Marine work steel with low yield ratio and high toughness and preparation method thereof
Through low C, medium and low Ni, Cr+Mo+V+Cu microalloyation and quenching + tempering heat treatment, the problem of the increase in the yield and strength ratio of marine steel when increasing the strength is solved, and high strength and toughness are achieved. and good low-temperature toughness improves production efficiency and reduces energy consumption.
Patent Information
- Application Number
- CN202411379694.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-30
AI Technical Summary
While the existing marine steel increases the yield and strength ratio while increasing the strength ratio, resulting in a decrease in plasticity and safety. It also has a large energy consumption and low production efficiency during the production process, making it difficult to achieve a low yield and strength ratio on the basis of maintaining high strength. Good low temperature toughness.
The composition design of low C, medium and low Ni, Cr+Mo+V+Cu microalloy is adopted. Through quenching + tempering heat treatment, the formation of carbides is controlled, the grains are refined, the soft and hard ratio is regulated, and the fine dispersed distribution is formed. The precipitation phase hinders the growth of grains, improves the strength and toughness of the material, and reduces the yield-strength ratio.
A high-strength toughness and low yield strength steel plate with a yield strength of 690MPa or above and a low temperature toughness value of -40℃ or above is achieved. It has good mechanical properties and low temperature toughness, which reduces production costs and improves production efficiency.
Smart Images

Figure CN118979195A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and specifically relates to a low-yield ratio high-strength and toughness marine engineering steel and a preparation method thereof. Background Art
[0002] Marine engineering steel is used in fields such as shipbuilding and marine engineering, and is an important material for manufacturing marine equipment. The service environment of marine engineering platforms is harsh. Not only must we consider the influence of multiple factors such as strong winds, surges, tides, ice collisions, earthquakes, etc., but we must also consider adapting to various sea conditions. The changeable and complex marine service environment determines that marine engineering steel must have high strength, high toughness, fatigue resistance, lamellar tearing resistance, good weldability, seawater corrosion resistance, and good cold processing properties. At the same time, in the application process of high-strength marine engineering steel, as the strength increases, the material's yield strength ratio will continue to increase, the plasticity will decrease, and the safety will decrease. Therefore, marine engineering steel must ensure a low yield strength ratio and maintain good low-temperature toughness on the basis of maintaining a high strength.
[0003] Patent CN114480960A discloses "a low-yield ratio, low-temperature toughness 800MPa grade high-strength steel and its production process". It adopts ultra-low C, high Mn and Cr content, Mo, B, Ti alloying, and no Ni and V addition. The TMCP+tempering process is used to achieve a yield strength of 690 level. The steel plate thickness reaches 25-30mm, the yield strength is ≥690MPa, the tensile strength is ≥770-910MPa, the -40℃ longitudinal low-temperature impact energy is ≥180J, and the yield ratio is in the range of 0.88-0.89.
[0004] Patent CN116219318A discloses "a low yield ratio, ultra-low temperature toughness, extra-thick marine engineering steel plate and its manufacturing method", which adopts a composition design of low C, low Mn, high Ni and Cr, Nb elements to obtain a steel plate with a yield strength of more than 550MPa, a tensile strength of 640-820MPa, a Charpy impact energy of ≥80J at -80℃, and a yield ratio of ≤0.84. Not only is the strength level limited, but it also needs to go through two high-temperature rolling processes, the heating time is too long, and the energy consumption is high.
[0005] CN112647019A discloses "a method for manufacturing low yield strength ratio steel of different strength levels", the alloy element content of which is C: 0.06-0.12%, Mn: 1.40-1.60%, Si: 0.10-0.20%, S≤0.005%, P≤0.015%, Nb: 0.020-0.050%, Ti: 0.080-0.120%, Alt: 0.020-0.040%, N≤0.006%, and the rest is Fe and unavoidable impurities. The hot continuous rolling controlled rolling controlled cooling + quenching process is adopted, the thickness specification is 2-16mm, the tensile strength is above 700MPa level, the yield strength is between 580-689MPa, the -40℃ longitudinal low-temperature impact energy is ≤138J, and the yield strength ratio is between 0.77-0.83.
[0006] Patent CN114032459A discloses "a method for preparing medium and thick steel plates with high strength and toughness and low yield strength ratio of 690MPa yield strength", which adopts a composite alloying design of low carbon, medium-low nickel and high Cu, Cr and Mo, and Nb+V+Ti composite microalloying, and obtains steel plates with a thickness of 10-50mm, a yield strength of ≥690MPa and a yield strength ratio of ≤0.85 through multi-step heat treatment. Although this method also reaches 690MPa, it uses a multi-step heat treatment process, has a long production cycle and low production efficiency.
[0007] Therefore, the present invention designs a new composition design, through quenching + tempering heat treatment, adopts low C, medium-low Ni and Cr+Mo+V+Cu micro-alloying composition design, by controlling the content of strong carbide forming elements such as Cr, Mo, Cu, V, etc., hindering the diffusion of carbon, thereby slowing down the formation speed of austenite, refining the grain size, and coordinating the quenching + tempering process to control the ratio of soft and hard phases, forming a fine and dispersed precipitation phase, hindering the growth of grains, thereby obtaining a high-strength and toughness low yield ratio steel plate with a yield strength of more than 690MPa and a low-temperature toughness value of more than 80J at -40°C. Summary of the invention
[0008] The present invention aims to provide a low yield ratio high strength and toughness marine engineering steel and a preparation method thereof. The basic design idea adopted is that on the basis of C+Ni+Cr+Mo+V+Cu steel, the carbon content is controlled below 0.1%. Too low carbon content will inevitably reduce the strength of the steel. The content of Ni element is increased to maximize the low temperature toughness of the steel. Ni element is an element that stabilizes austenite and can greatly improve the low temperature toughness of the steel plate; at the same time, through the appropriate ratio of Cr, Ni, Mo and Cu, it produces dispersed second phase strengthening and fine grain strengthening to improve strength and toughness, so that the steel can ensure the required strength and good low temperature toughness without increasing the cost. The preparation process achieves a low yield ratio through two-stage rolling and quenching + tempering heat treatment. Rapid cooling after quenching can inhibit the transformation of austenite to soft phases such as pearlite and promote the formation of martensite or bainite. These hard phases are conducive to improving the strength of the material. High temperature tempering can promote the release of internal stress generated during quenching, and decompose hard phases such as martensite to form stable structures such as bainite and tempered troostite. With the precipitation of carbides and the decomposition of martensite, the content of soft phase ferrite gradually increases. The ratio of soft and hard phases is regulated to improve the plasticity and toughness of the material and reduce the yield strength ratio. Finally, a low yield strength ratio and high toughness marine steel with good comprehensive mechanical properties is obtained.
[0009] To achieve the above object, the technical solution of the present invention is:
[0010] A low yield ratio and high strength and toughness marine engineering steel, the element composition of which is calculated by mass percentage: C 0.08%-0.1%, Si 0.30%-0.35%, Mn 1.05%-1.25%, Ni 1.80%-2.10%, Mo 0.30%-0.35%, Cr 0.13%-0.16%, Ti 0.008%-0.010%, V 0.015%-0.030%, Nb 0.045%-0.050%, B 0.0010%-0.0013%, Cu 0.08%-0.12%, Al 0.055%-0.060%, P≤0.010%, S≤0.0040%, carbon equivalent CET≤0.31, and the balance is Fe and unavoidable impurities;
[0011] The marine engineering steel has a yield strength of ≥690MPa, a tensile strength of ≥830MPa, a yield strength ratio of ≤0.87, an elongation after fracture A of ≥18%, a transverse impact energy at room temperature of ≥100J, and a transverse impact energy at -40°C of ≥80J.
[0012] The preparation method of the low yield ratio high strength and toughness marine engineering steel comprises smelting and continuous casting → heating → controlled rolling → controlled cooling → quenching and tempering, and the steps are as follows:
[0013] Step 1. smelting and continuous casting: smelting the raw materials to obtain molten iron; smelting the ingot according to the composition of the offshore steel billet, and the thickness of the ingot is not less than 150mm; the molten iron is subjected to desulfurization treatment, converter smelting, LF refining and RH vacuum treatment, and then continuously cast into billets, the sulfur content of the molten iron after desulfurization treatment is controlled to be ≤0.0040%, the converter adopts the double slag method to control P≤0.010%, the LF refining adopts white slag operation desulfurization and deoxidation, the vacuum degree of RH vacuum treatment is ≤3.0mbar, the vacuum holding time is ≥15min, calcium treatment is carried out after the vacuum ends, and then static stirring is carried out, the static stirring time is ≥12min, and the continuous casting controls the superheat of the tundish to be 10℃~15℃; the continuous casting implements full-process protection casting, adopts large reduction (single-pass reduction is more than 20mm) rolling technology to improve the internal quality of the continuous casting billet, and uses the end-stage electric stirring to control segregation;
[0014] Step 2. Heating: After continuous casting into ingots, the ingots with a thickness of more than 150 mm are heated in a soaking furnace, the heating temperature is controlled to be 1200°C-1250°C, the furnace time is 110min-120min, and the tapping temperature is 1100°C-1180°C;
[0015] Step 3. controlled rolling: rolling the heated ingot; the rolling is divided into two stages, rough rolling and finishing rolling, and the width is controlled to be 160mm-180mm during rolling; 0-3 vertical rolling processes are performed between the finishing and rough rolling stages; the starting rolling temperature of rough rolling is 1050℃-1120℃, and after 3-5 rolling passes, the reduction rate of the last 2-3 passes is ≥9%; large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity; the cumulative compression ratio of rough rolling is not less than 1.5, and the thickness of the intermediate billet is ≥64mm; the starting rolling temperature of the finishing rolling stage is 827℃-835℃, and after 3-5 rolling passes, the final rolling temperature is ≥800℃; the rolled steel plate is obtained, and the thickness of the rolled steel plate is 20mm-100mm;
[0016] Step 4. Controlled cooling: After rolling, laminar cooling is used for cooling, with a cooling rate of 5℃ / s-10℃ / s. The water inlet temperature is 775℃-798℃, and the red-return temperature is 600℃~660℃;
[0017] Step 5. Quenching and tempering: the steel plate after controlled cooling treatment is subjected to quenching and tempering heat treatment; the quenching temperature is the phase change temperature AC3±(10℃~30℃), the holding time is 15min-60min, and after the holding is completed, it is cooled by water cooling to room temperature; then tempering treatment is carried out, the tempering temperature is 660℃-680℃, the holding time is 30min-60min, and air cooling or wind cooling is carried out to room temperature.
[0018] The mechanism of component design in the present invention is as follows:
[0019] C: It is the main element to ensure strength and hardness. If the C content is too high, a large amount of hardened structure will be produced, affecting the low-temperature impact toughness and welding performance. If the C content is too low, the strength of the steel plate will decrease. Therefore, the present invention controls the C content range to be 0.08% to 0.10%.
[0020] Si: It plays a role of solid solution strengthening and can improve the strength of the steel plate. At the same time, Si can reduce the content of O as a deoxidizer. However, the present invention uses Al deoxidation to reduce the content of Si element. However, when the mass fraction of Si is high, the toughness and plasticity of the steel will be reduced. Adding an appropriate amount of Si to the steel inhibits the growth of carbides and improves the toughness of the steel. Therefore, the content of Si in the present invention is controlled to be in the range of 0.30% to 0.35%.
[0021] Mn: It is also one of the deoxidizers, which can effectively improve the hot working performance and tear resistance of steel. Mn has the effect of delaying the transformation of austenite to ferrite in steel, which is beneficial to refining ferrite and improving strength and toughness. When the content of Mn is low, the above effect is not significant, the strength and toughness of the steel plate are low, etc., and too high will cause segregation of continuous casting billets and poor toughness. Therefore, the present invention takes into account the comprehensive addition of alloys and controls the content of Mn to be in the range of 1.05% to 1.25%.
[0022] Ni: It can expand the austenite area in the steel, so that the steel can obtain more austenite structure during the quenching process. Since austenite is the precursor of hard phase structures such as martensite after quenching, it can indirectly increase the hardness and depth after quenching and improve the hardenability; it can also refine the soft phase ferrite grains to form a finer structure, thereby improving the strength and toughness of the steel. In addition, the compounding effect with the residual Cr and P in the steel will help improve the corrosion resistance of the steel. Therefore, the present invention controls the Ni content range to be 1.80% to 2.10%.
[0023] Mo: Mo can increase the stability of austenite in steel, slow down the decomposition rate of austenite during cooling, so that steel can form a deeper hardened layer during quenching, which can increase hardenability. Mo can inhibit the growth of grains, obtain finer grains and more grain boundaries, and hinder the expansion of cracks, thereby improving strength and toughness. However, too high a content can easily cause carbides to precipitate along grain boundaries, cracks to be generated and expanded along grain boundaries, and toughness will be inhibited. Therefore, the content of Mo in the present invention is controlled to be in the range of 0.30% to 0.35%.
[0024] Cr: Chromium and iron can form a continuous solid solution, reduce the austenite phase area, and slow down the decomposition rate of austenite, so that the steel can more easily obtain a deeper hardened layer during the quenching process. In addition, chromium can also form a variety of carbides with carbon, which help to refine the structure and improve the hardenability of steel during the quenching process. However, too high a content will affect the toughness of the steel and cause temper brittleness. Therefore, the present invention controls the Cr content range to be 0.13% to 0.16%.
[0025] B: Solid solution boron promotes the formation of fine bainite structure after controlled rolling and controlled cooling. This fine bainite contains more stable dislocations, and inherits the deformation dislocations generated in austenite during formation. This fine structure has a significant effect on improving the toughness of steel. It can also produce synergistic effects with other alloying elements (such as niobium, titanium, etc.) in steel to further improve the hardenability and mechanical properties of steel. The content of B in the present invention is controlled to be in the range of 0.0010% to 0.0013%.
[0026] Cu: solid solution in steel can increase the resistance to dislocation movement, thereby achieving solid solution strengthening effect and improving the strength and hardness of steel. The addition of Cu element can also make the grains in the steel smaller and increase the grain boundary area, thereby improving the hardness and strength of the steel. Refined grains can more effectively hinder the movement of dislocations, but the Cu content should not be too high, and a higher content is more likely to cause brittle fracture. Therefore, the present invention controls the Cu content range to be 0.08% to 0.12%.
[0027] Al: It is an important deoxidizing element in the steelmaking process. Adding a small amount of Al to steel can also effectively reduce the inclusion content in the steel and refine the grains. However, too much Al will promote surface cracks in the continuous casting billet, produce internal aluminum inclusions, and reduce the quality of the slab. Therefore, the present invention controls the total Al content range to 0.055% to 0.060%.
[0028] Ti: It has the effect of grain refinement and precipitation strengthening. Ti combines with carbon to form stable carbides, which play a role in pinning austenite grain boundaries and maintaining austenite grain refinement. Ti and S can combine to form Ti4C2S2 or (MnTi)S, reduce the content of MnS inclusions in steel, improve the inhomogeneity of the structure, and thus improve the impact toughness of the steel. Therefore, the content of Ti in the present invention is controlled within the range of 0.008% to 0.010%.
[0029] V: It is an element that refines grains. It has the highest solid solubility in steel. It mainly affects the organization and performance of steel by forming V (C, N). It precipitates in the ferrite at the austenite grain boundary. During the rolling process, it can inhibit the recrystallization of austenite and prevent the growth of grains, thereby refining ferrite grains and improving the strength and toughness of steel. However, the amount of V added should not be too much. Therefore, the content of V in the present invention is controlled to be in the range of 0.015% to 0.030%.
[0030] P and S are unfavorable elements in steel, which seriously affect the strength, toughness and corrosion resistance of steel, and their content needs to be controlled as low as possible. Therefore, the present invention controls the content of P to be below 0.010%, and the content of S to be below 0.0040%.
[0031] Beneficial effects of the present invention:
[0032] The present invention provides a low yield ratio high-strength and tough marine engineering steel and a preparation method thereof, which adopts the basic design concept of low C, high Ni and Cr+Mo+V+Cu microalloying. On the basis of C+Ni+Cr+Mo+V+Cu steel, the carbon content is controlled below 0.1%. Too low carbon content will inevitably reduce the strength of the steel. The content of Ni element is increased to maximize the low-temperature toughness of the steel. Ni element is an element that stabilizes austenite and can greatly improve the low-temperature toughness of the steel plate; at the same time, through the appropriate ratio of Cr, Ni, Mo and Cu, it produces dispersed second phase strengthening and fine grain strengthening to improve strength and toughness, so that the steel can ensure the required strength and good low-temperature toughness without increasing the cost. The preparation process achieves a low yield ratio through two-stage rolling and quenching + tempering heat treatment. Rapid cooling after quenching can inhibit the transformation of austenite to soft phases such as pearlite and promote the formation of martensite or bainite. These hard phases are beneficial to improving the strength of the material. High temperature tempering can promote the release of internal stress generated during quenching, and at the same time decompose hard phases such as martensite to form stable structures such as bainite and tempered troostite. With the precipitation of carbides and the decomposition of martensite, the content of soft phase ferrite gradually increases. The ratio of soft and hard phases is regulated to improve the plasticity and toughness of the material and reduce the yield strength ratio. The final marine steel has a yield strength of ≥690MPa, a tensile strength of ≥830MPa, a yield strength ratio of ≤0.87, an elongation after fracture A ≥18%, a room temperature transverse impact toughness of ≥100J, and a -40℃ transverse impact toughness of ≥80J, with good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The microstructure morphology of the steel plate at the 1 / 2 position in the quenched and tempered state in Example 1 of the present invention;
[0034] Figure 2 The microstructure morphology of the steel plate at the 1 / 2 position in the quenched and tempered state in Example 2 of the present invention;
[0035] Figure 3 The microstructure morphology of the steel plate at the 1 / 2 position in the quenched and tempered state in Example 3 of the present invention;
[0036] Figure 4 The microstructure morphology of the steel plate at the 1 / 2 position in the quenched and tempered state in Example 4 of the present invention;
[0037] Figure 5 This is the microstructure morphology of the steel plate at the 1 / 2 position in the tempered state in Example 5 of the present invention. DETAILED DESCRIPTION
[0038] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0039] Example 1
[0040] A low yield ratio and high strength marine steel, the steel plate thickness is 20mm, its chemical composition and mass percentage are shown in Table 1, the balance is Fe and unavoidable impurities. It includes smelting and continuous casting, heating, controlled rolling, controlled cooling and quenching and tempering processes, and the specific process steps are as follows:
[0041] (1) Smelting and continuous casting: Smelt 150mm thick ingots according to chemical composition requirements. The raw materials are melted in proportion to obtain molten iron. After desulfurization treatment, the molten iron is smelted in a converter, LF refined and RH vacuum treated, and then continuously cast into ingots. The sulfur content of the molten iron after desulfurization is controlled at ≤0.0040%. The converter adopts the double slag method to control P≤0.010%. LF refining uses white slag operation for desulfurization and deoxidation. The vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min. After the vacuum is over, calcium treatment is carried out, and then static stirring is carried out. The static stirring time is ≥12min. The continuous casting controls the superheat of the tundish to be 10℃~15℃. Continuous casting implements full protection casting, adopts rolling technology with a single pass reduction of 20mm to improve the internal quality of the continuous casting ingot, and uses end-stage electric stirring to control segregation.
[0042] (2) Heating: After continuous casting into billets, the 150 mm thick billets were heated in a soaking furnace, the heating temperature was controlled at 1200°C, the furnace time was 110 min, and the tapping temperature was 1150°C;
[0043] (3) Controlled rolling: Slab rolling is divided into two stages: rough rolling and finishing rolling. The width is controlled at 160mm during rolling. Two vertical rolling processes are performed in the middle (180-68-160 is the vertical rolling reduction process for controlling the width). The starting temperature of rough rolling is 1050-1120℃. After four rolling passes, large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity. The reduction rate of the last two passes is ≥15%. The reduction rates of the passes are 13.3%, 23.1%, 20%, and 20% respectively. The cumulative reduction ratio of rough rolling is 2.3, and the thickness of the intermediate slab is 64mm. The starting temperature of the finishing rolling stage is 827℃, the final rolling temperature is 805℃, and the reduction rates of the passes are 18.7%, 19.2%, 19.0%, 17.6%, 17.8%, and 11.5% respectively.
[0044] (4) Controlled cooling: The billet is rolled to a finished product thickness of 20 mm. After rolling, it is cooled by laminar cooling at a cooling rate of 8°C / s. The water inlet temperature is 778°C and the red-return temperature is 610°C.
[0045] (5) Quenching and tempering: After rolling, the steel plate is subjected to quenching and tempering heat treatment. The quenching temperature is 860°C, the holding time is 15 minutes, and after the holding is completed, it is cooled to room temperature by water cooling in a water tank; the tempering temperature is 660°C, the holding time is 30 minutes, and air cooling is performed to room temperature.
[0046] The performance indicators of the steel plate in this embodiment are shown in Table 1. The core structure of the steel plate is as follows: Figure 1 As shown, the metallographic structure of the steel is a mixed structure of 26.5% ferrite, lath bainite and granular bainite, and the grain size is 25μm-35μm.
[0047] Example 2
[0048] A low yield ratio and high strength marine steel, the steel plate thickness is 40mm, its chemical composition and mass percentage are shown in Table 1, the balance is Fe and unavoidable impurities. It includes smelting and continuous casting, heating, controlled rolling, controlled cooling and quenching and tempering processes, and the specific process steps are as follows:
[0049] (1) Smelting and continuous casting: Smelt 150mm thick ingots according to chemical composition requirements. The raw materials are melted in proportion to obtain molten iron. After desulfurization treatment, the molten iron is smelted in a converter, LF refined and RH vacuum treated, and then continuously cast into ingots. The sulfur content of the molten iron after desulfurization is controlled at ≤0.0040%. The converter adopts the double slag method to control P≤0.010%. LF refining uses white slag operation for desulfurization and deoxidation. The vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min. After the vacuum is over, calcium treatment is carried out, and then static stirring is carried out. The static stirring time is ≥12min. The continuous casting controls the superheat of the tundish to be 10℃~15℃. Continuous casting implements full protection casting, adopts rolling technology with a single pass reduction of 20mm to improve the internal quality of the continuous casting ingot, and uses end-stage electric stirring to control segregation.
[0050] (2) Heating: After continuous casting into billets, the 150 mm thick billets were heated in a soaking furnace, the heating temperature was controlled at 1200 °C, the furnace time was 113 min, and the tapping temperature was 1150 °C;
[0051] (3) Controlled rolling: Slab rolling is divided into two stages: rough rolling and finishing rolling. The width is controlled at 160mm during rolling. Two vertical rolling processes are performed in the middle (180-68-160 is the vertical rolling reduction process for controlling the width). The starting temperature of rough rolling is 1050-1120℃. After four rolling passes, large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity. The reduction rate of the last two passes is ≥15%. The reduction rates of the passes are 13.3%, 23.1%, 20%, and 15% respectively. The cumulative reduction ratio of rough rolling is 2.2, and the thickness of the intermediate slab is 68mm. The starting temperature of the finishing rolling stage is 827℃, the final rolling temperature is 805℃, and the reduction rates of the passes are 17.6%, 18%, and 13% respectively.
[0052] (4) Controlled cooling: The billet is rolled to a finished product thickness of 40 mm. After rolling, it is cooled by laminar cooling at a cooling rate of 9 °C / s. The water inlet temperature is 785 °C and the red-return temperature is 611 °C.
[0053] (5) Quenching and tempering: After rolling, the steel plate is subjected to quenching and tempering heat treatment. The quenching temperature is 900°C, the holding time is 20 minutes, and after the holding is completed, it is cooled by water tank water cooling to room temperature; the tempering temperature is 680°C, the holding time is 60 minutes, and air cooling is performed to room temperature.
[0054] The performance indicators of the steel plate in this embodiment are shown in Table 1. The core structure of the steel plate is as follows: Figure 2 As shown, the metallographic structure of the steel is a mixed structure of 34.5% ferrite and granular bainite, and the grain size is 20μm-30μm.
[0055] Example 3
[0056] A low yield ratio and high strength marine steel, the steel plate thickness is 60mm, its chemical composition and mass percentage are shown in Table 1, the balance is Fe and unavoidable impurities. It includes smelting and continuous casting, heating, controlled rolling, controlled cooling and quenching and tempering processes, and the specific process steps are as follows:
[0057] (1) Smelting and continuous casting: Smelt 180mm thick ingots according to chemical composition requirements. The raw materials are melted in proportion to obtain molten iron. After desulfurization treatment, the molten iron is smelted in a converter, LF refined and RH vacuum treated, and then continuously cast into ingots. The sulfur content of the molten iron after desulfurization is controlled at ≤0.0040%. The converter adopts the double slag method to control P≤0.010%. LF refining uses white slag operation for desulfurization and deoxidation. The vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min. After the vacuum is over, calcium treatment is carried out, and then the static stirring time is ≥12min. The continuous casting controls the superheat of the tundish to be 10℃~15℃. The continuous casting implements full protection casting, adopts the rolling technology with a single pass reduction of 20mm to improve the internal quality of the continuous casting ingot, and uses the end-stage electric stirring to control segregation.
[0058] (2) Heating: After continuous casting into billets, the 180 mm thick continuous casting billets are heated in a soaking furnace, the heating temperature is controlled at 1200 °C, the furnace time is 120 min, and the tapping temperature is 1180 °C;
[0059] (3) Controlled rolling: Slab rolling is divided into two stages: rough rolling and finishing rolling. The starting rolling temperature of rough rolling is 1050℃-1120℃. After 4 rolling passes, large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity. The reduction rate of the last two passes is ≥15%. The reduction rates of the passes are 16.7%, 16.7%, 16%, and 14.3% respectively. The cumulative reduction ratio of rough rolling is 2, and the thickness of the intermediate slab is 90mm. The starting rolling temperature of the finishing rolling stage is 834℃, the final rolling temperature is 805℃, and the reduction rates of the passes are 10%, 9.8%, 8.2%, 7.5%, and 3.2% respectively.
[0060] (4) Controlled cooling: The billet is rolled to a finished product thickness of 60 mm. After rolling, it is cooled by laminar cooling at a cooling rate of 10°C / s. The water inlet temperature is 792°C and the red-return temperature is 600°C.
[0061] (5) Quenching and tempering: After rolling, the steel plate is subjected to quenching and tempering heat treatment. The quenching temperature is 920℃, the holding time is 20min, and after the holding is completed, it is cooled by water tank water cooling to room temperature; the tempering temperature is 660℃, the holding time is 60min, and air cooling is performed to room temperature.
[0062] The performance indicators of the steel plate in this embodiment are shown in Table 1. The core structure of the steel plate is as follows: Figure 3 As shown, the metallographic structure of the steel is a mixed structure of 59.5% ferrite and granular bainite, and the grain size is 10μm-20μm.
[0063] Example 4
[0064] A low yield ratio and high strength marine steel, the steel plate thickness is 80mm, its chemical composition and mass percentage are shown in Table 1, the balance is Fe and unavoidable impurities. It includes smelting and continuous casting, heating, controlled rolling, controlled cooling and quenching and tempering processes, and the specific process steps are as follows:
[0065] (1) Smelting and continuous casting: Smelt 250mm thick ingots according to chemical composition requirements. The raw materials are melted in proportion to obtain molten iron. After desulfurization treatment, the molten iron is smelted in a converter, LF refined and RH vacuum treated, and then continuously cast into ingots. The sulfur content of the molten iron after desulfurization is controlled at ≤0.0040%. The converter adopts the double slag method to control P≤0.010%. LF refining uses white slag operation for desulfurization and deoxidation. The vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min. After the vacuum is over, calcium treatment is carried out, and then the static stirring time is ≥12min. The continuous casting controls the superheat of the tundish to be 10℃~15℃. The continuous casting implements full protection casting, adopts the rolling technology with a single pass reduction of 30mm to improve the internal quality of the continuous casting ingot, and uses the end-stage electric stirring to control segregation.
[0066] (2) Heating: After continuous casting into billets, the 250 mm thick continuous casting billets are heated in a soaking furnace, the heating temperature is controlled at 1200 °C, the furnace time is 120 min, and the steel tapping temperature is 1180 °C;
[0067] (3) Controlled rolling: Slab rolling is divided into two stages: rough rolling and finishing rolling. The starting rolling temperature of rough rolling is 1050℃-1120℃. After 4 rolling passes, large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity. The reduction rate of the last two passes is ≥15%. The reduction rates of the passes are 12%, 13.6%, 15.8%, 15.6%, and 17.2% respectively. The cumulative reduction ratio of rough rolling is 2.1, and the thickness of the intermediate slab is 120mm. The starting rolling temperature of the finishing rolling stage is 834℃, the final rolling temperature is 805℃, and the reduction rates of the passes are 12.5%, 9.5%, 8.4%, and 8% respectively.
[0068] (4) Controlled cooling: The billet is rolled to a finished product thickness of 80 mm. After rolling, it is cooled by laminar cooling at a cooling rate of 5°C / s. The water inlet temperature is 798°C and the red-return temperature is 633°C.
[0069] (5) Quenching and tempering: After rolling, the steel plate is subjected to conditioning heat treatment. The quenching temperature is 890°C, the holding time is 30 minutes, and after the holding is completed, it is cooled to room temperature by water cooling in a water tank; the tempering temperature is 680°C, the holding time is 60 minutes, and air cooling is performed to room temperature.
[0070] The performance indicators of the steel plate in this embodiment are shown in Table 1. The core structure of the steel plate is as follows: Figure 4 As shown, the metallographic structure of the steel is a mixed structure of 64.3% ferrite, tempered troostite and granular bainite, and the grains are fine, with a size of 5μm-15μm.
[0071] Example 5
[0072] A low yield ratio and high strength and toughness marine steel, the steel plate thickness is 100mm, its chemical composition and mass percentage are shown in Table 1, the balance is Fe and unavoidable impurities. It includes smelting and continuous casting, heating, controlled rolling, controlled cooling and quenching and tempering processes, and the specific process steps are as follows:
[0073] (1) Smelting and continuous casting: Smelt 300mm thick ingots according to chemical composition requirements. The raw materials are melted in proportion to obtain molten iron. After desulfurization treatment, the molten iron is smelted in a converter, LF refined and RH vacuum treated, and then continuously cast into ingots. The sulfur content of the molten iron after desulfurization is controlled at ≤0.0040%. The converter adopts the double slag method to control P≤0.010%. LF refining uses white slag operation for desulfurization and deoxidation. The vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min. After the vacuum is over, calcium treatment is carried out, and then the static stirring time is ≥12min. The superheat of the continuous casting ladle is controlled to be 10℃~15℃. The continuous casting implements full protection casting, adopts the rolling technology with a single pass reduction of 20mm to improve the internal quality of the continuous casting ingot, and uses the end-stage electric stirring to control segregation.
[0074] (2) Heating: After continuous casting into billets, the 300 mm thick continuous casting billets were heated in a soaking furnace, the heating temperature was controlled at 1200 °C, the furnace time was 120 min, and the tapping temperature was 1170 °C;
[0075] (3) Controlled rolling: Slab rolling is divided into two stages: rough rolling and finishing rolling. The starting rolling temperature of rough rolling is 1050℃-1120℃. After 4 rolling passes, large reduction rolling is adopted to ensure that the reduction rate of each pass is set as much as possible according to the maximum rolling capacity. The reduction rate of the last two passes is ≥9%. The reduction rates of the passes are 6.7%, 10.7%, 12%, 9.1%, and 10% respectively. The cumulative reduction ratio of rough rolling is 1.6, and the thickness of the intermediate slab is 180mm. The starting rolling temperature of the finishing rolling stage is 834℃, the final rolling temperature is 805℃, and the reduction rates of the passes are 16.7%, 16.7%, 12%, and 9.1% respectively.
[0076] (4) Controlled cooling: The billet is rolled to a finished product thickness of 100 mm. After rolling, it is cooled by laminar cooling at a cooling rate of 10°C / s. The water inlet temperature is 798°C and the red-return temperature is 660°C.
[0077] (5) Quenching and tempering: After rolling, the steel plate is subjected to quenching and tempering heat treatment. The quenching temperature is 900°C, the holding time is 60 minutes, and after the holding is completed, it is cooled by water tank water cooling to room temperature; the tempering temperature is 660°C, the holding time is 30 minutes, and air cooling is performed to room temperature.
[0078] The performance indicators of the steel plate in this embodiment are shown in Table 1. The core structure of the steel plate is as follows: Figure 5 As shown: the metallographic structure of the steel is a mixture of 64.4% ferrite, tempered troostite and granular bainite, with fine grains and a size of 4μm-13μm.
[0079] Table 1 Chemical composition and performance comparison table of steel plates in the embodiments of the present invention
[0080]
[0081]
[0082] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A low yield ratio and high toughness marine engineering steel, characterized in that: Its element composition is calculated by mass percentage: C 0.08% ~ 0.1%, Si 0.30% ~ 0.35%, Mn 1.05% ~ 1.25%, Ni 1.80% ~ 2.10%, Mo 0.30% ~ 0.35%, Cr 0.13% ~ 0.16%, Ti 0.008% ~ 0.010%, V 0.015% ~ 0.030%, Nb 0.045% ~ 0.050%, B 0.0010% ~ 0.0013%, Cu 0.08% ~ 0.12%, Al 0.055% ~ 0.060%, P ≤ 0.010%, S ≤ 0.0040%, carbon equivalent CET ≤ 0.31, and the balance is Fe and unavoidable impurities.
2. The low yield ratio and high toughness marine engineering steel according to claim 1, characterized in that: The marine engineering steel has a yield strength of ≥690MPa, a tensile strength of ≥830MPa, a yield strength ratio of ≤0.87, an elongation after fracture A of ≥18%, a transverse impact energy at room temperature of ≥100J, and a transverse impact energy at -40°C of ≥80J.
3. A method for preparing the low yield ratio and high toughness marine engineering steel according to claim 1 or 2, characterized in that: Including smelting and continuous casting → heating → controlled rolling → controlled cooling → quenching and tempering, the steps are as follows: Step 1. Smelting and continuous casting: smelting the raw materials to obtain molten iron; the molten iron is subjected to desulfurization treatment, converter smelting, LF refining and RH vacuum treatment, and then continuously cast into billets; wherein, the molten iron is smelted into billets according to the composition of marine steel, and the thickness of the billets is not less than 150mm; the single pass reduction in the continuous casting process is more than 20mm; Step 2. Heating: heating the ingot in a soaking furnace and then taking it out of the furnace; wherein the heating temperature is 1200°C-1250°C; Step 3. Controlled rolling: rolling the heated ingot to obtain a rolled steel plate; the rolling process is divided into finishing rolling and rough rolling, and 0-3 vertical rolling processes are performed between the finishing rolling and rough rolling stages; wherein the rough rolling is performed for 3-5 passes, and the reduction rate of the last 2-3 passes is ≥9%; the finishing rolling is performed for 3-5 passes; Step 4. Controlled cooling: The rolled steel plate is cooled by laminar cooling at a cooling rate of 5°C / s-10°C / s; Step 5. Quenching and tempering: The steel plate after controlled cooling treatment is subjected to quenching and tempering heat treatment and then water-cooled to room temperature, and then tempered and cooled to room temperature.
4. The method for preparing a low yield ratio and high toughness marine engineering steel according to claim 3, characterized in that: In step 1, the sulfur content of the molten iron after desulfurization treatment is controlled at ≤0.0040%; the converter adopts the double slag method to control P≤0.010%; LF refining adopts white slag operation for desulfurization and deoxidation; the vacuum degree of RH vacuum treatment is ≤3.0mbar, and the vacuum holding time is ≥15min; calcium treatment is carried out after the vacuum is ended, and then static stirring is carried out, and the static stirring time is ≥12min; continuous casting implements full casting protection, and the superheat of the tundish is controlled at 10℃~15℃ during the continuous casting process.
5. The method for preparing a low yield ratio and high toughness marine engineering steel according to claim 3, characterized in that: In step 2, during the heating process, the time in the furnace is 110min-120min; after the heating is completed, the steel tapping temperature is 1100℃-1180℃.
6. The method for preparing a low yield ratio and high toughness marine engineering steel according to claim 3, characterized in that: In step 3, the width is controlled to be 160 mm-180 mm during the rolling process; In the rough rolling stage, the starting rolling temperature is 1050℃-1120℃, the cumulative compression ratio of rough rolling is not less than 1.5, and the thickness of the intermediate billet is ≥64mm; In the finishing rolling stage, the starting rolling temperature is 827℃-835℃, and the final rolling temperature is ≥800℃; The thickness of the steel plate after rolling is 20mm-100mm.
7. The method for preparing a low yield ratio and high toughness marine engineering steel according to claim 3, characterized in that: In step 4, during cooling, the water inlet temperature is 775°C-798°C, and the red-returning temperature is 600°C-660°C.
8. The method for preparing a low yield ratio and high toughness marine engineering steel according to claim 3, characterized in that: In step 5, during the quenching and tempering heat treatment, the quenching temperature is the phase transition temperature AC3±(10°C~30°C), and the holding time is 15min-60min; The tempering temperature is 660℃-680℃, and the holding time is 30min-60min; the cooling after tempering is carried out by controlled cooling or air cooling.
Citation Information
Patent Citations
Manufacturing method of steel with high-strength and high-toughness for ocean engineering
CN113355583A
FH690-grade maritime work steel with excellent low-temperature toughness and manufacturing method of FH690-grade maritime work steel with excellent low-temperature toughness
CN113549827A
Production method of high-toughness low-yield-ratio low-alloy high-strength steel plate
CN114645183A
High-strength high-toughness low-temperature maritime work steel plate and manufacturing method thereof
CN116200682A
Thin-gauge low-yield-ratio 690MPa-grade steel for ocean engineering and manufacturing method of thin-gauge low-yield-ratio 690MPa-grade steel
CN116607076A
Cited By
Production method of steel plate for 440MPa-grade normalized ship body
CN119859741A
A method for producing a 440mpa grade normalized steel plate for a ship body
CN119859741B
High-strength and high-toughness multiphase high-manganese steel and preparation method thereof
CN120425239A
Thick normalized s355g8+n offshore steel plate and production method therefor
WO2026152848A1