Long-afterglow crystal material constructed by phosphine derivatives as well as preparation method and application of long-afterglow crystal material
By using phosphine derivatives and benzophene to construct host-guest crystal materials, the problem of short afterglow time of existing organic long afterglow materials is solved, and the preparation of high-efficiency long afterglow luminescent materials is achieved, with excellent afterglow performance and industrial application potential.
Patent Information
- Application Number
- CN202410986408.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-19
AI Technical Summary
The existing home-guest organic long afterglow materials have short afterglow time and fewer types, making it difficult to develop materials with high efficiency and long life.
Using phosphine derivatives (such as (+)-1,2-bis((2S,5S)-2,5-diphenylphosphine)ethane as the main material, combined with benzophenylade as the guest material, and by evaporation crystallization method Prepare subject-guest crystal materials to achieve regular structural integrity and long afterglow luminescence.
A green long afterglow material with an afterglow time of more than 6 seconds was successfully prepared, with good afterglow luminescence performance, suitable for industrial applications, and supports applications in fields such as data encryption and anti-counterfeiting.
Smart Images

Figure CN118978909A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic afterglow crystal materials, and in particular to a long afterglow crystal material constructed with phosphine derivatives and a preparation method and application thereof. Background Art
[0002] The core of long-persistent luminescence materials is a kind of "night-bright" material, which achieves the so-called "long-persistent luminescence" (LPL) by storing and slowly releasing excited state energy. It has been widely used in anti-counterfeiting, encryption, bio-imaging and optoelectronic devices. Compared with inorganic LPL materials, organic LPL (organic long-persistent luminescence, OLPL) materials have some obvious advantages, such as easy synthesis, easy functional modification and easy processing. In particular, the continuous room temperature phosphorescence can be regulated by reasonable molecular design, which makes OLPL materials applicable to some new application fields, such as high-end anti-counterfeiting, ultraviolet detection biomedical imaging and sensing, identity (fingerprint, hair, body fluid, etc.) recognition and marking or organic scintillator imaging applications. In particular, the use of afterglow light to achieve biomedical imaging detection can effectively avoid the background interference caused by in-situ excitation in existing technologies, which makes organic long-persistent materials more and more concerned by scientific researchers.
[0003] Although the afterglow time and afterglow brightness of organic long afterglow materials have been improved through various controls and designs, it is still a huge challenge to develop organic long afterglow materials with high efficiency and long lifetime due to weak spin-orbit coupling and very fast non-radiative decay in pure organic matter.
[0004] Compared with single-component organic long afterglow materials, the preparation methods and existence forms of molecular doped organic long afterglow materials are more diverse, and the unique properties of the host material itself will also have a great influence on the optical properties of the afterglow. Therefore, host-guest type organic long afterglow materials have attracted much attention in recent years. However, there are still huge problems with host-guest doped organic long afterglow materials: 1) The time of host-guest type organic long afterglow materials is still relatively short, mostly less than 3s; 2) There are currently few types of host-guest type organic afterglow luminescent materials, especially the sources of host materials are relatively few, most of which use compounds such as diphenylamine, triphenylphosphine, and benzophenone, making it difficult to obtain a longer afterglow time.
[0005] Therefore, developing more host-guest type organic long afterglow crystal luminescent materials to achieve longer afterglow time is a difficult problem that needs to be solved urgently in this field. Summary of the invention
[0006] Based on the above problems, one of the purposes of the present invention is to provide a long afterglow crystal material constructed with phosphine derivatives, the raw materials for its preparation are cheap and easily available, and the material has good afterglow luminescence performance, and the afterglow lifetime is as long as 6s.
[0007] The second object of the present invention is to provide a method for preparing the long afterglow crystal material constructed with phosphine derivatives, which uses a host material and a guest material with a simple structure and cheap and easily available to prepare the crystal material. The preparation method is simple, the conditions are mild, and harsh conditions such as high temperature and high pressure are not required. At the same time, the prepared material belongs to a host-guest type organic doped crystal afterglow material, which has a regular crystal morphology and good afterglow luminescence performance, and is suitable for industrial market applications.
[0008] The third object of the present invention is to provide the application of the long afterglow crystal material constructed with the phosphine derivatives.
[0009] The purpose of the present invention is achieved by the following technical solutions:
[0010] A long afterglow crystal material constructed with phosphine derivatives is prepared by evaporating and crystallizing a main material and a guest material; in the long afterglow crystal material constructed with phosphine derivatives, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material;
[0011] The main material is The guest material is
[0012] When constructing the crystal structure, the present invention selects a phosphine derivative ((+)-1,2-bis((2S,5S)-2,5-diphenylphosphino)ethane) that is easy to crystallize and cheap and readily available as the main material, and introduces triphenylene as the guest material to construct a structurally regular crystal structure, thereby obtaining a new green long afterglow luminescent material with an afterglow time of more than 6s and good afterglow luminescent performance. The present invention successfully prepares a green afterglow material that can exhibit a long life by only using the simplest host-guest material mixed crystallization, demonstrating its application potential in the fields of information encryption and anti-counterfeiting.
[0013] More preferably, the mass ratio of the host material to the guest material is (80-120):1, more preferably 100:1.
[0014] More preferably, the excitation wavelength of the long afterglow crystal material constructed with phosphine derivatives is 360-380 nm, more preferably 365 nm.
[0015] A method for preparing a long afterglow crystal material constructed with phosphine derivatives comprises the following steps:
[0016] (1) mixing the host material and the guest material uniformly to obtain a solid powder;
[0017] (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the long afterglow crystal material constructed with the phosphine derivative.
[0018] When preparing the crystal material, the present invention uses a simple evaporation crystal mixing method to dope a small amount of triphenylene as an electron guest material into a phosphine derivative ((+)-1,2-bis((2S,5S)-2,5-diphenylphosphino)ethane) host material, thereby successfully constructing a new host-guest type crystal afterglow material, which can be excited by ultraviolet light and can effectively enhance the afterglow time and brightness of the crystal material. The improvement of afterglow time and brightness can effectively support the high-efficiency long afterglow luminescence application of organic crystalline long afterglow materials.
[0019] Further preferably, in step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1:(80-120).
[0020] More preferably, in step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
[0021] Further preferably, in step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 min.
[0022] More preferably, in step (2), the temperature for standing and volatilizing is 15 to 30°C.
[0023] More preferably, after the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
[0024] The application of the long afterglow crystal material constructed with phosphine derivatives is specifically the application as a luminescent material in data encryption materials or anti-counterfeiting materials.
[0025] The long afterglow crystal material constructed with phosphine derivatives provided by the present invention can be excited by ultraviolet light, has the characteristics of environmental stability, can form a regular crystal morphology, and has an afterglow time of more than 6 seconds, with better performance than conventional crystal afterglow materials. The improvement of afterglow time, mild and undemanding preparation conditions, and stable performance are very beneficial to the application of organic crystalline long afterglow materials in various scenarios. Therefore, the long afterglow crystal material provided by the present invention can provide new ideas for the design and synthesis of new crystal long afterglow materials, and is also conducive to promoting the further development of long afterglow materials in practical applications such as data encryption and anti-counterfeiting. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for describing the embodiments and test examples;
[0027] Figure 1 The optical images of the afterglow display of the long afterglow crystal material constructed with phosphine derivatives obtained in Example 1 of the present invention before (a) and after (bh) irradiation with 365nm ultraviolet light;
[0028] Figure 2 These are optical images of the afterglow display of the crystal material obtained in Comparative Example 1 before (a) and after (bd) irradiation with 365nm ultraviolet light. DETAILED DESCRIPTION
[0029] The technical scheme and technical effects of the present invention will be clearly and completely described below in conjunction with specific embodiments and accompanying drawings. However, it should be understood by those skilled in the art that the embodiments are only used to illustrate the technical scheme of the present invention and should not be regarded as limiting the scope of protection of the present invention. Based on the following embodiments, all other implementation schemes obtained by ordinary technicians in the field without making creative work, such as modification, deformation or simple replacement, should belong to the scope of protection of the present invention.
[0030] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the raw materials used are all commonly used in the art, available to the public or commercially available, unless otherwise specified; the terms and abbreviations involved have the conventional meanings in the art.
[0031] Example 1
[0032] The long afterglow crystal material constructed with phosphine derivatives provided in this embodiment is prepared by using a host material and a guest material through an evaporation crystallization method; in the long afterglow crystal material constructed with phosphine derivatives, the host material forms regular crystals, and the guest material is freely dispersed in the crystals of the host material; wherein the structural formula of the host material is: The name is (+)-1,2-bis((2S,5S)-2,5-diphenylphosphine)ethane; the structural formula of the guest material is: The name is benzophenone.
[0033] The method for preparing the long afterglow crystal material constructed with the phosphine derivatives comprises the following steps:
[0034] According to the mass ratio of the host material to the guest material of 100:1, 0.0010 g of the guest material (triphenylene) and 0.1000 g of the host material ((+)-1,2-bis((2S,5S)-2,5-diphenylphosphino)ethane) were accurately weighed and mixed to obtain a solid powder;
[0035] Add 0.05 mL of dichloromethane to the solid powder and dissolve it for 1 min, then add 5 mL of ethanol, stir at room temperature (20-25°C) and 600 rpm for 5 min until it is completely dissolved, then place it in an atmospheric environment at room temperature of 20-25°C to evaporate slowly until crystals precipitate. After the crystals precipitate, centrifuge the solution containing the crystals, wash the crystals with ethanol after centrifugation, and dry them at room temperature (20-25°C) for 3 h to obtain the long afterglow crystalline material constructed with phosphine derivatives of Example 1.
[0036] Comparative Example 1
[0037] This comparative example provides a crystalline material, and its preparation process is carried out with reference to Example 1. The only difference from Example 1 is that the structure of the main material used is different. The main material used in this comparative example is diphenylamine, and the structural formula is
[0038]
[0039] Comparative Example 2
[0040] This comparative example provides a crystalline material, and its preparation process is carried out with reference to Example 1. The only difference from Example 1 is that the structure of the guest material used is different. The guest material used in this comparative example is benzanthracene, and its structural formula is
[0041]
[0042] Test Example 1: Performance test of the material in Example 1
[0043] Under room temperature and atmospheric environment, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material constructed with phosphine derivatives in Example 1, and then the excitation light source was turned off, and the afterglow brightness change of the crystal material after the light source was removed was recorded. The results are as follows: Figure 1 shown.
[0044] Depend on Figure 1 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 1 ( Figure 1 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 1 b) In the first 5 seconds, Figure 1 b~1f represent the 1s, 2s, 3s, 4s, and 5s after the light source is removed. During this time, the afterglow brightness of the compound is strong. From the 5.5s (such as Figure 1 g) after which the afterglow gradually weakened, and there was still afterglow after 5.5s. Figure 1 h) The afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Example 1 is as high as 6.2s, and the afterglow performance is excellent.
[0045] Test Example 2: Performance Test of Materials in Comparative Example 1
[0046] Under room temperature and atmospheric environment, the crystal material of comparative example 1 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the change in the afterglow brightness of the crystal material after the light source was removed was recorded. Figure 2 shown.
[0047] Depend on Figure 2 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Comparative Example 1 ( Figure 2 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 2 b), Figure 2 b~2c represent the 0.5s and 1s after the light source is removed. During this time, the afterglow brightness of the compound is strong. Figure 2 c) and then the afterglow gradually weakened, and the afterglow at 1.5s ( Figure 2 d) The afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Comparative Example 1 is only 1.5s, and the afterglow performance is poor, which means that when the same guest material is used, if aniline compounds are used to construct the crystal material, its performance is not as good as the crystal material constructed by phosphine derivatives of the present invention.
[0048] Test Example 3: Performance Test of Materials in Comparative Example 2
[0049] Under room temperature and atmospheric environment, after exciting the crystal material of Comparative Example 2 with a 365nm ultraviolet lamp, the excitation light source is turned off, and the change in the afterglow brightness of the crystal material after the light source is removed is recorded. The results show that after exciting the crystal material of Comparative Example 2 with a 365nm ultraviolet lamp, the excitation light source is turned off. After the light source is removed, the crystal material emits a pink afterglow, but the afterglow performance is poor, the afterglow phenomenon is not obvious, and the specific afterglow time cannot be tested. It can be seen that when the same main material is used, if benzanthracene is used as the guest material instead of phenylene to prepare the crystal material, the afterglow performance of the material is significantly affected.
[0050] In summary, the long afterglow crystal material constructed with phosphine derivatives provided by the present invention has an afterglow time of up to 6s and excellent afterglow luminescence performance. It can provide new ideas for the design and synthesis of new luminescent crystal long afterglow materials, and can also provide a theoretical basis and material foundation for practical applications such as data encryption and anti-counterfeiting.
[0051] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A long afterglow crystal material constructed with phosphine derivatives, characterized in that: The main material and the guest material are prepared by evaporation and crystallization; in the long afterglow crystal material constructed with phosphine derivatives, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material; The main material is The guest material is 2. The long afterglow crystal material constructed with phosphine derivatives according to claim 1, characterized in that: The mass ratio of the host material to the guest material is (80-120):
1.
3. The long afterglow crystal material constructed with phosphine derivatives according to claim 1, characterized in that: The excitation wavelength of the long afterglow crystal material constructed with phosphine derivatives is 360-380nm.
4. A method for preparing a long afterglow crystal material constructed with phosphine derivatives as claimed in claim 1, characterized in that: The following steps are involved: (1) mixing the host material and the guest material uniformly to obtain a solid powder; (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the long afterglow crystal material constructed with the phosphine derivative.
5. The method for preparing a long afterglow crystal material constructed with phosphine derivatives according to claim 4, characterized in that: In step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1: (80-120).
6. The method for preparing a long afterglow crystal material constructed with phosphine derivatives according to claim 4, characterized in that: In step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
7. The method for preparing a long afterglow crystal material constructed with phosphine derivatives according to claim 4, characterized in that: In step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 minutes.
8. The method for preparing a long afterglow crystal material constructed with phosphine derivatives according to claim 4, characterized in that: In step (2), the temperature for standing and volatilizing is 15 to 30°C.
9. The method for preparing a long afterglow crystal material constructed with phosphine derivatives according to any one of claims 4 to 8, characterized in that: After the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
10. An application of the long afterglow crystal material constructed with phosphine derivatives as claimed in claim 1, characterized in that: Application as luminescent material in data encryption material or anti-counterfeiting material.