Ion beam induced maskless deposition method and application

Through the ion beam-induced maskless deposition method, the focusing ion beam and three-electrode electrochemical system is used to solve the problems of cumbersome and low efficiency in traditional processes, and the nano-scale patterning of various solid materials on silicon-based chips is realized. Deposition, with high flexibility and high precision.

CN118979292APending Publication Date: 2024-11-19PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984320.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The patterning deposition process of traditional solid materials is cumbersome, low efficiency and difficult to modify. In particular, the mask preparation, transfer and alignment steps require high accuracy, resulting in insufficient pattern deposition accuracy and efficiency.

Method used

The ion beam-induced maskless deposition method is adopted to form a preset pattern on the silicon-based substrate by focusing ion beams, and a three-electrode electrochemical system is used to deposit solid materials under the external electric field, avoiding traditional mask preparation and Transfer steps to achieve flexible patterned deposition.

Benefits of technology

The process flow is simplified, the flexibility and accuracy of pattern deposition is improved, and nano-scale patterned deposition of a variety of solid materials can be realized on silicon-based chips. The pattern can be modified at any time before and after deposition, which significantly improves processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979292A_ABST
    Figure CN118979292A_ABST
Patent Text Reader

Abstract

The invention discloses an ion beam induced maskless deposition method and application, and relates to the technical field of solid material nanometer pattern deposition, the ion beam induced maskless deposition method comprises the following steps: obtaining a substrate, the surface of the substrate being partially covered with a metal electrode; dropwise adding a solution in which a to-be-deposited substance is dissolved on the substrate to form a liquid pool, wherein the liquid pool at least partially covers the surface of the metal electrode; performing irradiation treatment on the liquid pool by using a focused ion beam, so that the solution in the liquid pool directionally flows on the surface of the substrate to form a preset pattern; and constructing a three-electrode electrochemical system on the liquid pool and the metal electrode by using a probe, so that the to-be-deposited substance in the preset pattern is deposited under the action of an external electric field to form a solid material preset pattern. According to the technical scheme provided by the invention, simple, flexible and accurate patterned deposition of the solid material on the surface of the substrate can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid material nano-pattern deposition, and in particular to an ion beam induced maskless deposition method and application thereof. Background Art

[0002] Patterned deposition of solid materials refers to the deposition of micro-nano patterns with designed geometric structures on silicon-based solid substrates. This technology is of great significance in the fields of micro-nano device manufacturing, integrated circuit technology, etc. Solid materials include inorganic metals, metal organic complexes and other materials. Silicon-based substrates can be prepared by standard silicon-based semiconductor processes.

[0003] In the traditional integrated circuit and micro-nano device manufacturing process, the patterned deposition of solid materials usually involves multiple steps such as mask preparation, material deposition, pattern transfer / etching, and post-processing. By preparing a thin film cover layer with a designed pattern, a specific area of ​​the substrate is protected, thereby realizing subsequent patterned deposition, etching, and other processing of the silicon-based substrate. This method has three shortcomings: 1. The process is cumbersome. For example, mask preparation requires pattern design, mask manufacturing, mask transfer, mask alignment, and other processes. Any problem in any step will directly affect the accuracy and effect of the final patterned deposition of solid materials. 2. Low processing efficiency. The traditional deposition process has cumbersome steps, and multiple transfers and alignments have extremely high requirements for operating accuracy. Therefore, it often takes several weeks of iteration cycles from pattern design to solid pattern deposition completion and characterization. 3. After processing, there is a lack of the ability to modify on demand. Once the mask is processed, the pattern of subsequent solid deposition / etching is fixed, and it is difficult to modify the target pattern on demand.

[0004] Therefore, how to achieve simple, flexible and precise patterned deposition of various solid materials on the surface of silicon-based chips is a technology that needs to be developed urgently. Summary of the invention

[0005] The main purpose of the present invention is to propose an ion beam induced maskless deposition method and application, aiming to solve the problems of poor precision, low efficiency and inability to modify caused by mask preparation in the prior art.

[0006] To achieve the above object, on the one hand, the present invention provides an ion beam induced maskless deposition method, comprising the following steps:

[0007] Obtaining a substrate, wherein a surface of the substrate is partially covered with a metal electrode;

[0008] Dropping a solution containing a substance to be deposited on the substrate to form a liquid pool, wherein the liquid pool at least partially covers the surface of the metal electrode;

[0009] The liquid pool is irradiated with a focused ion beam to make the solution in the liquid pool flow in a directional manner on the surface of the substrate to form a preset pattern;

[0010] A three-electrode electrochemical system is constructed on the liquid pool and the metal electrode by using a probe, so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid materials.

[0011] In some embodiments, the step of constructing a three-electrode electrochemical system on the liquid pool and the metal electrode using a probe to deposit the material to be deposited in the preset pattern under the action of an external electric field to form a preset pattern of solid material comprises:

[0012] Connecting the working electrode probe to the surface of the metal electrode, and immersing the counter electrode probe and the reference electrode probe into the liquid pool respectively,

[0013] Connect the working electrode probe, counter electrode probe and reference electrode probe to the electrochemical workstation.

[0014] Deposition parameters are obtained, and according to the deposition parameters, the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material.

[0015] In some embodiments, the deposition parameters include deposition voltage, deposition time, and open circuit voltage of a reference electrode.

[0016] In some embodiments, the step of irradiating the liquid pool with a focused ion beam to make the solution in the liquid pool flow in a directional manner on the surface of the substrate to form a preset pattern includes:

[0017] Creating a preset pattern on a pattern generator, and setting geometric parameters of the pattern and parameters of the ion beam according to the created preset pattern;

[0018] The liquid pool is irradiated by a focused ion beam, and the focused ion beam drives the solution in the liquid pool to flow in a directional manner, so as to print the preset pattern on the substrate.

[0019] In some embodiments, in the step of creating a preset pattern on a pattern generator and setting geometric parameters of the pattern and parameters of the ion beam according to the created preset pattern,

[0020] The geometric parameters include one or more of length, width, height and radius;

[0021] The parameters of the ion beam include the acceleration voltage of the focused ion beam, the beam current of the focused ion beam, the dwell time of the focused ion beam, the beam spot spacing of the focused ion beam, and the total beam spot amount of the focused ion beam.

[0022] In some embodiments, in the step of irradiating the liquid pool with a focused ion beam, wherein the focused ion beam drives the solution in the liquid pool to flow in a directional manner to print the preset pattern on the substrate,

[0023] The irradiating the liquid pool with a focused ion beam includes irradiating the liquid pool with a focused ion beam perpendicular to an edge of the liquid pool.

[0024] In some embodiments, the focused ion beam comprises a helium ion beam; and / or gallium ions, xenon ions, etc.

[0025] The dose density of the focused ion beam is 1 to 5 ions / nm 2 .

[0026] In some embodiments, the solution containing the material to be deposited comprises a solvent and a solute, wherein the solvent comprises 1-ethyl-3-methylimidazolium trifluoromethylsulfonyl imide salt or 1-ethyl-3-methylimidazolium dicyanamide salt; the solute comprises trifluoromethylsulfonyl imide metal salt; and the concentration of the trifluoromethylsulfonyl imide metal salt in the solution is 6 to 18 mMol / L.

[0027] In some embodiments, the solute also includes an organic complex, wherein the organic complex is an organic complex that can bind to metal ions through coordination; the concentration of the organic complex in the solution is 5 to 15 mMol / L; and the concentration ratio of the metal ions to the organic complex in the solution is 1:1.2.

[0028] On the other hand, the present invention also provides an application of using the ion beam induced maskless deposition method to prepare a memory device.

[0029] In the technical solution of the present invention, the liquid pool is irradiated with a focused ion beam so that the solution in the liquid pool flows in a directional manner on the surface of the substrate to form a preset pattern; then a three-electrode electrochemical system is constructed on the liquid pool and the metal electrode using a probe so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid materials. The complex processes of mask preparation, mask transfer, and mask alignment in traditional micro-nano processing techniques are avoided, and patterned deposition of a variety of solid materials can be achieved by only ion beam-induced liquid film spreading combined with electrochemical constant pressure deposition. The technical solution of the present invention is extremely flexible, and the solid pattern can be modified and reprinted at any time before and after the solution liquid film pattern is printed and deposited. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0031] Figure 1 A flow chart of an ion beam induced maskless deposition method provided in an embodiment of the present invention.

[0032] Figure 2 A top view of a solution droplet addition method on a metal electrode surface of a substrate in an ion beam induced maskless deposition method provided by an embodiment of the present invention;

[0033] Figure 3 An image of a solution droplet pool, a square metal electrode and a silicon dioxide substrate under a helium ion microscope in an ion beam induced maskless deposition method provided in an embodiment of the present invention;

[0034] Figure 4 An image of a liquid film pattern formed on the surface of a metal electrode by a solution film induced by a focused ion beam in the ion beam induced maskless deposition method provided in an embodiment of the present invention, under a helium ion microscope;

[0035] Figure 5 A schematic diagram of the configuration of an electrochemical deposition probe electrode and a working electrode in the ion beam induced maskless deposition method provided by an embodiment of the present invention;

[0036] Figure 6 The present invention provides a silver-tetracyanoquinone complex particle pattern deposited on the surface of a gold electrode in the ion beam induced maskless deposition method provided in an embodiment of the present invention.

[0037] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.

[0040] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0041] Focused ion beam (FIB) is a technology that uses a certain specific ion to focus on a local area of ​​the sample surface for scanning. The interaction between ion beam and materials is complex, and generally has three important effects. First, the ions that have been subjected to a high acceleration voltage (usually on the order of 10kV) have a high kinetic energy. After entering the surface, the kinetic energy carried by the ions is transferred to the nuclei of the atoms of the sample material and their extranuclear electrons through collision. The energy transferred to the extranuclear electrons can cause the electrons to break away from their original orbits and enter the vacuum to become secondary electrons, which can be collected by a specific device and, after complex signal processing, form an image that can reflect the surface morphology and material information of the sample, which is the imaging function of the ion beam; in addition, the kinetic energy of the ions is transferred to the nuclei, which can cause the displacement of atoms to sputter off the sample, thereby achieving the etching processing function of the ion beam; finally, the ion beam carries a positive charge and can excite electrons to escape from the sample and leave holes, so continuous ion beam irradiation can deposit positive charges locally on the sample surface.

[0042] In existing technologies, the main functions of focused ion beams include: imaging, etching, and deposition / enhanced etching.

[0043] As mentioned above, the imaging and etching functions of the ion beam come from the kinetic energy carried by the ions being transferred to the extranuclear electrons and nuclei of the target atoms, causing the electrons to escape from the sample, and the sputtering of surface atoms to achieve subtractive processing on the surface of the solid substrate.

[0044] In the existing technology, the patterned deposition of solid materials can also be achieved by using the etching function of ion beams to process masks. The technical concept is as follows: first, a layer of dry film for protection is covered on the solid surface to be processed, and then the dry film is partially etched by the etching function of the ion beam to obtain a mask with a target pattern, and then a certain deposition system is used to deposit materials on the solid substrate partially covered by the dry film, and finally the dry film is removed by a stripping process to obtain a solid substrate with patterned deposition. The essence of this type of technology is still the sputtering etching function of the ion beam.

[0045] The ion beam induced maskless deposition method provided in the embodiment of the present invention is different from the traditional method that relies on the sputtering etching function caused by the kinetic energy transfer of the focused ion beam. Instead, it utilizes its special charging effect to provide precise driving force for the liquid on the surface of the solid substrate to achieve solution pattern printing, and combines with the electrochemical process to achieve maskless deposition of solid materials.

[0046] Specifically, on the one hand, an embodiment of the present invention provides an ion beam induced maskless deposition method, see Figure 1 , including the following steps:

[0047] Step S1, obtaining a substrate, wherein a surface of the substrate is partially covered with a metal electrode.

[0048] In this step, the substrate can be a solid substrate, which is an insulating material substrate with a surface metal electrode prepared by a standard silicon-based semiconductor process. The solid substrate can be exemplarily: a silicon dioxide substrate with a gold layer deposited on the surface or one of other insulating substrates (such as resin). When the solid substrate is a silicon dioxide substrate with a gold layer deposited on the surface, the substrate can be pretreated in advance: acetone, ethanol, and deionized water are used to successively wet the substrate and each time it is cleaned in an ultrasonic cleaning machine for 10 minutes; the surface of the substrate is washed with a nitrogen gas flow to remove residual liquid.

[0049] Step S2, dripping a solution containing the substance to be deposited onto the substrate to form a liquid pool, wherein the liquid pool at least partially covers the surface of the metal electrode.

[0050] The prepared solution is dripped near the surface of the metal electrode using a micro-injection capillary. The solution droplet needs to be in contact with the electrode part, such as Figure 2 The added solution droplet serves as a liquid reservoir for subsequent focused ion beam scanning to induce the formation of a solution film pattern.

[0051] In practical applications, a silicon-based chip with a prefabricated microfluidic structure inside can also be used to inject solution samples through the solution injection port, and use the microfluidic channel to drain the solution to a series of outlet positions in the target area as a subsequent ion beam-induced liquid pool, thereby achieving array-based precise control of the subsequent patterned deposition positions of solid materials.

[0052] Step S3, irradiating the liquid pool with a focused ion beam to make the solution in the liquid pool flow in a directional manner on the surface of the substrate to form a preset pattern;

[0053] In this step, the graphic scanning control system can be used to control the ion optical system to scan the liquid droplet pool on the surface of the metal electrode. The interaction between the focused ion beam and the solid and liquid materials can be used to induce the solution in the liquid pool to flow and spread in a directional manner on the surface of the metal electrode, forming a nanoscale solution film with a designed pattern.

[0054] Specifically, the graphic scanning control system can realize the design of scanning graphics with given dimensions and geometric features, such as lines, rectangles, stars, circles, etc. It can also convert externally imported binary images into corresponding scanning graphics and allow users to set relevant parameters of ion beam scanning to generate patterns.

[0055] The parameters related to the scanning pattern include: scanning area length, width, radius, angle, scanning direction, scanning mode, number of scanning patterns, scanning pattern sequence and spatial position relationship. It should be noted that the above parameters related to the scanning pattern need to be adjusted in combination with the appropriate parameter range of the ion beam and the complexity and size of the target processing pattern; in addition, the position of the scanning pattern needs to be set at the edge of the droplet on the metal electrode surface.

[0056] Step S4, using a probe to construct a three-electrode electrochemical system on the liquid pool and the metal electrode, so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material.

[0057] Specifically, the silicon dioxide substrate with the solution film pattern printed on the surface of the metal electrode is transferred out of the vacuum sample chamber where the ion optical system is located; the sample is placed on a sample stage with three probe electrodes and fixed; the probe connected to the working electrode of the electrochemical workstation is placed in contact with the metal electrode; the other two probes are respectively connected to the counter electrode and the reference electrode of the workstation and immersed in the large droplet as a liquid pool; for specific settings, see Figure 5 According to the requirements of the actual application, the prepared silicon dioxide chip can be properly rinsed.

[0058] In one embodiment, step S4 may be specifically that the step of constructing a three-electrode electrochemical system on the liquid pool and the metal electrode using a probe so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material comprises:

[0059] Connecting the working electrode probe to the surface of the metal electrode, and immersing the counter electrode probe and the reference electrode probe into the liquid pool respectively,

[0060] Connect the working electrode probe, counter electrode probe and reference electrode probe to the electrochemical workstation.

[0061] Deposition parameters are obtained, and according to the deposition parameters, the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material.

[0062] In some embodiments, the deposition parameters include deposition voltage, deposition time, and open circuit voltage of the reference electrode. According to the different reduction potentials of the deposited solid materials, the appropriate potential difference between the working electrode and the counter electrode is selected to ensure efficient deposition of the target solid material on the surface of the metal electrode; according to different deposition pattern sizes and required particle sizes, the appropriate deposition time, deposition voltage, reactant concentration ratio, and solvent type are set.

[0063] Taking the deposition of silver tetracyanoquinone complex as an example, the reduction potential selected according to the electrochemical reaction and other experimental system characteristic parameters is -0.1V vsAg 0 , deposited 500 μm 2 The constant pressure deposition time selected for the medium-sized particle pattern was 360 seconds.

[0064] In some embodiments, the step of irradiating the liquid pool with a focused ion beam to make the solution in the liquid pool flow in a directional manner on the surface of the substrate to form a preset pattern includes:

[0065] Creating a preset pattern on a pattern generator, and setting geometric parameters of the pattern and parameters of the ion beam according to the created preset pattern;

[0066] The liquid pool is irradiated by a focused ion beam, and the focused ion beam drives the solution in the liquid pool to flow in a directional manner, so as to print the preset pattern on the substrate.

[0067] In some embodiments, in the step of creating a preset pattern on a pattern generator and setting geometric parameters of the pattern and parameters of the ion beam according to the created preset pattern,

[0068] The geometric parameters include one or more of length, width, height and radius;

[0069] The parameters of the ion beam include the acceleration voltage of the focused ion beam, the beam current of the focused ion beam, the dwell time of the focused ion beam, the beam spot spacing of the focused ion beam, and the total beam spot amount of the focused ion beam.

[0070] In some embodiments, the step of irradiating the liquid pool with a focused ion beam, and driving the solution in the liquid pool to flow in a directional manner to print the preset pattern on the substrate, comprises irradiating the liquid pool with a focused ion beam perpendicular to the edge of the liquid pool. The focused ion beam is used to scan the edge of the liquid pool to induce the liquid film to spread and flow: the scanning direction of the ion beam is perpendicular to the contact line of the droplet-liquid pool and is outward, the scanning starting position is located within the contact line of the liquid pool, adjacent scanning patterns are connected end to end, and the entire scanning pattern area is gradually scanned to induce the liquid to spread over the entire area.

[0071] In some embodiments, the focused ion beam comprises a helium ion beam; the dose density of the focused ion beam is 1 to 5 ions / nm 2 The irradiation dose density of the helium ion beam should be between 1 and 5 ions / nm2. A dose below this range may not be sufficient to completely induce the patterning and spreading of the solution. A dose exceeding this range may cause a decrease in patterning accuracy, which may damage the solution and solid sample, and exert the etching processing function of the focused ion beam.

[0072] In some embodiments, the solution containing the material to be deposited comprises a solvent and a solute, wherein the solvent comprises 1-ethyl-3-methylimidazolium trifluoromethylsulfonyl imide salt or 1-ethyl-3-methylimidazolium dicyanamide salt; the solute comprises trifluoromethylsulfonyl imide metal salt; and the concentration of the trifluoromethylsulfonyl imide metal salt in the solution is 6 to 18 mMol / L.

[0073] In some embodiments, the solute also includes an organic complex, wherein the organic complex is an organic complex that can bind to metal ions through coordination; the concentration of the organic complex in the solution is 5 to 15 mMol / L; and the concentration ratio of the metal ions to the organic complex in the solution is 1:1.2.

[0074] Different solvent and solute combinations can be selected according to specific functional requirements. For example, when the ion beam induced solid material maskless precision deposition method provided in the present application example is used for random access memory (RAM) device preparation, a mixed solution of target metal and tetracyanobenzoquinone can be selected.

[0075] It should be noted that in the embodiment of the present invention, a three-electrode electrochemical system is constructed on the liquid pool and the metal electrode using a probe, so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material. Metal materials, organic matter, metal-organic complexes, etc. can be deposited to form a patterned solid material.

[0076] On the other hand, an embodiment of the present invention further provides an application of using the ion beam induced maskless deposition method to prepare a memory device. Exemplarily, the ion beam induced maskless deposition method can be used to prepare a random access memory device (RAM).

[0077] In summary, compared with the existing solid micro-nano pattern deposition technology, this application has the following advantages:

[0078] (1) The ion beam induced solid patterned deposition method provided in the embodiment of the present application does not require the pre-preparation of a mask having a target pattern, thereby greatly reducing the time and economic cost of solid patterned deposition;

[0079] (2) The ion beam induced solid patterned deposition method provided in the embodiment of the present application has simplified steps, avoiding the complex processes such as mask preparation, mask transfer, and mask alignment in the traditional micro-nano processing technology. It only requires ion beam induced liquid film spreading combined with electrochemical constant pressure deposition to achieve patterned deposition of various solid materials;

[0080] (3) The ion beam induced solid patterned deposition method provided in the embodiment of the present application has extremely strong flexibility, and the solid pattern can be modified and reprinted at any time before and after the solution film pattern printing and deposition;

[0081] (4) The ion beam induced solid pattern deposition method provided in the embodiment of the present application can achieve nanometer-level patterning accuracy and realize the printing of complex solid patterns across scales. Maskless printing of various solid materials can be realized on silicon-based chips, with a pattern accuracy of 100nm and a maximum pattern size of 100μm. It can be used in the fields of micro-nano circuit elements, sensor circuits, integrated circuit processing, etc.

[0082] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0083] Example 1

[0084] This embodiment uses a silicon dioxide solid chip with a gold electrode evaporated on the surface, 1-ethyl-3-methylimidazolium trifluoromethylsulfonyl imide ionic liquid as solvent, silver trifluoromethylsulfonyl imide and tetracyanoquinone (TCNQ) as solute, and a helium ion microscope.

[0085] This embodiment includes the following steps:

[0086] (1) Prepare a solid substrate: Purchase a silicon dioxide substrate with a gold electrode array deposited on the surface prepared by a standard semiconductor process. The substrate is 1 cm long, 1 cm wide, and 1 mm thick. The gold electrode is 500 μm long, 500 μm wide, and 30 nm thick. Use an ultrasonic cleaner to immerse the above substrate in acetone, ethanol, and deionized water for ultrasonic cleaning for 10 minutes each to remove organic impurities that may remain on the surface. Finally, use nitrogen to purge the substrate to remove residual water and other liquids.

[0087] (2) Prepare solution samples: Purchase commercial ionic liquid 1-ethyl-3-methylimidazolium trifluoromethylsulfonyl imide and dry it in a vacuum cabinet at 80 degrees Celsius for more than 48 hours to remove residual moisture and volatile impurities. Purchase commercial silver trifluoromethylsulfonyl imide salt and TCNQ, and prepare the solution with the dry ionic liquid to make the silver ion concentration reach 6mMol / L and the TCNQ concentration reach 5mMol / L.

[0088] (3) Sample preparation: Use a micro-injection capillary to dip a small amount of the above solution and drop it on the surface of the above solid substrate. Use a micro-injection capillary to drop a drop of the freshly prepared solution sample on the surface of the silicon-based chip as described above. Make part of the droplet directly contact the surface metal electrode, see Figure 2 This large droplet serves as a liquid pool for subsequent ion beam-induced solution film pattern printing. In order to minimize the dissolution of potential water molecules and other volatile impurities, the above sample preparation process is completed under a nitrogen atmosphere as much as possible.

[0089] (4) Sample delivery: The prepared solid substrate is fixed on a T-shaped bracket and mounted on the sample stage of the helium ion microscope, and finally delivered into the vacuum sample chamber of the helium ion microscope.

[0090] Adjust the scanning parameters of the ion optical system to a level suitable for observation and imaging, including contrast, focal length, magnification, ion beam centering, astigmatism, etc., until the image contrast in the field of view is moderate, the sample morphology is clear, and the edges are sharp. Only then can the subsequent ion beam induced liquid film patterning steps be carried out. Figure 3 Detailed description of the helium ion microscope imaging field of view.

[0091] See also Figure 3 , where the dark circular area makes the image of the solution droplet under the helium ion microscope ( Figure 3 Solution droplets in the middle), the gray background is the silicon dioxide substrate image ( Figure 3 The light grey square area is the metal electrode image ( Figure 3 “Metal Electrode”).

[0092] (5) Ion beam induced liquid film: First, adjust the magnification of the helium ion microscope and move the ion beam scanning area position. Select an area with a window size of approximately 30 μm, which contains an edge of the solution droplet on the metal electrode surface as the starting position for inducing the liquid film pattern.

[0093] In the graphic scanning control system, a rectangle with a width of 5μm and a length of 100μm and a "PKU" letter pattern with a height of 5μm are designed; the scanning direction is set from the inside of the solution droplet to the outside horizontally and from the bottom to the top vertically; the acceleration voltage is 30kV; the beam current is around 0.9 to 1pA; the dwell time is 2μs; and the beam spot spacing is 2nm. A rectangular pattern with a longer length can be completed by splicing multiple rectangular patterns with a length of 20μm end to end, and scanning them one by one according to the scanning sequence set from near to far from the droplet pool.

[0094] Finally, after completing the scanning parameters and mode settings and confirming that they are correct, the graphic scanning control system is used to control the ion optical system to scan the droplet pool and solid substrate. The special charging effect of the focused helium ion beam is used to induce the solution to spread in a directional manner on the substrate surface and form a nanoscale solution film covering the scanning pattern area. Figure 4 The solution liquid film patterning induced by focused ion beam printing is explained.

[0095] See also Figure 4 The dark gray part in the figure is the solution film pattern induced by the ion beam ( Figure 4 The light grey part is the gold electrode background ( Figure 4 "Metal Electrode" area).

[0096] (6) Solid pattern deposition: The substrate on which the solution film pattern is induced is transferred from the vacuum sample chamber of the helium ion microscope to the external probe electrode sample stage; the three probes on the sample stage are connected to the three standard electrodes of a commercial electrochemical workstation; the probe connected to the working electrode contacts the metal electrode deposited on the silicon dioxide substrate, and the two probes connected to the counter electrode and the reference electrode are immersed in the large droplet of the solution; Figure 5 The setup of the electrode probe as well as the liquid sample and solid substrate is described.

[0097] See also Figure 5 , the white area is the surface of the silicon dioxide substrate; the oblique line shaded area is the metal electrode in contact with the solution droplet; the dot shaded area is the solution droplet and the solution film pattern. Note that the film pattern needs to be printed on the surface of the metal electrode to facilitate the electrochemical deposition of solid materials; the three black solid triangles are schematic diagrams of the positions where the probe electrodes are applied.

[0098] For the silver ion and TCNQ mixed solution used in this embodiment, the reference voltage is about -0.001V after experimental calibration, and the deposition voltage is selected as -0.1V to ensure that the current system liquid film is not affected while efficiently depositing the target solid material, and the deposition time is selected as 360 seconds. Using the above parameters, the solution pattern is deposited as a solid particle pattern of the silver-tetracyanoquinone complex.

[0099] (7) Post-treatment: The processed solid substrate is immersed in deionized water and ultrasonically cleaned for 10 minutes to obtain a sample with a solid deposition pattern of the target material on the surface. The sample is observed under a commercial optical microscope, and it can be seen that blue-green silver-tetracyanobenzoquinone particles with a designed pattern are deposited on the surface of the golden metal electrode; combined with Figure 6 Provide explanation.

[0100] See also Figure 6 , the golden background is the gold metal electrode surface ( Figure 6 “Metal electrode” area); the blue-green particles are silver-tetracyanoquinone complex precipitation ( Figure 6 "Solid Particle Precipitation Pattern" area), it is noted that the solid pattern is consistent with the geometric features and dimensions of the above-designed pattern.

[0101] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. An ion beam induced maskless deposition method, characterized in that: The following steps are involved: obtaining a substrate, wherein a surface of the substrate is partially covered with a metal electrode; Dropping a solution containing a substance to be deposited onto the substrate to form a liquid pool, wherein the liquid pool at least partially covers the surface of the metal electrode; irradiating the liquid pool with a focused ion beam to cause the solution in the liquid pool to flow directionally on the surface of the substrate to form a preset pattern; A three-electrode electrochemical system is constructed on the liquid pool and the metal electrode using a probe, so that the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material.

2. The ion beam induced maskless deposition method according to claim 1, wherein: The step of constructing a three-electrode electrochemical system on the liquid pool and the metal electrode using a probe to deposit the material to be deposited in the preset pattern under the action of an external electric field to form a preset pattern of solid material includes: Connect the working electrode probe to the surface of the metal electrode, immerse the counter electrode probe and the reference electrode probe in the liquid pool respectively, Connect the working electrode probe, counter electrode probe and reference electrode probe to the electrochemical workstation. Deposition parameters are acquired, and according to the deposition parameters, the material to be deposited in the preset pattern is deposited under the action of an external electric field to form a preset pattern of solid material.

3. The ion beam induced maskless deposition method according to claim 2, characterized in that: The deposition parameters include deposition voltage, deposition time and open circuit voltage of a reference electrode.

4. The ion beam induced maskless deposition method according to claim 1, wherein: The step of irradiating the liquid pool with a focused ion beam to make the solution in the liquid pool flow directionally on the surface of the substrate to form a preset pattern includes: Creating a preset pattern on a pattern generator, and setting geometric parameters of the pattern and parameters of the ion beam according to the created preset pattern; The liquid pool is irradiated by using a focused ion beam, and the focused ion beam drives the solution in the liquid pool to flow in a directional manner, so as to print the preset pattern on the substrate.

5. The ion beam induced maskless deposition method according to claim 4, characterized in that: In the step of creating a preset pattern on the pattern generator and setting the geometric parameters of the pattern and the parameters of the ion beam according to the created preset pattern, The geometric parameters include one or more of length, width, height, and radius; The parameters of the ion beam include the acceleration voltage of the focused ion beam, the beam current of the focused ion beam, the dwell time of the focused ion beam, the beam spot spacing of the focused ion beam, and the total beam spot volume of the focused ion beam.

6. The ion beam induced maskless deposition method according to claim 4, characterized in that: In the step of irradiating the liquid pool with a focused ion beam, wherein the focused ion beam drives the solution in the liquid pool to flow in a directional manner so as to print the preset pattern on the substrate, The irradiating the liquid pool with a focused ion beam includes irradiating the liquid pool with a focused ion beam perpendicular to an edge of the liquid pool.

7. The ion beam induced maskless deposition method according to claim 1, wherein: The focused ion beam comprises a helium ion beam; and / or, The dose density of the focused ion beam is 1 to 5 ions / nm 2 .

8. The ion beam induced maskless deposition method according to claim 1, wherein: The solution containing the material to be deposited includes a solvent and a solute, wherein the solvent includes 1-ethyl-3-methylimidazolium trifluoromethylsulfonyl imide salt or 1-ethyl-3-methylimidazolium dicyanamide salt; the solute includes a trifluoromethylsulfonyl imide metal salt; and the concentration of the trifluoromethylsulfonyl imide metal salt in the solution is 6 to 18 mMol / L.

9. The ion beam induced maskless deposition method according to claim 8, characterized in that: The solute also includes an organic complex, wherein the organic complex is an organic complex that can combine with metal ions through coordination; the concentration of the organic complex in the solution is 5 to 15 mMol / L; and the concentration ratio of the metal ions to the organic complex in the solution is 1:1.

2.

10. An application, characterized in that: The ion beam induced maskless deposition method according to any one of claims 1 to 9 is used to prepare a memory device.