Fluorine-containing rare earth polishing powder, preparation method thereof and polishing composition
By performing multiple gradient roasting and crushing of fluorocarbonate rare earths, fluorine-containing rare earth polishing powder with high grinding force and low scratching rate was prepared, which solved the problems of insufficient grinding force and high scratching rate of rare earth polishing powder in the prior art, and avoided The use of hydrofluoric acid is risky and high cost.
Patent Information
- Application Number
- CN202411072024.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing rare earth polishing powder has insufficient grinding force and high scratching rate. The use of hydrofluoric acid when introducing fluorine element has safety risks and high cost problems.
By calcining fluorocarbonate rare earths under different temperature gradients, three roasted substances were obtained and then crushed, fluoro-containing rare earth polishing powder was prepared, and its particle size and composition were optimized, the grinding force was increased and the scratching rate was reduced.
The grinding force of fluorine-containing rare earth polishing powder is significantly improved, the scratch rate is reduced, and the safety hazards and high costs of using hydrofluoric acid are avoided.
Abstract
Description
Technical Field
[0001] The invention relates to fluorine-containing rare earth polishing powder and a preparation method and a polishing composition thereof. Background Art
[0002] Rare earth polishing materials are an important component of rare earth functional materials and one of the main applications of light rare earths. Rare earth polishing materials are widely used in the polishing of mobile phone cover glass, 3D glass back shell, SNT glass, etc. Fluorine, as an important doping element of rare earth polishing materials, can improve the polishing speed and service life of polishing powder. Fluorine is usually introduced by adding hydrofluoric acid or rare earth fluoride, but these raw materials are expensive and there is a certain risk when using them.
[0003] CN115321578A discloses a method for preparing a nano-spherical rare earth fluoride polishing powder, which comprises the following steps: mixing lanthanum cerium carbonate and deionized water to prepare a lanthanum cerium carbonate suspension; adding a dispersant and hydrofluoric acid to the lanthanum cerium carbonate suspension, and stirring and mixing; then standing for aging induction, and filtering to obtain a solid product; the dispersant is any one or more combinations of EDTA, citric acid, and tartaric acid; drying the solid product, and then grinding it into powder; calcining the powder, and dispersing the calcined powder in a jet mill to obtain a nano-spherical rare earth fluoride polishing powder.
[0004] CN103288119A discloses a method for preparing rare earth polishing powder, which comprises mixing rare earth carbonate with water, adding a mineralizer, aging, and obtaining a basic rare earth carbonate slurry; adding a hydrofluoric acid solution to the basic rare earth carbonate slurry, stirring for 1 to 3 hours, and dehydrating to obtain a fluorocarbonate rare earth; calcining the fluorocarbonate rare earth to obtain a fluorinated rare earth; and crushing and classifying the fluorinated rare earth to obtain a rare earth polishing powder. In the above document, hydrofluoric acid is used as a fluorine source.
[0005] CN113772713A discloses a method for preparing rare earth lanthanum cerium fluoride polishing powder by roasting method, wherein the raw material of rare earth lanthanum cerium fluoride carbonate is placed in a corundum crucible, placed in a muffle furnace and heated to 400-1050°C at a heating rate of 2-10°C / min, kept warm for 2-8h, and then cooled naturally. The method regulates the crystal form and phase structure of the lanthanum cerium fluoride polishing powder by regulating one or more of the roasting temperature, heating rate, and holding time.
[0006] CN103253694A discloses a calcination process of lanthanum oxide cerium rare earth polishing powder, which undergoes the following temperature history in sequence during the calcination process: (a) the first heating stage, the temperature rises from room temperature to 970°C within 180 to 210 minutes; (b) the first constant temperature stage, the temperature is maintained at 970±5°C for 150 to 180 minutes; (c) the second heating stage, the temperature is raised from 970°C to 1090°C within 30 to 60 minutes; (d) the second constant temperature stage, the temperature is maintained at 1090±5°C for 180 to 240 minutes; (e) the cooling stage, the temperature is reduced from 1090°C to 60 to 100°C within 20 to 40 minutes. The grinding force of the polishing powder prepared by this process needs to be improved, and the scratch rate needs to be reduced. Summary of the invention
[0007] In view of this, one object of the present invention is to provide a method for preparing a fluorine-containing rare earth polishing powder, which can improve the grinding force of the fluorine-containing rare earth polishing powder and reduce the scratch rate of the fluorine-containing rare earth polishing powder. Another object of the present invention is to provide a fluorine-containing rare earth polishing powder. Another object of the present invention is to provide a polishing composition.
[0008] The above purpose is achieved through the following technical solutions.
[0009] In one aspect, the present invention provides a method for preparing a fluorine-containing rare earth polishing powder, comprising the following steps:
[0010] Calcine the rare earth fluorocarbonate at 400-600°C for 0.5-3h to obtain a primary calcined product;
[0011] The primary calcined product is calcined at 600-850°C for 0.5-3h to obtain a secondary calcined product;
[0012] The secondary calcined product is calcined at 850-1200°C for 1-8 hours to obtain a tertiary calcined product;
[0013] The tertiary calcined product is crushed to obtain fluorine-containing rare earth polishing powder.
[0014] According to the preparation method of the present invention, preferably, the primary roasting temperature is less than the secondary roasting temperature and less than the tertiary roasting temperature.
[0015] According to the preparation method of the present invention, preferably, the primary calcination temperature is 450-550° C. and the primary calcination time is 1-2 h.
[0016] According to the preparation method of the present invention, preferably, the primary calcination temperature is 500-550° C.; and the primary calcination time is 1-1.5 h.
[0017] According to the preparation method of the present invention, preferably, the secondary calcination temperature is 650-800° C. and the secondary calcination time is 1-2 h.
[0018] According to the preparation method of the present invention, preferably, the temperature of the third calcination is 900-1100° C.; and the time of the third calcination is 2-6 hours.
[0019] According to the preparation method of the present invention, preferably, the particle size D of the rare earth fluorocarbonate is 50 The particle size is 10 to 70 μm; in the fluorocarbonate rare earth, the total rare earth element content is 50 to 80 wt%, the fluorine element content is 2 to 7 wt%, and the SiO2 content is ≤0.050 wt%.
[0020] On the other hand, the present invention provides a fluorine-containing rare earth polishing powder, which is obtained by the above-mentioned preparation method.
[0021] According to the fluorine-containing rare earth polishing powder of the present invention, preferably, the D 10 0.5~0.9μm, D 50 1.2~1.8μm, D 90 4.5~5.9μm.
[0022] In yet another aspect, the present invention provides a polishing composition comprising the above-mentioned fluorine-containing rare earth polishing powder and water; the mass ratio of the fluorine-containing rare earth polishing powder to water is 1:(2-6).
[0023] The invention bakes rare earth fluorine carbonate at a specific temperature in a gradient heating manner, thereby improving the grinding force of the fluorine-containing rare earth polishing powder and reducing the scratch rate of the fluorine-containing rare earth polishing powder. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0025] The following is an explanation of the terms:
[0026] D 10 : The particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 10%.
[0027] D 50 : The particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%.
[0028] D 90 : The particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 90%.
[0029] Preparation method of fluorine-containing rare earth polishing powder
[0030] The preparation method of the fluorine-containing rare earth polishing powder of the present invention comprises the following steps: a calcination step and a post-treatment step, which are described in detail below.
[0031] The present invention finds that the raw material rare earth fluorine carbonate is very important for improving the grinding force of the fluorine-containing rare earth polishing powder and reducing the scratch rate of the fluorine-containing rare earth polishing powder.
[0032] Particle size D of rare earth fluorocarbonate 50 In some embodiments, the particle size D 50 In some other embodiments, the particle size D 50 The diameter of the polishing powder is 45-55 μm. This is beneficial to improving the grinding force of the fluorine-containing rare earth polishing powder and reducing the scratch rate of the fluorine-containing rare earth polishing powder.
[0033] The content of total rare earth elements in rare earth fluorocarbonate can be 50-80wt%; preferably 60-75wt%; more preferably 65-72wt%. This is conducive to improving the grinding force of fluorine-containing rare earth polishing powder. The content of fluorine element in rare earth fluorocarbonate can be 2-7wt%; preferably 3-6wt%; more preferably 4-5wt%. This is conducive to reducing the scratch rate of fluorine-containing rare earth polishing powder. The content of SiO2 in rare earth fluorocarbonate is ≤0.050wt%; preferably, the content of SiO2 is ≤0.010wt%. This is conducive to improving the grinding force of fluorine-containing rare earth polishing powder and reducing the scratch rate of fluorine-containing rare earth polishing powder.
[0034] The rare earth fluorocarbonate is roasted at 400-600°C for 0.5-3h to obtain a primary roasted product; the primary roasted product is roasted at 600-850°C for 0.5-3h to obtain a secondary roasted product; the secondary roasted product is roasted at 850-1200°C for 1-8h to obtain a tertiary roasted product. The roasting can be carried out in a conventional roasting furnace, which will not be described in detail here.
[0035] The primary calcination temperature may be 400-600°C, preferably 450-550°C, and more preferably 500-550°C.
[0036] The primary calcination time may be 0.5 to 3 hours, preferably 1 to 2 hours, and more preferably 1 to 1.5 hours.
[0037] The secondary calcination temperature may be 600 to 850°C, preferably 650 to 800°C, and more preferably 700 to 800°C.
[0038] The secondary calcination time may be 0.5 to 3 hours, preferably 1 to 2 hours, and more preferably 1 to 1.5 hours.
[0039] The temperature of the third calcination may be 850-1200°C, preferably 900-1100°C, and more preferably 950-1000°C.
[0040] The three calcination times may be 1 to 8 hours, preferably 2 to 6 hours, and more preferably 3 to 4 hours.
[0041] In the present invention, the primary roasting temperature is less than the secondary roasting temperature and less than the tertiary roasting temperature.
[0042] According to one embodiment of the present invention, rare earth fluoride carbonate is calcined at 450-550°C for 1-2 hours to obtain a primary calcined product; the primary calcined product is calcined at 650-800°C for 1-2 hours to obtain a secondary calcined product; the secondary calcined product is calcined at 900-1100°C for 2-6 hours to obtain a tertiary calcined product. In this way, a fluorine-containing rare earth polishing powder with high grinding force and low scratch rate can be obtained.
[0043] According to another embodiment of the present invention, the fluorinated rare earth carbonate is calcined at 500-550°C for 1-1.5 hours to obtain a primary calcined product; the primary calcined product is calcined at 700-800°C for 1-1.5 hours to obtain a secondary calcined product; the secondary calcined product is calcined at 950-1000°C for 3-4 hours to obtain a tertiary calcined product. In this way, a fluorinated rare earth polishing powder with higher grinding force and lower scratch rate can be obtained.
[0044] The above-mentioned calcination conditions are used to treat rare earth fluoride carbonate, which helps to improve the grinding force of the fluorine-containing rare earth polishing powder and reduce the scratch rate of the rare earth polishing powder.
[0045] Post-processing steps
[0046] The tertiary calcined product is crushed to obtain fluorine-containing rare earth polishing powder.
[0047] The tertiary calcined product can be crushed by a method known in the art. For example, the tertiary calcined product can be crushed by wet ball milling. Since the ball milling slurry obtained by wet ball milling contains water, preferably, the following step is also included: drying the ball milling slurry to obtain fluorine-containing rare earth polishing powder. Drying can be carried out by a method commonly used in the art, such as spray drying.
[0048] Fluorine-containing rare earth polishing powder and polishing composition
[0049] The fluorine-containing rare earth polishing powder of the present invention is prepared by the above method. The particle size D of the fluorine-containing rare earth polishing powder is 10 It can be 0.5 to 0.9 μm; preferably 0.6 to 0.8 μm; more preferably 0.65 to 0.75 μm. 50 It can be 1.2 to 1.8 μm; preferably 1.3 to 1.7 μm; more preferably 1.5 to 1.6 μm. 90 It can be 4.5 to 5.9 μm, preferably 4.8 to 5.5 μm, and more preferably 5.1 to 5.2 μm. This helps to improve the grinding force of the fluorine-containing rare earth polishing powder and reduce the scratch rate of the rare earth polishing powder.
[0050] In the fluorine-containing rare earth polishing powder, the content of fluorine element can be 3-8wt% based on the total mass of rare earth compounds; preferably 4-7wt%; more preferably 5-6wt%. Rare earth compounds include rare earth oxides, rare earth fluorides and rare earth fluorides. In the fluorine-containing rare earth polishing powder, the content of total rare earth elements can be 93-98wt%; preferably 94-97wt%; more preferably 96-97wt%. The content of total rare earth elements is calculated in TREO. This helps to improve the grinding force of the fluorine-containing rare earth polishing powder and reduce the scratch rate of the rare earth polishing powder.
[0051] The grinding force of fluorine-containing rare earth polishing powder is ≥0.14mg / cm 2 ·min; preferably, the grinding force ≥ 0.15mg / cm 2 ·min; more preferably, the grinding force ≥ 0.16mg / cm 2 ·min.
[0052] The scratch rate of the fluorine-containing rare earth polishing powder is ≤15%; preferably, the scratch rate is ≤10%; more preferably, the scratch rate is ≤8%.
[0053] The polishing composition of the present invention comprises the above-mentioned fluorine-containing rare earth polishing powder and water. The mass ratio of the fluorine-containing rare earth polishing powder to water can be 1:(2-6); preferably 1:(3-5); more preferably 1:(3.5-4.5).
[0054] The test method of the present invention is described below:
[0055] Particle size: Test according to the method specified in GB / T20170.1.
[0056] Total rare earth content: tested according to the method specified in GB / T14635.
[0057] Content of each rare earth element: tested according to the method specified in GB / T16484.3.
[0058] Fluorine content: tested according to the method specified in GB / T 20166.2-2012. SiO2 content: tested according to the method specified in GB / T 18882.3-2019.
[0059] Example 1
[0060] In lanthanum cerium fluorocarbonate, the mass ratio of lanthanum element to cerium element in terms of chloride is 35:65. The particle size D of lanthanum cerium fluorocarbonate 50 The total rare earth element content calculated by TREO is 67.78wt%; the fluorine content is 4.74wt%; and the SiO2 content is ≤0.010wt%.
[0061] The cerium lanthanum fluorocarbonate is calcined at 500°C for 1 hour to obtain a primary calcined product; the primary calcined product is calcined at 800°C for 1 hour to obtain a secondary calcined product; the secondary calcined product is calcined at 980°C for 3 hours to obtain a tertiary calcined product.
[0062] The three-calcined product is ball-milled in a ball mill and then spray-dried to obtain fluorine-containing rare earth polishing powder.
[0063] The particle size D of the obtained fluorine-containing rare earth polishing powder 10 =0.71μm, D 50 =1.54μm, D 90 =5.17μm. In the fluorine-containing rare earth polishing powder, the total rare earth element content calculated by TREO is 96.4wt%. Based on the rare earth compound, the fluorine content is 5.74wt%. The rare earth compound is the sum of rare earth oxides, rare earth fluoride oxides and rare earth fluorides.
[0064] Example 2
[0065] In lanthanum cerium fluorocarbonate, the mass ratio of lanthanum element to cerium element in terms of chloride is 35:65. The particle size D of lanthanum cerium fluorocarbonate 50 The total rare earth element content calculated by TREO is 71.74wt%; the fluorine content is 4.90wt%; and the SiO2 content is ≤0.010wt%.
[0066] The cerium lanthanum fluorocarbonate is calcined at 500°C for 1 hour to obtain a primary calcined product; the primary calcined product is calcined at 700°C for 1 hour to obtain a secondary calcined product; the secondary calcined product is calcined at 950°C for 6 hours to obtain a tertiary calcined product.
[0067] The three-calcined product is ball-milled in a ball mill and then spray-dried to obtain fluorine-containing rare earth polishing powder.
[0068] Particle size D of fluorine-containing rare earth polishing powder 10 =0.61μm, D 50 =1.52μm, D 90 =5.13 μm. In the fluorine-containing rare earth polishing powder, the total rare earth element content calculated by TREO is 96.12 wt%. Based on the rare earth compound, the fluorine content is 5.81 wt%. The rare earth compound is the sum of rare earth oxides, rare earth fluoride oxides and rare earth fluorides.
[0069] Comparative Example 1
[0070] In lanthanum cerium fluorocarbonate, the mass ratio of lanthanum element to cerium element in terms of chloride is 35:65. The particle size D of lanthanum cerium fluorocarbonate 50The total rare earth element content in terms of TREO is 36.23 wt %, the fluorine content is 1.63 wt %, and the SiO2 content is 0.019 wt %.
[0071] The cerium lanthanum fluorocarbonate is calcined at 500°C for 1 hour to obtain a primary calcined product; the primary calcined product is calcined at 800°C for 1 hour to obtain a secondary calcined product; the secondary calcined product is calcined at 980°C for 3 hours to obtain a tertiary calcined product.
[0072] The three-calcined product is ball-milled in a ball mill and then spray-dried to obtain fluorine-containing rare earth polishing powder.
[0073] Particle size D of fluorine-containing rare earth polishing powder 10 =0.64μm, D 50 =1.54μm, D 90 =5.53μm. In the fluorine-containing rare earth polishing powder, the content of total rare earth elements in terms of TREO is 95.32wt%. Based on the rare earth compound, the content of fluorine element is 5.41wt%. The rare earth compound is the sum of rare earth oxides, rare earth fluoride oxides and rare earth fluorides.
[0074] Comparative Example 2
[0075] Except that the cerium lanthanum fluorocarbonate is calcined once at 800°C for 2 hours to obtain a primary calcined product; and the primary calcined product is calcined twice at 980°C for 3 hours to obtain a secondary calcined product for ball milling, other conditions are the same as those in Example 1, and the details are as follows:
[0076] In lanthanum cerium fluorocarbonate, the mass ratio of lanthanum element to cerium element in terms of chloride is 35:65. The particle size D of lanthanum cerium fluorocarbonate 50 The total rare earth element content calculated by TREO is 67.78wt% and the fluorine content is 4.74wt%; the SiO2 content is ≤0.010wt%.
[0077] The cerium lanthanum fluorocarbonate is calcined once at 800° C. for 2 hours to obtain a primary calcined product; the primary calcined product is calcined twice at 980° C. for 3 hours to obtain a secondary calcined product.
[0078] The secondary calcined product is ball-milled in a ball mill and then spray-dried to obtain fluorine-containing rare earth polishing powder.
[0079] Examples 3 to 4 and Comparative Examples 3 to 4
[0080] The fluorine-containing rare earth polishing powder was slurried with water to obtain a polishing composition with a concentration of 20 wt %. The types of the fluorine-containing rare earth polishing powder are shown in Table 1.
[0081] The grinding force and scratch rate were tested using the method specified in GB / T 20167-2012. The grinding machine used was Shenyang Kejing UNIPOL-1200S, and the glass was JSD-15. The results are shown in Table 1.
[0082] Table 1
[0083] Example 3 Example 4 Comparative Example 3 Comparative Example 4 Types of fluorine-containing rare earth polishing powder Example 1 Example 2 Comparative Example 1 Comparative Example 2 <![CDATA[Grinding force (mg / cm 2 ·min)]]> 0.16 0.15 0.12 0.13 Scratch rate (%) 8 9 16 17
[0084] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing fluorine-containing rare earth polishing powder, It is characterized in that The steps include: Calcine the rare earth fluorocarbonate at 400-600°C for 0.5-3h to obtain a primary calcined product; The primary calcined product is calcined at 600-850°C for 0.5-3h to obtain a secondary calcined product; The secondary calcined product is calcined at 850-1200°C for 1-8 hours to obtain a tertiary calcined product; The tertiary calcined product is crushed to obtain fluorine-containing rare earth polishing powder.
2. The preparation method according to claim 1, It is characterized in that The first roasting temperature is less than the second roasting temperature and less than the third roasting temperature.
3. The preparation method according to claim 1, It is characterized in that The primary calcination temperature is 450-550°C; the primary calcination time is 1-2h.
4. The preparation method according to claim 1, It is characterized in that The primary calcination temperature is 500-550°C; the primary calcination time is 1-1.5h.
5. The preparation method according to claim 1, It is characterized in that The secondary roasting temperature is 650-800°C; the secondary roasting time is 1-2h.
6. The preparation method according to claim 1, It is characterized in that The temperature of the three roastings is 900-1100°C; the time of the three roastings is 2-6h.
7. The preparation method according to claim 1, It is characterized in that Particle size D of rare earth fluorocarbonate 50 The content of total rare earth elements in the fluorocarbonate rare earth is 50-80wt%, the content of fluorine elements is 2-7wt%, and the content of SiO 2 The content is ≤0.050wt%.
8. A fluorine-containing rare earth polishing powder, It is characterized in that The fluorine-containing rare earth polishing powder is obtained by the preparation method according to any one of claims 1 to 7.
9. The fluorine-containing rare earth polishing powder according to claim 8, It is characterized in that The D of the fluorine-containing rare earth polishing powder 10 0.5~0.9μm, D 50 1.2~1.8μm, D 90 4.5~5.9μm.
10. A polishing composition, It is characterized in that The polishing composition comprises the fluorine-containing rare earth polishing powder according to claim 8 or 9 and water; the mass ratio of the fluorine-containing rare earth polishing powder to water is 1:(2-6).