Preparation method of wear-resistant coating of gravure plate, gravure plate and application of gravure plate

By using a composite method of high-power pulse magnetron sputtering and medium-frequency magnetron sputtering technology on the surface of the gravure printing plate, a composite wear-resistant coating is formed, which solves the problem of insufficient film-based bonding and denseness in magnetron sputtering technology. , achieving high density and efficient deposition.

CN118979232APending Publication Date: 2024-11-19CHINA BANKNOTE PRINTING & MINTING +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040969.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When plating the gravure printing plate, magnetron sputtering technology has problems such as poor film base bonding force and poor film layer structure density.

Method used

The bottom layer is plated by high-power pulse magnetron sputtering method, the middle layer is plated by the first intermediate frequency magnetron sputtering method, and the wear-resistant layer is plated by the second intermediate frequency magnetron sputtering method, and the high-power pulse magnetron sputtering method is plated by the composite use of high-power pulse magnetron sputtering Explosion technology and intermediate frequency magnetron sputtering technology form a composite wear-resistant coating.

Benefits of technology

The high density and high film-based binding force of the composite wear-resistant coating are achieved, the deposition efficiency is improved, and the printing resistance level is better than that of the coating made by a single magnetron sputtering technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972374420000121
    Figure BDA0004972374420000121
Patent Text Reader

Abstract

The invention relates to the technical field of banknote printing, and discloses a preparation method of a wear-resistant coating of a gravure plate, the gravure plate and application of the gravure plate. The gravure plate comprises a gravure plate substrate, a base layer plated on the surface of the gravure plate substrate by adopting a high-power pulse magnetron sputtering technology, a middle layer plated on the surface of the base layer by adopting a first medium-frequency magnetron sputtering technology, and a wear-resistant layer plated on the surface of the middle layer by adopting a second medium-frequency magnetron sputtering technology. According to the gravure plate provided by the invention, the high-power pulse magnetron sputtering technology and the medium-frequency magnetron sputtering technology are compositely used for the first time, and the composite wear-resistant coating is plated on the surface of the gravure plate, so that high compactness and high film-substrate binding force of the composite wear-resistant coating are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of banknote printing, and in particular to a method for preparing a wear-resistant coating of a gravure printing plate, a gravure printing plate and uses thereof. Background Art

[0002] The preparation of traditional gravure plate wear-resistant coating is mainly completed by electroplating chromium. However, the electroplating chromium process is not friendly to the environment and personnel, and is gradually being replaced by other processes.

[0003] PVD (Physical Vapor Deposition) technology is a clean coating process and is considered the most competitive alternative to electroplating chromium due to its minimal impact on the environment. Magnetron sputtering technology has the advantages of high deposition efficiency, low ambient temperature and good coating adhesion, and is considered the most likely technology to achieve industrial production among various PVD technologies.

[0004] In the related art, magnetron sputtering technology has been tried for gravure plate coating, where a Cr layer is first plated on the surface of the gravure printing plate, and then a CrN coating is plated using magnetron sputtering technology. However, when the above method is used for coating or magnetron sputtering technology is directly used to coat the surface of the gravure plate, there are problems such as poor film-base bonding and poor film layer structure density. Summary of the invention

[0005] In view of this, the present invention provides a method for preparing a wear-resistant coating of a gravure plate, a gravure plate and uses thereof, so as to solve the problems of poor film-base bonding and poor film layer structure density existing in the related art when the gravure plate is coated with magnetron sputtering technology.

[0006] In a first aspect, the present invention provides a wear-resistant coating, comprising a base layer plated on the surface of a substrate by a high-power pulsed magnetron sputtering method, an intermediate layer plated on the surface of the base layer by a first medium-frequency magnetron sputtering method, and a wear-resistant layer plated on the surface of the intermediate layer by a second medium-frequency magnetron sputtering method.

[0007] Preferably, the substrate comprises a gravure plate, kitchenware, a watch or a decorative item.

[0008] In the wear-resistant coating provided by the present invention, high-power pulsed magnetron sputtering technology and medium-frequency magnetron sputtering technology are used in combination for the first time to plate the composite wear-resistant coating on the surface of the gravure plate, thereby achieving high density and high film-base bonding strength of the composite wear-resistant coating.

[0009] In an optional embodiment, the primer layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer;

[0010] and / or, the intermediate layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer;

[0011] And / or, the wear-resistant layer is selected from at least one of a chromium nitride layer, a titanium nitride layer, an aluminum nitride layer, a calcium nitride layer and a boron nitride layer.

[0012] In a second aspect, the present invention provides a method for preparing a wear-resistant coating of a gravure printing plate, comprising the following steps:

[0013] Taking the gravure printing plate substrate, a high-power pulsed magnetron sputtering method is used to plate the bottom layer to obtain the first intermediate plate;

[0014] Taking the first intermediate plate, and using a first medium-frequency magnetron sputtering method to plate an intermediate layer on the surface of the base layer, to obtain a second intermediate plate;

[0015] The second intermediate plate is taken, and a wear-resistant layer is plated on the surface of the intermediate layer by a second medium-frequency magnetron sputtering method.

[0016] In an optional embodiment, when coating the base layer, the conditions of the high-power pulsed magnetron sputtering method include at least one of the following:

[0017] The deposition temperature is 150°C to 160°C;

[0018] and / or, the deposition time is 30 min to 40 min;

[0019] And / or, the power supply has an operating power of 10kW to 15kW;

[0020] And / or, the substrate bias voltage is -300V to -400V.

[0021] In an optional embodiment, when coating the intermediate layer, the conditions of the first medium frequency magnetron sputtering method include at least one of the following:

[0022] The deposition temperature is 150°C to 160°C;

[0023] and / or, the deposition time is 40 to 50 minutes;

[0024] And / or, the power supply has an operating power of 15kW to 25kW;

[0025] And / or, the substrate bias voltage is -30V to -80V.

[0026] In an optional embodiment, when coating the wear-resistant layer, the conditions of the second medium-frequency magnetron sputtering method include at least one of the following:

[0027] The deposition temperature is 150°C to 160°C;

[0028] and / or, the deposition time is 60 min to 70 min;

[0029] And / or, the power supply has an operating power of 15kW to 25kW;

[0030] And / or, the substrate bias voltage is -30V to -80V.

[0031] In an optional embodiment, when preparing the primer layer and the intermediate layer, argon gas is introduced into the working chamber, and the argon gas flow rate is 200 sccm to 400 sccm;

[0032] And / or, when preparing the wear-resistant layer, nitrogen gas is introduced into the working chamber, and the nitrogen gas flow rate is 20 sccm to 40 sccm.

[0033] In an optional embodiment, before the high-power pulsed magnetron sputtering method is used to plate the base layer, the steps of ultrasonic cleaning, drying, dust removal and etching cleaning are also included in sequence for the gravure plate;

[0034] Optionally, the etching and cleaning process includes:

[0035] Placing the dust-free gravure printing plate in a working chamber, evacuating the working chamber to a vacuum degree not higher than 1.0×10-3Pa, and setting the temperature in the working chamber to 150°C to 160°C;

[0036] Argon gas is introduced into the working chamber until the pressure in the working chamber is not less than 0.5 Pa, the substrate bias voltage is set to -100V to -150V, and the gravure plate is bombarded with argon ions for 60min to 90min under the bias voltage condition.

[0037] In a third aspect, the present invention provides a gravure printing plate, the gravure printing plate comprising a gravure printing plate substrate and the wear-resistant coating, the wear-resistant coating comprising the above-mentioned wear-resistant coating or the wear-resistant coating prepared by the preparation method. The wear-resistant coating comprises a base layer plated on the surface of the gravure printing plate substrate by a high-power pulsed magnetron sputtering method, an intermediate layer plated on the surface of the base layer by a first medium-frequency magnetron sputtering method, and a wear-resistant layer plated on the surface of the intermediate layer by a second medium-frequency magnetron sputtering method.

[0038] In an optional embodiment, the gravure printing plate substrate includes a nickel gravure printing plate and / or a copper gravure printing plate.

[0039] In a fourth aspect, the present invention provides use of the above-mentioned gravure printing plate or the gravure printing plate prepared by the above-mentioned preparation method in banknote printing. DETAILED DESCRIPTION

[0040] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and scope of protection of the present invention.

[0041] Any product identical or similar to the present invention obtained by combining the features of the present invention shall fall within the protection scope of the present invention.

[0042] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0043] In order to solve the problems existing in the above-mentioned related technologies, according to the first aspect of the present invention, the present invention provides a wear-resistant coating, which includes a base layer plated on the surface of a substrate using a high-power pulse magnetron sputtering technology (high-power pulse magnetron sputtering method), an intermediate layer plated on the surface of the base layer using a first medium-frequency magnetron sputtering technology (medium-frequency magnetron sputtering method), and a wear-resistant layer plated on the surface of the intermediate layer using a second medium-frequency magnetron sputtering technology (medium-frequency magnetron sputtering method).

[0044] The wear-resistant coating of the present invention can also be a multi-layer structure. The coating is plated on the surface of the substrate using high-power pulsed magnetron sputtering technology to form a base layer, and then the middle layer plated using the first medium-frequency magnetron sputtering technology and the wear-resistant layer plated using the second medium-frequency magnetron sputtering technology are deposited in a superimposed manner.

[0045] Preferably, the substrate comprises a gravure plate, kitchenware, a watch or a decorative item.

[0046] The method for preparing the wear-resistant coating comprises the following steps: using high-power pulsed magnetron sputtering technology to plate a base layer on the surface of a substrate to obtain a first intermediate plate;

[0047] Taking the first intermediate plate, and using the first intermediate frequency magnetron sputtering technology to plate an intermediate layer on the surface of the base layer, to obtain a second intermediate plate;

[0048] The second intermediate plate is taken, and a wear-resistant layer is plated on the surface of the intermediate layer by using a second medium-frequency magnetron sputtering technology.

[0049] In a second aspect, the present invention provides a gravure plate, comprising a gravure plate substrate and the wear-resistant coating, wherein the wear-resistant coating comprises a base layer plated on the surface of the gravure plate substrate using a high-power pulsed magnetron sputtering technique, an intermediate layer plated on the surface of the base layer using a first medium-frequency magnetron sputtering technique, and a wear-resistant layer plated on the surface of the intermediate layer using a second medium-frequency magnetron sputtering technique.

[0050] In the wear-resistant coating or gravure plate provided by the present invention, high-power pulsed magnetron sputtering technology and medium-frequency magnetron sputtering technology are used in combination for the first time to plate a composite wear-resistant coating on the surface of the gravure plate substrate, thereby achieving high density and high film-base bonding strength of the composite wear-resistant coating, and also achieving high deposition efficiency that is not available with a single magnetron sputtering technology.

[0051] Specifically, through ball pit test, roughness test, scratch test, hardness test, surface morphology observation and other analyses, it was found that the composite wear-resistant coating prepared by HiPIMS and MFMS technology has a dense structure and strong film-base bonding. After on-machine printing test, the printing durability level is relatively high, which is better than the coating made by single magnetron sputtering technology.

[0052] In an optional embodiment, when coating the base layer, the conditions of the high-power pulsed magnetron sputtering technology include at least one of the following:

[0053] The deposition temperature is 150°C to 160°C;

[0054] and / or, the deposition time is 30 min to 40 min;

[0055] And / or, the power supply has an operating power of 10kW to 15kW;

[0056] And / or, the substrate bias voltage is -300V to -400V.

[0057] In an optional embodiment, when coating the intermediate layer, the conditions of the first medium frequency magnetron sputtering technology include at least one of the following:

[0058] The deposition temperature is 150°C to 160°C;

[0059] and / or, the deposition time is 40 to 50 minutes;

[0060] And / or, the power supply has an operating power of 15kW to 25kW;

[0061] And / or, the substrate bias voltage is -30V to -80V.

[0062] In an optional embodiment, when coating the wear-resistant layer, the conditions of the second medium-frequency magnetron sputtering technology include at least one of the following:

[0063] The deposition temperature is 150°C to 160°C;

[0064] and / or, the deposition time is 60 min to 70 min;

[0065] And / or, the power supply has an operating power of 15kW to 25kW;

[0066] And / or, the substrate bias voltage is -30V to -80V.

[0067] In an optional embodiment, the primer layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer;

[0068] and / or, the intermediate layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer;

[0069] And / or, the wear-resistant layer is selected from at least one of a chromium nitride layer, a titanium nitride layer, an aluminum nitride layer, a calcium nitride layer and a boron nitride layer.

[0070] In an optional embodiment, the gravure printing plate substrate includes a nickel gravure printing plate and / or a copper gravure printing plate.

[0071] In a third aspect, the present invention provides a method for preparing a wear-resistant coating of a gravure printing plate, comprising the following steps:

[0072] Take the gravure printing plate substrate and use high-power pulsed magnetron sputtering technology to plate the bottom layer to obtain the first intermediate plate;

[0073] Taking the first intermediate plate, and using the first intermediate frequency magnetron sputtering technology to plate an intermediate layer on the surface of the base layer, to obtain a second intermediate plate;

[0074] The second intermediate plate is taken, and a wear-resistant layer is plated on the surface of the intermediate layer by using a second medium-frequency magnetron sputtering technology.

[0075] In an optional embodiment, when preparing the primer layer and the intermediate layer, argon gas is introduced into the working chamber, and the argon gas flow rate is 200 sccm to 400 sccm;

[0076] And / or, when preparing the wear-resistant layer, nitrogen gas is introduced into the working chamber, and the nitrogen gas flow rate is 20 sccm to 40 sccm.

[0077] In an optional embodiment, before the high-power pulsed magnetron sputtering technology is used to plate the base layer, the steps of ultrasonic cleaning, drying, dust removal and etching cleaning are also included in sequence for the gravure plate;

[0078] Optionally, the etching and cleaning process includes:

[0079] The dust-free gravure plate is placed in a working chamber and evacuated until the vacuum degree in the working chamber is no higher than 1.0×10 -3 Pa, and the temperature in the working chamber is set to 150°C to 160°C;

[0080] Argon gas is introduced into the working chamber until the pressure in the working chamber is not less than 0.5 Pa, the substrate bias voltage is set to -100V to -150V, and the gravure plate is bombarded with argon ions for 60min to 90min under the bias voltage condition.

[0081] Optionally, the process of ultrasonically cleaning, drying and dusting the gravure plate in sequence includes: using an aqueous cleaning agent to ultrasonically clean the gravure plate for 10 to 15 minutes before clamping, rinsing with deionized water and drying with an air knife, then evenly spraying anhydrous ethanol on the surface of the gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal.

[0082] In a fourth aspect, the present invention provides the use of the above-mentioned gravure printing plate in banknote printing.

[0083] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.

[0084] Example 1

[0085] The gravure printing plate with a wear-resistant coating was prepared as follows:

[0086] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 10 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-free gravure plate;

[0087] (2) The working chamber is equipped with a HiPIMS power supply and a MFMS power supply, and the dust-free gravure plate is placed in the working chamber and fixed on the coating machine rotating frame, and then the working chamber is evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 150°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -100V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 60min to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0088] (3) Taking the above-mentioned gravure plate after etching and cleaning, under the condition of passing argon gas (argon gas flow rate is 200 sccm), using HiPIMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a chromium layer as a base layer to obtain a first intermediate plate, wherein the time for plating the chromium layer using the HiPIMS power supply is 30 minutes, the operating power of the HiPIMS power supply is 10 kW, and the substrate bias voltage is -300 V;

[0089] (4) Take the first intermediate plate, and under the condition of passing argon gas (argon gas flow rate is 200 sccm), use MFMS power supply and a high purity chromium target with purity not less than 99.9% to plate a chromium layer as an intermediate layer to obtain a second intermediate plate, wherein the chromium layer is plated using the MFMS power supply for 40 minutes, the MFMS power supply has an operating power of 15 kW, and the substrate bias voltage is -30 V;

[0090] (5) Take the above-mentioned second intermediate plate, and under the condition of introducing nitrogen (nitrogen flow rate is 20sccm), use MFMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a layer of chromium nitride as a wear-resistant layer to obtain a finished gravure plate, wherein the time for plating the chromium nitride layer using MFMS power supply is 60 minutes, the working power of MFMS power supply is 15kW, and the substrate bias voltage is -30V.

[0091] Example 2

[0092] The gravure printing plate with a wear-resistant coating was prepared as follows:

[0093] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 15 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-removed gravure plate;

[0094] (2) The working chamber is equipped with a HiPIMS power supply and a MFMS power supply, and the dust-free gravure plate is placed in the working chamber and fixed on the coating machine rotating frame, and then the working chamber is evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 160°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -150V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 90 minutes to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0095] (3) Taking the above-mentioned gravure plate after etching and cleaning, under the condition of passing argon gas (argon gas flow rate is 400 sccm), using HiPIMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a chromium layer as a base layer to obtain a first intermediate plate, wherein the time for plating the chromium layer using the HiPIMS power supply is 40 minutes, the operating power of the HiPIMS power supply is 15 kW, and the substrate bias voltage is -400 V;

[0096] (4) Take the first intermediate plate, and under the condition of passing argon gas (argon gas flow rate is 400 sccm), use MFMS power supply and a high purity chromium target with purity not less than 99.9% to plate a chromium layer as an intermediate layer to obtain a second intermediate plate, wherein the chromium layer is plated using the MFMS power supply for 50 min, the MFMS power supply has an operating power of 25 kW, and the substrate bias voltage is -80 V;

[0097] (5) Take the above-mentioned second intermediate plate, and under the condition of introducing nitrogen (nitrogen flow rate is 40sccm), use MFMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a layer of chromium nitride as a wear-resistant layer to obtain a finished gravure plate, wherein the time for plating the chromium nitride layer using MFMS power supply is 70 minutes, the working power of MFMS power supply is 25kW, and the substrate bias voltage is -80V.

[0098] Comparative Example 1

[0099] Prepare the gravure printing plate as follows:

[0100] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 10 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-free gravure plate;

[0101] (2) A HiPIMS power supply is installed in the working chamber, and the dust-free gravure plate is placed in the working chamber and fixed on the coating machine rotating rack. The working chamber is then evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 150°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -100V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 60min to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0102] (3) Taking the above-mentioned gravure plate after etching and cleaning, under the condition of passing argon gas (argon gas flow rate is 200 sccm), using HiPIMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a chromium layer as a base layer to obtain a first intermediate plate, wherein the time for plating the chromium layer using the HiPIMS power supply is 30 minutes, the operating power of the HiPIMS power supply is 10 kW, and the substrate bias voltage is -300 V;

[0103] (4) Take the first intermediate plate, and under the condition of passing argon gas (argon gas flow rate is 200 sccm), use HiPIMS power supply and a high purity chromium target with purity not less than 99.9% to plate a chromium layer as an intermediate layer to obtain a second intermediate plate, wherein the chromium layer is plated using the HiPIMS power supply for 40 min, the HiPIMS power supply working power is 10 kW, and the substrate bias voltage is -300 V;

[0104] (5) Take the above-mentioned second intermediate plate, and under the condition of introducing nitrogen (nitrogen flow rate is 20sccm), use HiPIMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a layer of chromium nitride as a wear-resistant layer to obtain a finished gravure plate, wherein the time for plating the chromium nitride layer using HiPIMS power supply is 60 minutes, the working power of HiPIMS power supply is 10kW, and the substrate bias is -300V.

[0105] Comparative Example 2

[0106] Prepare the gravure printing plate as follows:

[0107] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 10 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-free gravure plate;

[0108] (2) The working chamber is equipped with an MFMS power supply, and the dust-free gravure plate is placed in the working chamber and fixed on the coating machine rotating frame, and then the working chamber is evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 150°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -100V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 60min to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0109] (3) Taking the above-mentioned gravure plate after etching and cleaning, under the condition of passing argon gas (argon gas flow rate is 200 sccm), using MFMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a chromium layer as a base layer to obtain a first intermediate plate, wherein the MFMS power supply is used to plate the chromium layer for 30 minutes, the MFMS power supply working power is 15 kW, and the substrate bias voltage is -30 V;

[0110] (4) Take the first intermediate plate, and under the condition of passing argon gas (argon gas flow rate is 200 sccm), use MFMS power supply and a high purity chromium target with purity not less than 99.9% to plate a chromium layer as an intermediate layer to obtain a second intermediate plate, wherein the chromium layer is plated using the MFMS power supply for 40 minutes, the MFMS power supply has an operating power of 15 kW, and the substrate bias voltage is -30 V;

[0111] (5) Take the above-mentioned second intermediate plate, and under the condition of introducing nitrogen (nitrogen flow rate is 20sccm), use MFMS power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a layer of chromium nitride as a wear-resistant layer to obtain a finished gravure plate, wherein the time for plating the chromium nitride layer using MFMS power supply is 60 minutes, the working power of MFMS power supply is 15kW, and the substrate bias voltage is -30V.

[0112] Comparative Example 3

[0113] Prepare the gravure printing plate as follows:

[0114] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 10 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-free gravure plate;

[0115] (2) A DC power supply is installed in the working chamber, and the dust-free gravure plate is placed in the working chamber and fixed on the rotating rack of the coating machine. Then, the working chamber is evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 150°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -100V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 60min to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0116] (3) taking the above-mentioned gravure printing plate after etching and cleaning, and plating a chromium layer as a base layer using a DC power supply and a high-purity chromium target with a purity of not less than 99.9% under the condition of passing argon gas (argon gas flow rate is 200 sccm), wherein the DC power supply is used to plate the chromium layer for 30 minutes, the DC power supply working power is 10 kW, and the substrate bias voltage is -30 V;

[0117] (4) taking the first intermediate plate, and plating a chromium layer as an intermediate layer using a DC power supply and a high-purity chromium target with a purity of not less than 99.9% under the condition of passing argon gas (argon gas flow rate is 200 sccm), wherein the DC power supply is used to plate the chromium layer for 40 min, the DC power supply has an operating power of 10 kW, and the substrate bias voltage is -30 V;

[0118] (5) Take the second intermediate plate and, under the condition of introducing nitrogen (nitrogen flow rate is 20 sccm), use a DC power supply and a high-purity chromium target with a purity of not less than 99.9% to plate a chromium nitride layer as a wear-resistant layer to obtain a finished gravure plate, wherein the DC power supply is used to plate the chromium nitride layer for 60 minutes, the DC power supply working power is 10 kW, and the substrate bias is -30 V.

[0119] Comparative Example 4

[0120] The gravure printing plate with a wear-resistant coating was prepared as follows:

[0121] (1) taking a nickel gravure plate, using an aqueous cleaning agent (composed of a surfactant such as sodium dodecyl sulfate, sodium tripolyphosphate and water) to ultrasonically clean the plate for 10 minutes, then rinsing the plate with deionized water and performing air knife drying, then spraying anhydrous ethanol evenly on the surface of the dried gravure plate, and wiping the surface of the gravure plate with a dust-free cloth for secondary dust removal, thereby obtaining a dust-free gravure plate;

[0122] (2) A HiPIMS power supply is installed in the working chamber, and the dust-free gravure plate is placed in the working chamber and fixed on the coating machine rotating rack. The working chamber is then evacuated to a pressure of 1.0×10 -3 Pa, set the chamber temperature to 150°C; introduce pure argon gas into the working chamber until the chamber pressure reaches 0.5Pa, adjust the substrate bias voltage to -100V, and bombard the gravure plate with argon ions generated by ionization of argon atoms under this bias condition for 60min to complete the etching and cleaning of the gravure plate surface, and obtain the etched and cleaned gravure plate;

[0123] (3) Taking the above-mentioned gravure plate after etching and cleaning, a layer of chromium is plated as a base layer using a HiPIMS power supply and a high-purity chromium target with a purity of not less than 99.9% under the condition of passing argon gas (argon gas flow rate is 200 sccm). The deposition time of the base layer is 30 min to obtain a first intermediate plate. The operating power of the HiPIMS power supply is 10 kW, and the substrate bias voltage is -300 V;

[0124] (4) Take the first intermediate plate mentioned above, and under the condition of introducing nitrogen (nitrogen flow rate is 20sccm), use HiPIMS power supply and a high purity chromium target with purity not less than 99.9% to plate a layer of chromium nitride as a wear-resistant layer to obtain a finished gravure plate, wherein the time for plating the chromium nitride layer using HiPIMS power supply is 30 minutes, the working power of HiPIMS power supply is 10kW, and the substrate bias is -300V.

[0125] Test Case

[0126] The finished gravure printing plates prepared in Examples 1-2 and Comparative Examples 1-4 were respectively tested in the following order:

[0127] (1) Ball pit test

[0128] The ball pit method is used to measure the film thickness. The ball pit method is a simple and practical method for testing the coating thickness. The coating surface is ball milled using a ball pit meter. After ball milling, a ball pit is formed on the coating sample. Through a digital CCD microscope, combined with intelligent measurement and analysis software, the coating thickness can be quickly and accurately obtained.

[0129] (2) Roughness test

[0130] The roughness of the film layer is measured using a roughness meter. When measuring the surface roughness of the sample, the sensor is placed on the surface of the sample to be measured, and the driving mechanism inside the instrument drives the sensor to slide along the surface to be measured at a constant speed. The sensor senses the roughness of the surface to be measured through the built-in sharp stylus. At this time, the roughness of the sample surface to be measured causes the stylus to displace, and this displacement changes the inductance of the sensor inductor coil, so that the output end of the phase-sensitive rectifier generates an analog signal proportional to the roughness of the surface to be measured. After amplification and level conversion, the signal is sent to the data acquisition system. The DSP chip performs digital filtering and parameter calculation on the collected data. The measurement results are read out on the LCD display, which can be stored or output on a printer.

[0131] (3) Scratch test

[0132] The detection scheme of film layer bonding strength is to use material surface performance tester for testing. The test conditions are diamond indenter cone angle of 120°, tip radius of 200μm, and loading force adjustable in the range of 0-50N. The load is continuously added to the stylus (diamond indenter) at a speed in the range of 0-50N / min through the automatic loading mechanism. At the same time, the sample is moved to make the stylus scratch across the coating surface. The scratch length is 5-10mm. By obtaining the acoustic emission signal and friction force and friction coefficient change signal when the coating falls off, the critical bonding strength between the coating and the substrate is obtained.

[0133] (4) Hardness test

[0134] The Vickers hardness is tested using a microhardness tester. A 25gf (0.245N) indenter is pressed into the sample surface, held for 10 seconds, and then removed. The diagonal length of the indentation is measured to obtain the Vickers hardness of the film. The test is then repeated at 5 points, and the average value is taken as the final Vickers hardness value of the film.

[0135] (5) Surface morphology observation

[0136] SEM (scanning electron microscope) was used to observe the surface morphology and microstructure of the samples, including crystal structure, grain size, fiber structure, etc.

[0137] The test results are shown in Table 1.

[0138] Table 1 Test results of finished gravure plates

[0139]

[0140] The above test results show that by adopting the preparation method provided by the present invention, a composite wear-resistant coating is plated on the surface of the gravure plate using a combination of high-power pulsed magnetron sputtering technology and medium-frequency magnetron sputtering technology, thereby achieving high density and high film-base bonding strength of the composite wear-resistant coating, while also achieving high deposition efficiency that is not available with a single magnetron sputtering technology.

[0141] Moreover, through ball pit test, roughness test, scratch test, hardness test, surface morphology observation and other analyses, it was found that the composite wear-resistant coating prepared by HiPIMS and MFMS technology has a dense structure and strong film-base bonding. After on-machine printing test, the printing durability level is relatively high, which is better than the coating made by single magnetron sputtering technology.

[0142] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A wear-resistant coating, characterized in that: The wear-resistant coating includes a base layer plated on the surface of a substrate by a high-power pulsed magnetron sputtering method, an intermediate layer plated on the surface of the base layer by a first intermediate frequency magnetron sputtering method, and a wear-resistant layer plated on the surface of the intermediate layer by a second intermediate frequency magnetron sputtering method.

2. The wear-resistant coating according to claim 1, characterized in that: The primer layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer; and / or, the intermediate layer is selected from at least one of a chromium layer, a titanium layer, an aluminum layer, a calcium layer and a boron layer; And / or, the wear-resistant layer is selected from at least one of a chromium nitride layer, a titanium nitride layer, an aluminum nitride layer, a calcium nitride layer and a boron nitride layer.

3. A method for preparing a gravure plate wear-resistant coating, characterized in that: The steps include: Take the gravure plate and use high-power pulsed magnetron sputtering technology to plate the bottom layer to obtain the first intermediate plate; Taking the first intermediate plate, and using the first intermediate frequency magnetron sputtering technology to plate an intermediate layer on the surface of the base layer, to obtain a second intermediate plate; The second intermediate plate is taken, and a wear-resistant layer is plated on the surface of the intermediate layer by using a second medium-frequency magnetron sputtering technology.

4. The preparation method according to claim 3, characterized in that: The conditions of the high-power pulsed magnetron sputtering method include at least one of the following: The deposition temperature is 150°C to 160°C; and / or, the deposition time is 30 min to 40 min; And / or, the power supply has an operating power of 10kW to 15kW; And / or, the substrate bias voltage is -300V to -400V.

5. The preparation method according to claim 3, characterized in that: The conditions of the first medium frequency magnetron sputtering method include at least one of the following: The deposition temperature is 150°C to 160°C; and / or, the deposition time is 40 to 50 minutes; And / or, the power supply has an operating power of 15kW to 25kW; And / or, the substrate bias voltage is -30V to -80V.

6. The preparation method according to claim 3, wherein the conditions of the second medium frequency magnetron sputtering method include at least one of the following: The deposition temperature is 150°C to 160°C; and / or, the deposition time is 60 min to 70 min; And / or, the power supply has an operating power of 15kW to 25kW; And / or, the substrate bias voltage is -30V to -80V.

7. The preparation method according to any one of claims 3 to 6, characterized in that: When preparing the bottom layer and the middle layer, argon gas is introduced into the working chamber, and the argon gas flow rate is 200 sccm to 400 sccm; And / or, when preparing the wear-resistant layer, nitrogen gas is introduced into the working chamber, and the nitrogen gas flow rate is 20 sccm to 40 sccm.

8. The preparation method according to any one of claims 3 to 6, characterized in that: Before the high-power pulsed magnetron sputtering method is used to plate the base layer, the method further includes the steps of sequentially performing ultrasonic cleaning, drying, dust removal and etching cleaning on the gravure plate; Optionally, the etching and cleaning process includes: The dust-free gravure plate is placed in a working chamber and evacuated until the vacuum degree in the working chamber is no higher than 1.0×10 - 3 Pa, and the temperature in the working chamber is set to 150°C to 160°C; Argon gas is introduced into the working chamber until the pressure in the working chamber is not less than 0.5 Pa, the substrate bias voltage is set to -100V to -150V, and the gravure plate is bombarded with argon ions for 60min to 90min under the bias voltage condition.

9. A gravure printing plate, characterized in that: The gravure printing plate comprises a gravure printing plate substrate and a wear-resistant coating, wherein the wear-resistant coating comprises the wear-resistant coating according to claim 1 or 2 or the wear-resistant coating prepared by the preparation method according to any one of claims 3 to 8; Preferably, the gravure printing plate substrate comprises a nickel gravure printing plate and / or a copper gravure printing plate.

10. Use of the gravure printing plate according to any one of claims 2 to 6 or the gravure printing plate prepared by the preparation method according to any one of claims 7 to 9 in banknote printing.