Compound leaching agent for electrified mining of rare earth ore
Through the compounding method and electric field effect of ammonium-free leaching agent, the problems of ammonia nitrogen pollution and excessive chloride ions in the rare earth ore with power-on mining are solved, the exchange rate and electromigration rate of rare earth ions are improved, and the soil permeability and rare earth mining are enhanced. efficiency.
Patent Information
- Application Number
- CN202411083807.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing methods of mining rare earth ores with electricity, the leaching agent exchanges the rare earth and causes ammonia nitrogen pollution, and excessive chloride ions lead to environmental pollution, and the resource extraction rate is low.
The ammonium-free leaching agent is used to combine the combination method of sodium sulfate, potassium sulfate, magnesium sulfate, ferrous sulfate and aluminum sulfate. Through the combination of monovalent and high-valent cations, combined with the action of electric fields, the rapid migration and efficient exchange of rare earth ions can be achieved. , avoid ammonia nitrogen contamination and excessive use of chloride ions.
It improves the exchange rate and electromigration rate of rare earth ions, reduces environmental pollution, enhances soil permeability and rare earth mining efficiency, and solves the problems of ammonia nitrogen pollution and low resource extraction rates.
Smart Images

Figure CN118979162A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth mining, in particular to a compound leaching agent for mining rare earth ores through electricity. Background Art
[0002] Ion-adsorbed rare earth elements are primarily found in southern my country, where the vast majority of them are adsorbed on mineral surfaces in various cationic states. Existing ammonium salt in-situ leaching processes cause significant environmental damage and low resource extraction rates.
[0003] CN109402417A proposes the use of electrochemical mining, using ammonium salt solutions as rare earth leaching solutions, including ammonium chloride, ammonium acetate, ammonium citrate or ammonium sulfate. However, this does not fundamentally solve the ammonia nitrogen pollution problem.
[0004] CN106702181A proposes the use of a mixture of one or more of ammonium sulfate, ammonium chloride, potassium chloride, magnesium sulfate, and magnesium chloride. However, ammonium salts are still used, and the ratio of the mixed salts is not clearly stated. Different mixing ratios have different effects on rare earth extraction.
[0005] CN108034842A proposes the use of one or more of magnesium sulfate, ferric chloride, and aluminum chloride. However, excessive chloride ions can cause a serious loss of cations in the soil, which can easily lead to soil compaction. Summary of the Invention
[0006] The present invention aims to address the shortcomings of the prior art by providing a composite leaching agent for electric mining of rare earth ores. By utilizing an ammonium-free leaching agent for rare earth mining, the present invention addresses the problem of ammonia nitrogen pollution caused by the leaching agent after rare earths are exchanged in existing electric mining methods. Furthermore, the composite leaching agent provides a high ion exchange rate and high electrical migration rate, while effectively avoiding environmental pollution caused by excessive chloride ion use.
[0007] The present invention adopts the following technical solutions:
[0008] A compound leaching agent for electric mining of rare earth ores, wherein the leaching agent for electric mining of rare earth ores comprises sodium sulfate, potassium sulfate, magnesium sulfate, ferrous sulfate, ferric sulfate and aluminum sulfate;
[0009] The mass ratio of monovalent cation and high-valent (divalent or trivalent) cation leaching agent is 1:8;
[0010] The mass ratio of the monovalent cation, divalent cation and trivalent cation leaching agents is 1:4:4.
[0011] A method for using a compound leaching agent for electric mining of rare earth ores. After the above-mentioned leaching agent soaks the weathering crust for a period of time, an electric field is applied to the anode and cathode after ensuring that the cations exchange the rare earth ions. Under the action of the electric field force, the freely moving rare earth ions can quickly migrate to the cathode, saving leaching time while avoiding the ammonia nitrogen pollution problem caused by the use of ammonium salts.
[0012] In some examples, the amount of leaching agent used is twice the total mass of the rare earth oxides. The total mass of the rare earth oxides is obtained by sampling at different locations and depths, measuring the mass fraction of rare earth oxides in each sample, and then calculating the average value, which is then multiplied by the mass of the ore body.
[0013] In some examples, the mass concentration of the leaching agent is 1.0 wt% to 2.0 wt%.
[0014] In some examples, a method for mining rare earths using a compound leaching agent for electrified mining of rare earth ores comprises arranging at least two rows and at least two columns of injection holes in a mining area, and arranging conductive injection pipes in the injection holes; connecting N (N≥1, N is a positive integer) conductive injection pipes in the same row in parallel and then connecting them to an electrified control system according to the current when each conductive injection pipe is energized; adding a leaching agent to the injection holes, and applying direct current between the conductive injection pipes using the electrified control system; applying a voltage to the anode and the cathode so that the voltage gradient in the ore body is 10-60V / m.
[0015] Beneficial effects of the present invention:
[0016] 1. There are cations of different valences in the compound leaching agent. There is a difference in the electrochemical behavior of ions of different valences in the electric field environment. The exchange capacity of high-valent ions and rare earth ions is strong. The use of high-valent ion solution with appropriate concentration ensures complete exchange of rare earths. Considering cost and safety issues, the present invention uses the extractant ion with the highest valence of trivalent. The migration ability of monovalent ions in the soil environment is relatively strong. Monovalent ions can enhance the conductivity of soil aqueous solution, thereby promoting electromigration and electroosmosis, accelerating the flow of rare earth ions and leachate, and improving the permeability of difficult-to-mining areas, thereby improving rare earth mining efficiency. The use of a monovalent leaching agent and a high-valent leaching agent is suitable for rare earth electric drive mining. It can not only ensure the rare earth ion exchange leaching efficiency, but also adjust the current size and improve the rare earth ion migration efficiency. It has the advantages of high rare earth recovery rate and short mining cycle, and is particularly suitable for difficult-to-permeate mining areas.
[0017] 2. Compound leaching agents solve the problem of ammonia nitrogen pollution and avoid the environmental damage caused by excessive use of single cationic leaching agents. A concentration range of 1.0wt% to 2.0wt% is suitable. Too high a concentration will cause the leaching agent ions to become the primary contributors to the current. Too low a concentration will reduce the exchange capacity for rare earth ions.
[0018] 3. According to the different migration principles of different ions, electricity is applied to promote the seepage and staged accumulation of the compound leaching agent, thereby preventing rare earth from being adsorbed back by the soil.
[0019] 4. Compared with CN106702181A, the present invention selects leaching agent cations not only based on exchange activity but also based on the permeability under current and electric field conditions, and selects the leaching agent cations with the best electromigration and electroosmosis under coupled electric field conditions.
[0020] 5. Compared with CN108034842A, the leaching agents selected in the present invention are all sulfate solutions, which effectively avoid the environmental impact caused by excessive chloride ions. Moreover, sulfate at the same concentration has a stronger exchange capacity for rare earth than chloride. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Graph showing the current changes of Example 1, Comparative Example 1 and Comparative Example 2;
[0022] Figure 2 Graph showing the relationship between rare earth elements in the leachate of Example 1, Comparative Example 1, and Comparative Example 2 and time;
[0023] Figure 3 Graph showing the current changes of Example 2, Comparative Example 3 and Comparative Example 4;
[0024] Figure 4 The relationship between rare earth and time in the leachate of Example 2, Comparative Example 3 and Comparative Example 4;
[0025] Figure 5 Graph showing the current changes of Example 3, Comparative Example 5, Comparative Example 6, and Comparative Example 7;
[0026] Figure 6 The relationship between rare earth and time in the leachate of Example 3 and Comparative Examples 5, 6 and 7;
[0027] Figure 7 It is a flow chart of the steps of the present invention. DETAILED DESCRIPTION
[0028] To make the objectives, technical solutions, and advantages of the present invention more clear, the technical solutions of the present invention are described clearly and completely below. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0029] like Figure 7 As shown, the method for mining rare earth using a composite leaching agent for mining rare earth ores by electricity of the present invention comprises:
[0030] Arrange at least two rows and at least two columns of injection holes in the mining area, and arrange conductive injection pipes in the injection holes; connect N (N≥1, N is a positive integer) conductive injection pipes in the same row in parallel and then connect them to the power control system respectively according to the current when each conductive injection pipe is energized;
[0031] Adding a leaching agent into the injection hole, and then applying a direct current between the conductive injection pipes using an electrical control system;
[0032] The leaching agent comprises two or more different valence states selected from sodium sulfate, potassium sulfate, magnesium sulfate, ferrous sulfate, ferric sulfate and aluminum sulfate.
[0033] At least two rows of injection holes are arranged in the mining area. The number of rows of injection holes can be three, four, five, or even 1,000 rows. The number of rows of injection holes is determined by the area of the mining area. The spacing between each row of injection holes is 0.5-3 meters, and can be 0.5 meters, 1 meter, 2 meters, or 3 meters. The reason for having at least two rows of injection holes is that at least two rows of conductive injection pipes are required to form a set of positive and negative electrodes for electric mining.
[0034] A conductive liquid injection tube is arranged in the liquid injection hole, and the conductive liquid injection tube can be made of metal or non-metallic material. The present invention does not limit the number of anodes and cathodes.
[0035] In which, a leaching agent is added to the injection hole, and then a power-on control system is used to apply direct current between the conductive injection tubes; a voltage is generated between the conductive injection tubes, and a current is formed under the action of the leaching liquid. Under the action of the current, the rare earth ions replaced by the leaching agent can flow quickly to the cathode, thereby accelerating the migration rate of the rare earth ions and saving rare earth mining time.
[0036] When a voltage is applied between the two electrodes, rare earth ions in the soil undergo directional migration under the action of the electric field. Based on experimental results, a voltage gradient of 10-60V / m within the ore body favors the flow of rare earth ions toward the cathode. The voltage gradient within the ore body can be 10V / m, 20V / m, 50V / m, 60V / m, and so on.
[0037] It is understandable that in the embodiments of the present application, a voltage may be applied between the anode and the cathode according to actual conditions so that the voltage gradient in the ore body is within other ranges.
[0038] As an example, the leaching agent includes two or more of sodium sulfate, potassium sulfate, magnesium sulfate, ferrous sulfate, ferric sulfate and aluminum sulfate.
[0039] The following is the formula for the current in porous media
[0040]
[0041] The system current is related to the ion concentration, charge, diffusion coefficient and the size of the applied electric field. The monovalent ions have a larger diffusion coefficient and are more likely to break away from the electrostatic attraction of the soil, generating a higher current and promoting migration. High-valent ions have a strong exchange capacity with rare earth ions.
[0042] The diffusion coefficient of the ion is given by:
[0043]
[0044] There are differences in the chemical behaviors of leaching agent cations in natural leaching and electric leaching. The mobility of monovalent ions with relatively strong migration ability is greatly improved under the action of the electric field, and their exchange capacity is weakened. The migration ability of high-valent ions is also enhanced due to soil adsorption, but if it is controlled within a reasonable voltage gradient range, its exchange capacity will be improved.
[0045] The results of a large number of previous experimental studies have shown that under the action of an electric field, the mixed ions promote each other in the leaching of rare earths: the mass ratio of monovalent ions to high-valent cations is 1:8 (monovalent ions to divalent ions; or monovalent ions to trivalent ions);
[0046] Or 1:4:4 can ensure that the rare earth is completely exchanged (monovalent ions: divalent ions: trivalent ions).
[0047] As mentioned above, the present invention provides a fixed-ratio compound leaching agent for electric mining of rare earth ores, which is suitable for the above-mentioned method for electric mining of rare earth ores.
[0048] The features and performance of the present invention are further described in detail below with reference to the embodiments.
[0049] Example 1 Simulating the mining of rare earths by electrification in the laboratory
[0050] A cylindrical device was used to simulate the electric mining of ion adsorption rare earth ore. First, 400g of simulated weathering crust sample was added to the cylindrical tube and compressed to 9.5cm, so that the compaction density was 1.489g / cm 3 200 mL of a 0.1 mol / L solution of potassium sulfate and magnesium sulfate (at a mass ratio of 1:8) was added to the simulated weathering crust sample. After complete wetting, deionized water was continuously added at a rate of 0.4 mL / min. Graphite electrodes were applied to the top and bottom of the cylindrical device and a 40 V / m DC power supply was applied. The cathode continuously received the leachate and the amount of rare earth and leachant ions in the collected solution was recorded over time.
[0051] Comparative Example 1
[0052] The difference between Comparative Example 1 and Example 1 is that 200 mL of potassium sulfate with a molar concentration of 0.1 mol / L was added to the simulated weathering crust sample.
[0053] After complete wetting, ensure that potassium ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of potassium ions in the soil, preventing rare earths from being adsorbed by the soil. Figure 2 As shown, the rare earth leaching rate is 65%.
[0054] Comparative Example 2
[0055] The difference between Comparative Example 2 and Example 1 is that 200 mL of magnesium sulfate with a molar concentration of 0.1 mol / L was added to the simulated weathering crust sample.
[0056] After complete wetting, ensure that magnesium ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of magnesium ions in the soil, preventing rare earths from being adsorbed by the soil. Figure 2 As shown, the rare earth leaching rate is 75%.
[0057] Experimental conclusion:
[0058] For the system with potassium sulfate and magnesium sulfate mixed solution, the system current and the rare earth ion content in the collected solution change with the power-on time as shown in the following figure: Figure 1 and Figure 2 As shown, the rare earth recovery rate of magnesium sulfate is 75%, the rare earth recovery rate of potassium sulfate is 65%, and the rare earth recovery rate of the composite solution is 88%. It can be considered that the monovalent ions promote the exchange of divalent ions for rare earths and at the same time increase the current to promote the migration of rare earth ions.
[0059] like Figure 1 As shown, the current of the three experimental systems changes with the power-on time. As can be seen from Example 1 and Comparative Example 1, compared with the single sulfate solution used as the leaching agent in Comparative Examples 1 and 2, the current in Example 1, which incorporates potassium sulfate and magnesium sulfate as leaching agents, remains higher for a longer period of time under the same voltage gradient, injection rate, and concentration conditions, indirectly reflecting that the composite leaching agent improves rare earth recovery.
[0060] like Figure 2 As shown in Figure 1, the relationship between rare earth ions in the leachate of Example 1, Comparative Example 1 and Comparative Example 2 and time. Figure 2 It can be seen that the amount of rare earth in the leachate of Example 1 is significantly higher than that of Comparative Example 1, indicating that the potassium sulfate and magnesium sulfate compound solution improves the leaching efficiency of rare earth ions in the soil.
[0061] Example 2
[0062] The difference between this embodiment and embodiment 1 is that after the weathering crust sample is compressed, 200 mL of sodium sulfate and aluminum sulfate with a molar concentration of 0.1 mol / L are added to the device, and the composite mass ratio is 1:8.
[0063] For the system with sodium sulfate and aluminum sulfate mixed solution, the system current and the rare earth ion content in the collected solution change with the power-on time as shown in the following figure: Figure 3 and Figure 4 As shown, the rare earth recovery rate of the composite solution is 95%.
[0064] Comparative Example 3
[0065] The difference between Comparative Example 3 and Example 2 is that after the weathering crust sample is compressed, 200 mL of sodium sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0066] After complete wetting, ensure that sodium ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of sodium ions in the soil, preventing rare earths from being adsorbed by the soil. Figure 4 As shown, the rare earth leaching rate of sodium sulfate is 12%.
[0067] Comparative Example 4
[0068] The difference between this comparative example 4 and example 2 is that after the weathering crust sample is compressed, 200 mL of aluminum sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0069] After complete wetting, ensure that aluminum ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of aluminum ions in the soil, preventing rare earth ions from being reversely adsorbed by the soil. Figure 4 As shown in the figure, the rare earth leaching rate of aluminum sulfate is 93%. Compared with the compound leaching agent, the rare earth leaching rate using only aluminum sulfate is slightly lower. It is possible that the presence of other cations promotes the exchange of high-valent ions for rare earth ions.
[0070] like Figure 3 As shown, the current of the three experimental systems changes with the power-on time. In Example 2, aluminum sulfate and sodium sulfate were added as leaching agents. Under the same voltage gradient, injection rate and concentration conditions, the current maintained a high value for a longer time.
[0071] like Figure 4 As shown in Figure 2, the relationship between rare earth ions in the leachate of Example 2, Comparative Example 3 and Comparative Example 4 and time. Figure 4 It can be seen that the amount of rare earth in the leachate of Example 2 is significantly higher than that of Comparative Example 3, indicating that the aluminum sulfate and sodium sulfate composite solution improves the leaching efficiency of rare earth ions in the soil.
[0072] Example 3
[0073] The difference between this embodiment and embodiment 1 is that after the weathering crust sample is compressed, 200 mL of sodium sulfate, magnesium sulfate and aluminum sulfate with a molar concentration of 0.1 mol / L are added to the device, and the composite mass ratio is 1:4:4.
[0074] The system with sodium sulfate, magnesium sulfate and aluminum sulfate mixed solution added, the system current and the rare earth ion content in the collected solution change with the power-on time as shown in the following figure: Figure 5 and Figure 6 As shown, the rare earth recovery rate of the composite solution is 95%.
[0075] Comparative Example 5
[0076] The difference between Comparative Example 5 and Example 3 is that after the weathering crust sample is compressed, 200 mL of sodium sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0077] After complete wetting, ensure that sodium ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of sodium ions in the soil, preventing rare earths from being adsorbed by the soil. Figure 6 As shown, the rare earth leaching rate of sodium sulfate is 12%.
[0078] Comparative Example 6
[0079] The difference between Comparative Example 6 and Example 3 is that after the weathering crust sample is compressed, 200 mL of magnesium sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0080] After complete wetting, ensure that magnesium ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of magnesium ions in the soil, preventing rare earths from being adsorbed by the soil. Figure 6 As shown, the rare earth leaching rate of magnesium sulfate is 48%.
[0081] Comparative Example 7
[0082] The difference between this comparative example 7 and example 3 is that after the weathering crust sample is compressed, 200 mL of aluminum sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0083] After complete wetting, ensure that aluminum ions and rare earth ions are fully exchanged, and then continue to add deionized water at 0.4mL / min. Graphite electrode plates are applied to the upper and lower parts of the cylindrical device and a 40V / m DC power supply is connected. Under the action of the electric field, the migration of mobile rare earth ions is promoted, saving mining time. The applied current can also promote the migration and enrichment of aluminum ions in the soil, preventing rare earth ions from being reversely adsorbed by the soil. Figure 6 As shown in the figure, the rare earth leaching rate of aluminum sulfate is 93%. Compared with the compound leaching agent, the rare earth leaching rate using only aluminum sulfate is slightly lower. It is possible that the presence of other cations promotes the exchange of high-valent ions for rare earth ions.
[0084] exist Figure 5 By comparing Example 3 with Comparative Example 5, Comparative Example 6 and Comparative Example 7, it can be seen that in Example 3, a leaching agent with a compound mass ratio of 1:4:4 is added. Under the conditions of the same voltage gradient, injection rate and concentration, the current maintains a high value for a longer time, which indirectly reflects that the compound leaching agent improves the rare earth recovery rate.
[0085] from Figure 6 It can be seen that the amount of rare earth in the leachate of Example 3 is significantly higher than that of Comparative Example 5, indicating that the composite solution improves the leaching efficiency of rare earth ions in the soil.
[0086] Example 4
[0087] The difference between this embodiment and embodiment 1 is that:
[0088] After the weathering crust sample is compressed, 200 mL of sodium sulfate, ferrous sulfate and ferric sulfate with a molar concentration of 0.1 mol / L are added to the device, and the composite mass ratio is 1:4:4.
[0089] The simulated electrification mining experiment was carried out for 100 hours, and the rare earth recovery rate was 95%.
[0090] Comparative Example 8
[0091] The difference between Comparative Example 8 and Example 4 is that after the weathering crust sample is compressed, 200 mL of sodium sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0092] The simulated electrification mining experiment was carried out for 100 hours, and the rare earth recovery rate was 25%.
[0093] Comparative Example 9
[0094] The difference between this comparative example 9 and example 4 is that after the weathering crust sample is compressed, 200 mL of ferrous sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0095] The simulated electrification mining experiment was carried out for 100 hours, and the rare earth recovery rate was 85%.
[0096] Comparative Example 10
[0097] The difference between Comparative Example 10 and Example 4 is that after the weathering crust sample is compressed, 200 mL of ferric sulfate with a molar concentration of 0.1 mol / L is added to the device.
[0098] The simulated electrification mining experiment was carried out for 100 hours, and the rare earth recovery rate was 90%.
[0099] From the above, it can be seen that in the method provided by the embodiment of the present invention, the compound leaching agent significantly improves the rare earth recovery rate.
[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present invention.
Claims
1. A composite leaching agent for mining rare earth ores by electricity, characterized in that: The leaching agent for mining rare earth ores by electricity includes sodium sulfate, potassium sulfate, magnesium sulfate, ferrous sulfate, ferric sulfate and aluminum sulfate; Among them, the mass ratio of monovalent cation to divalent cation or monovalent ion to trivalent cation leaching agent is 1:8; Or the mass ratio of monovalent cation, divalent cation and trivalent cation leaching agents is 1:4:
4.
2. The composite leaching agent for mining rare earth ores by electricity according to claim 1, characterized in that: The mass concentration of the leaching agent is 1.0wt% to 2.0wt%.
3. The composite leaching agent for mining rare earth ores by electricity according to claim 1, characterized in that: The dosage of the leaching agent is twice the total mass of the rare earth oxides.
4. A method for mining rare earth using a composite leaching agent for mining rare earth ores by powering on as claimed in claim 1, characterized in that: When in use, the leaching agent soaks the weathering crust for a period of time to ensure that the cations exchange the rare earth ions before applying the electric field to the anode and cathode.
5. A method for mining rare earth using the composite leaching agent for mining rare earth ores by electricity as claimed in claim 1, characterized in that: At least 2 rows and at least 2 columns of injection holes are arranged in the mining area, and conductive injection pipes are arranged in the injection holes; according to the current size when each conductive injection pipe is energized, N conductive injection pipes in the same row are connected in parallel to the power-on control system respectively, N≥1, N is a positive integer; leaching agent is added to the injection holes, and direct current is applied between the conductive injection pipes using the power-on control system; voltage is applied to the anode and the cathode so that the voltage gradient in the ore body is 10-60V / m.
Citation Information
Patent Citations
Ion-adsorption-type rare earth extracting method
CN103266224A
Leaching agent used for leaching rare earth in ion-adsorption type rare earth ore and leaching method
CN105483373A
Method for synergistically leaching ion adsorption type rare earth by using aluminum salt and low-valence inorganic salt
CN117626007A
Process for purifying rare-earth compositions
EP0014553A1
Extraction method for ion-adsorbed rare earths
WO2022033041A1