and mixed evenly to obtain a silicone sealant. The vacuum degree is -0.12 MPa, the stirring time is 3 hours, and the stirring speed is 300 rpm.

[0072] Table 1 Raw material dosage of silicone sealant in Examples 1-3

[0073]

[0074]

[0075] Example 2: A yellowing and aging resistant silicone sealant, the raw material dosage is as shown in Table 1, wherein α-hydrogen-ω-hydroxy-polydimethylsiloxane is selected from Hubei Wande Chemical, the product number is WD1207, the plasticizer is polydimethylsiloxane, the cross-linking agent is methyl trisbutyl ketoxime silane, the catalyst is dibutyl tin dilaurate, the coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane, the light stabilizer includes a benzotriazole ultraviolet light absorber and a hindered amine light stabilizer in a mass ratio of 1:2, the benzotriazole light stabilizer is BASF Tinuvin326, and the hindered amine light stabilizer is BASF Tinuvin770. PDMS-modified flower-shaped copper sulfide is prepared from Preparation Example 2, and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 5.

[0076] The method for preparing the above-mentioned anti-yellowing and aging silicone sealant comprises the following steps:

[0077] α-Hydrogen-ω-hydroxy-polydimethylsiloxane, plasticizer, mildewproof agent, light stabilizer, coupling agent, PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate are mixed, the temperature is raised to 130°C, and vacuum stirred to obtain a base material, which is cooled to below 50°C. Under nitrogen protection, a cross-linking agent and a catalyst are added and mixed evenly to obtain a silicone sealant. The vacuum degree is -0.05 MPa, the stirring time is 4 hours, and the stirring speed is 400 rpm.

[0078] Example 3: An anti-yellowing and aging silicone sealant, which is different from Example 1 in that the amounts of raw materials used are as shown in Table 1.

[0079] Example 4: A yellowing-resistant aging silicone sealant, which is different from Example 1 in that the PDMS-modified flower-shaped copper sulfide is prepared by Preparation Example 3.

[0080] Example 5: A yellowing-resistant and aging-resistant silicone sealant, which is different from Example 1 in that phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 6.

[0081] Example 6: A yellowing-resistant and aging-resistant silicone sealant, which is different from Example 1 in that phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 7.

[0082] Example 7: An anti-yellowing and aging silicone sealant, which is different from Example 1 in that phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 8.

[0083] Example 8: An anti-yellowing and aging silicone sealant, which is different from Example 1 in that phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 9.

[0084] Example 9: An anti-yellowing and aging silicone sealant, which is different from Example 1 in that phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is prepared from Preparation Example 10.

[0085] Comparative Example

[0086] Comparative Example 1: A yellowing-resistant aging silicone sealant, which differs from Example 1 in that an equal amount of flower-shaped copper sulfide is used to replace the PDMS-modified flower-shaped copper sulfide.

[0087] Comparative Example 2: A yellowing-resistant aging silicone sealant, which differs from Example 1 in that an equal amount of talcum powder is used to replace the PDMS-modified flower-shaped copper sulfide.

[0088] Comparative Example 3: A yellowing-resistant aging silicone sealant, which differs from Example 1 in that an equal amount of calcium carbonate is used to replace the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate.

[0089] Comparative Example 4: A yellowing and aging resistant silicone sealant, which differs from Example 1 in that an equal amount of zinc oxide-coated calcium carbonate is used to replace phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, zinc oxide and calcium carbonate are mixed to prepare zinc oxide-coated calcium carbonate, and the amount of zinc oxide used is 4% of the mass of calcium carbonate.

[0090] Comparative Example 5: A yellowing-resistant aging silicone sealant, which differs from Example 1 in that an equal amount of phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate is used to replace the PDMS-modified flower-shaped copper sulfide.

[0091] Comparative Example 6: An anti-yellowing and aging silicone sealant, which differs from Example 1 in that an equal amount of PDMS-modified flower-shaped copper sulfide is used to replace phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate.

[0092] Performance testing

[0093] Silicone sealants were prepared according to the methods in the examples and comparative examples, and performance tests were performed according to the following methods. The test results are recorded in Table 2.

[0094] 1. Tensile bond strength and elongation at break: Aluminum alloy is used as the bonding substrate and the test is carried out in accordance with GB / T13477.8-2017 "Test methods for building sealing materials Part 8: Determination of tensile adhesion", and the tensile speed is 6 mm / min.

[0095] 2. Yellowing resistance: Place the film cured at room temperature for 14 days in an oven at 180°C for 12 hours, observe its yellowing degree, and use 0 to 5 levels of yellowing to indicate its yellowing degree. The higher the level, the more serious the yellowing degree.

[0096] 3. UV aging resistance: Put the sample into the aging box, put the test piece into the aging box, and UV age it for 24 hours under a 1000W mercury lamp. Test the tensile strength and elongation at break, and calculate the change rate of mechanical properties before and after UV aging.

[0097] Table 2 Performance test of silicone sealant

[0098]

[0099]

[0100] It can be seen from the data in Examples 1-3 in Table 2 that the silicone sealants prepared by using the PDMS-modified flower-shaped copper sulfide prepared in Preparation Examples 1 and 2 and the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate prepared in Preparation Examples 4 and 5 have high tensile bonding strength, good heat-resistant yellowing effect, are not prone to yellowing, and have strong resistance to ultraviolet aging.

[0101] In Example 4, the PDMS modified flower-like copper sulfide prepared in Preparation Example 3 was used, and tetrabutyl titanate was not used to prepare titanium dioxide to load the flower-like copper sulfide. It can be seen that its yellowing grade is 2, and the change rate of tensile bonding strength and elongation at break increases.

[0102] In Example 5 and Example 6, phenyltriethoxysilane-modified zinc oxide prepared in Preparation Example 6 and Preparation Example 7 was used to coat calcium carbonate, respectively. Compared with Preparation Example 4, the mass of expanded vermiculite-loaded zinc oxide on calcium carbonate was changed. It can be seen that the tensile bonding strength and maximum elongation of the silicone sealants prepared in Example 5 and Example 6 were reduced, indicating that the coating of expanded vermiculite-loaded zinc oxide on calcium carbonate can improve the mechanical strength of the sealant, and the higher the coating amount, the better the anti-aging ability, but too high a coating amount will also affect the mechanical properties.

[0103] In Example 7, phenyltriethoxysilane-modified zinc oxide prepared in Preparation Example 8 was used to coat calcium carbonate. Compared with Preparation Example 4, expanded vermiculite was blended with zinc oxide to prepare expanded vermiculite-loaded zinc oxide powder. The data in Table 2 show that the tensile bonding strength of the silicone sealant prepared in Example 7 is reduced and the yellowing grade is increased, indicating that the use of zinc acetate to prepare zinc oxide can uniformly load zinc oxide in expanded vermiculite, thereby uniformly coating the calcium carbonate, thereby improving the mechanical strength, anti-yellowing and anti-ultraviolet aging capabilities of the sealant.

[0104] In Example 8, compared with Example 1, the phenyltriethoxysilane-modified zinc oxide prepared in Preparation Example 9 was used to coat calcium carbonate, and silica sol was not used to coat the expanded vermiculite-loaded zinc oxide on the calcium carbonate. As can be seen from the data in Table 2, the yellowing grade increased, the mechanical properties deteriorated, and the anti-ultraviolet aging ability weakened, indicating that silica sol can firmly adhere the expanded vermiculite-loaded zinc oxide to the calcium carbonate, thereby improving the anti-ultraviolet ability of calcium carbonate in the sealant.

[0105] In Example 9, phenyltriethoxysilane-modified zinc oxide prepared in Preparation Example 10 was used to coat calcium carbonate. Compared with Preparation Example 1, zinc oxide was directly adhered to calcium carbonate using silica sol and then treated with phenyltriethoxysilane. As shown in Table 2, the anti-yellowing ability deteriorated and the anti-ultraviolet ability weakened.

[0106] Comparative Example 1 Compared with Example 1, flower-shaped copper sulfide that is not modified with PDMS is used instead of flower-shaped copper sulfide that is modified with PDMS. As shown in Table 2, the tensile bonding strength of the silicone sealant decreases and the anti-yellowing ability is slightly weakened.

[0107] In Comparative Example 2, talcum powder is used to replace the PDMS-modified flower-shaped copper sulfide. Compared with Example 1, it can be seen that the tensile bonding strength of the silicone sealant prepared in Comparative Example 2 is reduced, and the anti-yellowing and anti-ultraviolet effects are deteriorated.

[0108] In Comparative Example 3, an equal amount of calcium carbonate was used to replace the phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate. It can be seen that the yellowing level of the silicone sealant increased and the anti-ultraviolet ability weakened.

[0109] In Comparative Example 4, zinc oxide-coated calcium carbonate was used instead of phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate. The anti-ultraviolet and anti-yellowing capabilities of the silicone sealant were slightly improved compared with those of Comparative Example 3, but were still inferior to those of Example 1.

[0110] Compared with Example 1, Comparative Examples 5 and 6 use PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate to replace each other in equal amounts. It can be seen that compared with Example 1, the anti-aging and yellowing resistance of the sealants prepared in Comparative Examples 5 and 6 are reduced.

[0111] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A yellowing and aging-resistant silicone sealant, characterized in that: The invention comprises the following raw materials in parts by weight: 1000 parts of alpha-hydrogen-omega-hydroxy-polydimethylsiloxane, 5-10 parts of a cross-linking agent, 0.05-5 parts of a catalyst, 1-10 parts of a plasticizer, 5-15 parts of phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, 0.5-2 parts of a mildewproofing agent, 1-3 parts of a light stabilizer, 0.5-5 parts of a coupling agent, and 3-8 parts of PDMS-modified flower-shaped copper sulfide.

2. The anti-yellowing and aging silicone sealant according to claim 1, characterized in that: The preparation method of the PDMS-modified flower-shaped copper sulfide is as follows: Tetrabutyl titanate is mixed with anhydrous ethanol and deionized water, hydrochloric acid is added, and the mixture is stirred to form a sol. Flower-shaped copper sulfide is evenly mixed with hydrochloric acid and sodium hexametaphosphate, and the mixture is added to the sol. The mixture is reacted at 110-120° C. for 12-14 hours, cooled to room temperature, centrifuged, washed, and dried to obtain a load. The mass ratio of tetrabutyl titanate to flower-shaped copper sulfide is 30-40:

1. The load is mixed with polydimethylsiloxane, a curing agent and isopropyl alcohol, stirred evenly and then dried at 100-180° C. for 10-80 minutes.

3. The anti-yellowing and aging silicone sealant according to claim 1, characterized in that: The phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate comprises phenyltriethoxysilane and zinc oxide-coated calcium carbonate in a mass ratio of 1:2-3.

4. The anti-yellowing and aging silicone sealant according to claim 3, characterized in that: The preparation method of the phenyltriethoxysilane modified zinc oxide coated calcium carbonate is as follows: The zinc oxide coated calcium carbonate is dispersed in a mixture of anhydrous ethanol and an ammonia solution, phenyltriethoxysilane is added after uniform dispersion, ultrasonicated for 30-40 minutes, heated at 50-55° C. and stirred for 20-24 hours, washed with anhydrous ethanol, vacuum dried at 60-80° C. for 20-24 hours, and ground to obtain phenyltriethoxysilane-modified zinc oxide coated calcium carbonate.

5. The anti-yellowing and aging silicone sealant according to claim 4, characterized in that: The preparation method of the zinc oxide coated calcium carbonate is as follows: In parts by weight, 30-35 parts of expanded vermiculite are dispersed in 600-700 parts of deionized water to form a suspension, 9-10.5 parts of hydrochloric acid and 9-10.5 parts of sodium chloride are added, and after stirring evenly, suction filtration and washing are repeated until no chloride ions remain, drying to constant weight, grinding through a 300-mesh sieve, and obtaining an acidified sodium powder; 5.4-5.5 parts of sodium acidified powder and 162-165 parts of deionized water are mixed to form a suspension, an ethanol solution and a zinc acetate solution with a concentration of 1-1.5 mol / l are added, and the mixture is ultrasonically dispersed for 15-20 min, and a zinc acetate solution with a concentration of 3-4.5 mol / l is added, and the mixture is heated in a water bath at 85-90° C. and stirred for 2.5-3 h, washed and filtered until there is no acetate ion, dried to constant weight, calcined at 350-360° C. for 2 h, and ground through a 300 mesh sieve to obtain expanded vermiculite-loaded zinc oxide powder; The expanded vermiculite loaded zinc oxide powder is added to silica sol with a concentration of 40wt%, and after being uniformly dispersed by ultrasonication, it is sprayed on calcium carbonate particles and dried to obtain zinc oxide coated calcium carbonate. The mass ratio of expanded vermiculite to silica sol is 0.05-0.1:

1.

6. The anti-yellowing and aging silicone sealant according to claim 5, characterized in that: The amount of expanded vermiculite loaded with zinc oxide in the zinc oxide coated calcium carbonate is 3-4% of the mass of the calcium carbonate particles.

7. The anti-yellowing and aging silicone sealant according to claim 1, characterized in that: The light stabilizer comprises a benzotriazole ultraviolet light absorber and a hindered amine light stabilizer in a mass ratio of 1-2:

5.

8. The anti-yellowing and aging silicone sealant according to claim 1, characterized in that: The plasticizer is polydimethylsiloxane; The crosslinking agent is selected from at least one of methyltriacetoxysilane, methyltributylidene oxime silane, methyltrimethoxysilane or methylisopropenyloxysilane; The catalyst is selected from stannous octoate, dibutyltin dilaurate, dibutyltin dioctoate, dibutyltin diacetate, dibutyltin dimethoxide, dibutyltin oxide, and a compound of tetraisopropyl titanate, tetra-n-butyl titanate, diisopropoxy-bis(acetylacetonato) titanium, and diisopropoxy-bis(ethyl acetoacetate) titanium. The coupling agent is γ-(2,3-epoxypropoxy)propyltrimethoxysilane or γ-(methacryloyloxy)propyltrimethoxysilane.

9. The method for preparing the anti-yellowing and aging silicone sealant according to any one of claims 1 to 8, characterized in that: The following steps are involved: Mix α-hydrogen-ω-hydroxy-polydimethylsiloxane, a plasticizer, a mildew preventer, a light stabilizer, a coupling agent, 3-8 parts of PDMS-modified flower-shaped copper sulfide and phenyltriethoxysilane-modified zinc oxide-coated calcium carbonate, heat to 120-130° C., stir in vacuum to obtain a base material, cool to below 50° C., add a crosslinking agent and a catalyst under nitrogen protection, mix well, and obtain a silicone sealant.

10. The method for preparing the anti-yellowing and aging silicone sealant according to claim 9, characterized in that: During the vacuum stirring, the vacuum degree is -(0.05-0.12)MPa, the stirring time is 3-4h, and the stirring speed is 300-400rpm.

Citation Information

Patent Citations

  • Preparation method for super-hydrophobic ultraviolet-proof textiles

    CN107524011A

  • Preparation method of super-hydrophobic photocatalytic anti-ultraviolet textile

    CN108842437A

  • Anti-yellowing and anti-aging silicone sealant and preparation method thereof

    CN110835515A

  • Single-component silicone sealant with excellent yellowing resistance and weather resistance and preparation method thereof

    CN112480860A

  • High-temperature-resistant oil-bath room-temperature-cured silicone rubber and preparation method thereof

    CN112625648A