Manufacturing method of novel aluminum alloy strip for battery protection

By optimizing the composition and processing technology of aluminum alloy strip, the problems of easy cracking and poor burst resistance of aluminum alloy strip in stamping were solved, realizing the manufacturing of aluminum alloy strip with high plasticity and high strength, which is suitable for battery protection.

CN118979164AActive Publication Date: 2024-11-19NORTHEAST LIGHT ALLOY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411049671.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing aluminum alloy strips are prone to cracking during stamping and have poor burst resistance, which cannot meet the high performance and protection requirements of new energy vehicles.

Method used

By optimizing the content of major and trace elements, adding V element, and combining rolling and annealing treatments, fine grain strengthening and substructure strengthening are formed to prepare a new type of aluminum alloy strip.

Benefits of technology

It improves the plastic forming performance and burst resistance of aluminum alloy strip, meets the high forming and protection requirements of new energy vehicles, is less prone to cracking during stamping, and significantly improves tensile strength and elongation after fracture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979164A_ABST
    Figure CN118979164A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a novel aluminum alloy strip for battery protection, and belongs to the field of aluminum alloy processing. The problems that an existing aluminum alloy strip is prone to cracking and poor in blasting resistance during punch forming are solved. The method comprises the steps of 1, preparing a square cast ingot blank; 2, heating and rolling into a thin plate of 0.2 mm; and 3, annealing and slitting to obtain a strip with the width of 50-60mm. The prepared novel alloy is annealed after being rolled, the requirement of a battery protection product for the plastic forming performance of the novel alloy strip is met, and the prepared aluminum alloy strip is excellent in plasticity and structure in industrial production. After the strip is subjected to annealing heat treatment, a more uniform recrystallization structure is obtained, and the grain size is ideal to control, so that the alloy strip has relatively good plastic forming capability, is beneficial to processing forming and protection performance improvement of a battery protection product, is not easy to crack after punch forming, and is high in explosion resistance; and the requirements of a novel battery on high forming performance and protection of the aluminum alloy strip are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of aluminum alloy processing, and in particular relates to a method for manufacturing a novel aluminum alloy strip for battery protection. Background Art

[0002] Aluminum alloy battery protection sheet is an aluminum alloy sheet that is resistant to strong ultrasonic impact and can effectively prevent battery explosion. It is mainly used in power batteries and energy storage batteries, especially in new energy vehicles. With the rapid development of new energy power locomotives in my country, the requirements for safety hazards and protection are very stringent, and the requirements for the material's anti-explosion performance and forming performance are getting higher and higher. However, the existing commonly used aluminum alloy strips for battery protection still have low plasticity, which leads to easy cracking during stamping and poor anti-explosion performance, and cannot meet the high performance and protection requirements of new energy vehicles. Summary of the invention

[0003] The purpose of the present invention is to provide a method for manufacturing a novel aluminum alloy strip for battery protection, so as to solve the problem that the existing aluminum alloy strip is easy to crack and has poor anti-explosion performance during stamping.

[0004] A method for manufacturing a novel aluminum alloy strip for battery protection is carried out according to the following steps:

[0005] 1. Billet preparation:

[0006] The composition of the billet is as follows: Fe: 1.0% to 1.6%, Mn: 0.2% to 0.6%, Ti: 0.01% to 0.1%, V: 0.03% to 0.15% and the balance Al, and then the raw materials are weighed according to the billet composition and smelted, and then a semi-continuous casting method is used to prepare a square ingot billet;

[0007] 2. Heating and rolling:

[0008] The square ingot was placed in a resistance heating furnace for heating, and then rolled at room temperature on a two-roll hot rolling mill to obtain a thin plate with a thickness of 0.2 mm.

[0009] 3. Annealing and slitting:

[0010] The above-mentioned thin plate with a thickness of 0.2 mm is placed in an air cushion heating furnace and heated at 400°C for 60-90s to obtain an annealed thin plate. After cleaning, it is cut into strips with a width of 50 to 60 mm, thus completing the manufacture of the new aluminum alloy strip for battery protection.

[0011] Furthermore, in step 1, the composition of the blank is as follows: Fe: 1.5%, Mn: 0.3%, Ti: 0.05%, V: 0.1% and the balance Al in terms of mass percentage.

[0012] Furthermore, the size of the Chinese ingot in step 1 is: thickness 500 mm, width 1200 mm.

[0013] Furthermore, the heating in step 2 is: heating at 600° C. for 5 h to 20 h, then cooling to 450° C. to 500° C. at a rate of 10 to 50° C. / h, and then heating for 5 h to 20 h.

[0014] Furthermore, the room temperature rolling in step 2: at room temperature, it is rolled on a two-roll hot rolling mill for 10 to 20 passes to a thickness of 5 mm, and after curling, it is continued to be rolled on a two-roll cold rolling mill at room temperature, and then rolled to a thickness of 0.2 mm through 2 to 5 passes.

[0015] Furthermore, the operating speed of the air cushion heating furnace in step three is 20 to 30 m / s.

[0016] Furthermore, the slitting in step three is performed using a precision shearing machine.

[0017] Beneficial effects of the present invention:

[0018] 1. Based on the original 8 series aluminum alloy, the present invention optimizes the content of main elements and trace elements, adds V elements that improve superplasticity to form a new alloy, and performs annealing after rolling. By means of fine grain strengthening, substructure strengthening and deformation strengthening, the plastic forming performance requirements of the new alloy strip for battery protection products are met. The prepared aluminum alloy strip has excellent plasticity and organization in industrial production.

[0019] 2. The present invention adopts V and Ti elements to refine the grains, improve plasticity, and facilitate forming. At the same time, rolling deformation and annealing treatment are adopted to control the grain size of the alloy strip and greatly improve the plasticity. After annealing heat treatment, the strip obtains a more uniform recrystallization structure, and the grain size is ideally controlled, so that the alloy strip has good plastic forming ability, which is conducive to the processing and forming of battery protection products and the improvement of protection performance. Stamping is not easy to crack, and the anti-explosion performance is strong, which meets the high forming performance and protection requirements of new batteries for aluminum alloy strips.

[0020] 3. The tensile strength of the 0.2mm thick strip in the O state tested according to GB / T16865 "Specimens and methods for tensile testing of deformed aluminum, magnesium and their alloy products" is 106-112MPa, the yield strength is 57-71MPa, and the elongation after fracture is 45-53%, which is 22.5% higher than the plasticity of 8014 aluminum alloy strip; the stamping blasting value at room temperature is 5.0-5.5MPa, which is more than 17% higher than that of 8014 aluminum alloy strip.

[0021] The invention is suitable for manufacturing aluminum alloy strips for battery protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The recrystallization structure diagram of the strip prepared in the example. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0024] Specific implementation method 1: This implementation method is a method for manufacturing a novel aluminum alloy strip for battery protection, which is carried out according to the following steps:

[0025] 1. Billet preparation:

[0026] The composition of the billet is as follows: Fe: 1.0% to 1.6%, Mn: 0.2% to 0.6%, Ti: 0.01% to 0.1%, V: 0.03% to 0.15% and the balance Al, and then the raw materials are weighed according to the billet composition and smelted, and then a semi-continuous casting method is used to prepare a square ingot billet;

[0027] 2. Heating and rolling:

[0028] The square ingot was placed in a resistance heating furnace for heating, and then rolled at room temperature on a two-roll hot rolling mill to obtain a thin plate with a thickness of 0.2 mm.

[0029] 3. Annealing and slitting:

[0030] The above-mentioned thin plate with a thickness of 0.2 mm is placed in an air cushion heating furnace and heated at 400°C for 60-90s to obtain an annealed thin plate. After cleaning, it is cut into strips with a width of 50 to 60 mm, thus completing the manufacture of the new aluminum alloy strip for battery protection.

[0031] In step 1 of this embodiment, there are some inevitable impurity elements in the blank composition, and the impurity content is less than 0.001%.

[0032] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the blank composition in step 1 is as follows: Fe: 1.5%, Mn: 0.3%, Ti: 0.05%, V: 0.1% and the balance Al. The other steps and parameters are the same as those in specific embodiment 1.

[0033] Specific implementation method 3: This implementation method is different from specific implementation method 1 in that the blank composition in step 1 is as follows: Fe: 1.4%, Mn: 0.4%, Ti: 0.05%, V: 0.12% and the balance Al. The other steps and parameters are the same as those in specific implementation method 1.

[0034] Specific implementation method 4: This implementation method is different from the specific implementation method 1 in that the size of the square ingot in step 1 is: thickness 500 mm, width 1200 mm. The other steps and parameters are the same as those in the specific implementation method 1.

[0035] Specific embodiment 5: This embodiment is different from specific embodiment 1 in that the heating in step 2 is: heating at 600°C for 5h to 20h, then cooling to 450°C to 500°C at a rate of 10 to 50°C / h, and then heating for 5h to 20h. Other steps and parameters are the same as those in specific embodiment 1.

[0036] Specific embodiment 6: This embodiment is different from specific embodiment 5 in that the heating in step 2 is: heating at 600°C for 10 hours, then cooling to 480°C at a rate of 20°C / h, and heating for another 10 hours. Other steps and parameters are the same as those in specific embodiment 5.

[0037] Specific embodiment 7: This embodiment is different from specific embodiment 1 in that the room temperature rolling in step 2 is: at room temperature, it is rolled to a thickness of 5 mm through 10 to 20 passes on a two-roll hot rolling mill, and then rolled to a thickness of 0.2 mm through 2 to 5 passes on a two-roll cold rolling mill after curling. The other steps and parameters are the same as those in specific embodiment 1.

[0038] Specific embodiment eight: This embodiment differs from specific embodiment seven in that the room temperature rolling in step two is: at room temperature, the steel sheet is rolled to a thickness of 5 mm through 15 passes on a two-roll hot rolling mill, and then rolled to a thickness of 0.2 mm through 4 passes on a two-roll cold rolling mill after curling. The other steps and parameters are the same as those of specific embodiment seven.

[0039] Specific implementation method 9: This implementation method is different from specific implementation method 1 in that the running speed of the air cushion type heating furnace in step 3 is 20-30 m / s. The other steps and parameters are the same as those in specific implementation method 1.

[0040] Specific implementation method 10: This implementation method is different from the specific implementation method 1 in that the slitting in step 3 is performed using a fine shearing machine. The other steps and parameters are the same as those in the specific implementation method 1.

[0041] The beneficial effects of the present invention are verified by the following examples:

[0042] Example:

[0043] A method for manufacturing a novel aluminum alloy strip for battery protection is carried out according to the following steps:

[0044] 1. Billet preparation:

[0045] The composition of the billet is as follows: Fe: 1.5%, Mn: 0.3%, Ti: 0.05%, V: 0.1% and the balance Al, and then the raw materials are weighed according to the billet composition and smelted, and then the square ingot billet is prepared by a semi-continuous casting method;

[0046] 2. Heating and rolling:

[0047] The square ingot was placed in a resistance heating furnace for heating, and then rolled at room temperature on a two-roll hot rolling mill to obtain a thin plate with a thickness of 0.2 mm.

[0048] 3. Annealing and slitting:

[0049] The above-mentioned thin plate with a thickness of 0.2 mm is placed in an air cushion heating furnace and heated at 400°C for 70 seconds to obtain an annealed thin plate. After cleaning, it is cut into strips with a width of 55 mm, thus completing the manufacture of the new aluminum alloy strip for battery protection.

[0050] In step 1 of this embodiment, the composition of the blank is as follows: Fe: 1.5%, Mn: 0.3%, Ti: 0.05%, V: 0.1% and the balance Al in terms of mass percentage.

[0051] The dimensions of the square ingot in step 1 of this embodiment are: thickness 500 mm, width 1200 mm.

[0052] The heating in step 2 of this embodiment is as follows: heating at 600° C. for 10 h, then cooling to 480° C. at a rate of 20° C. / h, and heating for another 10 h.

[0053] The room temperature rolling in step 2 of this embodiment is as follows: at room temperature, the steel sheet is rolled on a two-roll hot rolling mill through 15 passes to a thickness of 5 mm, and then, after curling, it is continuously rolled on a two-roll cold rolling mill at room temperature and then rolled on a two-roll cold rolling mill through 4 passes to a thickness of 0.2 mm.

[0054] The operating speed of the air cushion heating furnace described in step three of this embodiment is 25m / s.

[0055] The slitting described in step three of this embodiment uses a precision shearing machine.

[0056] The 55 mm wide strip prepared in this embodiment is in O state and 0.2 mm thick. It is tested according to GB / T16865 "Test specimens and methods for tensile testing of deformed aluminum, magnesium and their alloy products". The tensile strength is 110 MPa, the yield strength is 62 MPa, and the elongation after fracture is 49%, which is 22.5% higher than that of 8014 aluminum alloy strip at room temperature. The recrystallized grain size in the strip structure is relatively small (such as Figure 1 The stamping burst value is increased by more than 17% compared with 8014 aluminum alloy strip.

[0057] Table 1 0.2mm thickness strip performance comparison table

[0058]

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a novel aluminum alloy strip for battery protection, characterized in that It proceeds as follows:

1. Billet preparation: The composition of the billet is as follows: Fe: 1.0% to 1.6%, Mn: 0.2% to 0.6%, Ti: 0.01% to 0.1%, V: 0.03% to 0.15% and the balance Al, and then the raw materials are weighed according to the billet composition and smelted, and then a semi-continuous casting method is used to prepare a square ingot billet; 2. Heating and rolling: The square ingot was placed in a resistance heating furnace for heating, and then rolled at room temperature on a two-roll hot rolling mill to obtain a thin plate with a thickness of 0.2 mm.

3. Annealing and slitting: The above-mentioned thin plate with a thickness of 0.2 mm is placed in an air cushion heating furnace and heated at 400°C for 60-90s to obtain an annealed thin plate. After cleaning, it is cut into strips with a width of 50 to 60 mm, thus completing the manufacture of the new aluminum alloy strip for battery protection.

2. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that In step 1, the composition of the blank is as follows: Fe: 1.5%, Mn: 0.3%, Ti: 0.05%, V: 0.1% and the balance Al according to the mass percentage.

3. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that In step 1, the composition of the blank is as follows: Fe: 1.4%, Mn: 0.4%, Ti: 0.05%, V: 0.12% and the balance Al according to the mass percentage.

4. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that The size of the Chinese ingot in step 1 is: thickness 500mm, width 1200mm.

5. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that The heating in step 2 is as follows: heating at 600° C. for 5 h to 20 h, then cooling to 450° C. to 500° C. at a rate of 10 to 50° C. / h, and then heating for 5 h to 20 h.

6. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 5, characterized in that The heating in step 2 is as follows: heating at 600°C for 10 h, then cooling to 480°C at a rate of 20°C / h, and further heating for 10 h.

7. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that The room temperature rolling in step 2: at room temperature, the steel sheet is rolled on a two-roll hot rolling mill for 10 to 20 passes to a thickness of 5 mm, and then rolled on a two-roll cold rolling mill for 2 to 5 passes to a thickness of 0.2 mm.

8. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 7, characterized in that The room temperature rolling in step 2: at room temperature, the steel sheet is rolled on a two-roll hot rolling mill through 15 passes to a thickness of 5 mm, and then rolled on a two-roll cold rolling mill at room temperature after curling, and then rolled on a two-roll cold rolling mill through 4 passes to a thickness of 0.2 mm.

9. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that The operating speed of the air cushion heating furnace in step three is 20 to 30 m / s.

10. The method for manufacturing a novel aluminum alloy strip for battery protection according to claim 1, characterized in that The slitting described in step 3 is performed using a precision shearing machine.

Citation Information

Patent Citations

  • Manufacturing method for high-quality double-zero foil aluminum alloy slab ingot

    CN109536786A

  • Aluminum alloy sheet for battery lid for forming integrated explosion prevention valve, and method for producing same

    CN111212925A

  • Aluminum alloy, and electroconductive member, battery member, fastener component, spring component, structural component and cabtyre cable using same

    CN113039302A

  • Method for preparing explosion-proof sheet and flip sheet of battery cover plate from 8xxx aluminum alloy strip

    CN113403506A

  • Manufacturing method of aluminum alloy strip for energy storage shell