Preparation method of offset printing paper
Through the combination of mixed slurry and auxiliary materials of coniferous wood, broadleaf wood and bamboo fiber chemical mechanical pulp, the problems of rough surface and fluorescent whitening agent of offset printing paper are solved, and high-quality, visually safe offset printing paper is prepared, achieving printing effect and cost increase.
Patent Information
- Application Number
- CN202411142162.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-19
AI Technical Summary
When using bamboo fiber chemical mechanical pulp, existing offset printing paper can easily lead to roughness, hair loss and powder loss on the paper surface. The use of fluorescent whitening agent is not conducive to vision health, resulting in poor printing effect and quality problems.
Using a mixed slurry of coniferous wood chemical pulp, broad-leaved wood chemical pulp and bamboo fiber chemical mechanical pulp, combined with calcium carbonate, polymer aluminum chloride and other auxiliary materials, through refining, slurrying, slurrying, crushing, pressing, drying and glue filling processes , prepare offset printing paper without fluorescent whitening agent to improve paper surface smoothness and surface strength.
It realizes smooth, hair-free and powder-free offset printing paper, improves printing effect and vision safety, reduces production costs and transportation costs, and ensures the quality stability of printed materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pulping and papermaking, and in particular relates to a method for preparing offset printing paper. Background Art
[0002] Offset printing paper has a smooth surface, high printing clarity and good color reproduction. It is suitable for printing monochrome or multi-color high-end color prints, such as color pictorials, albums, posters, color printed trademarks, as well as some high-end books, book covers, illustrations, etc.
[0003] Currently, 70g to 120g offset printing paper is widely used in the market, and there are also high-weight offset printing papers of 150g to 300g, which are mainly used for offset printing machines or other printing machines. Some offset printing papers on the market have a high whiteness and use a large amount of whitening agents, which increases the treatment load of papermaking wastewater and is also not good for readers' eyesight health.
[0004] Bamboo fiber chemical mechanical pulp, also known as bamboo fiber chemimechanical pulp, is a kind of pulp made from bamboo through mechanical pulping and chemical treatment, with low production cost. In the existing offset printing paper process, adding some bamboo fiber chemical mechanical pulp not only improves the bulk, but also greatly reduces the production cost. However, when the amount of bamboo fiber chemical mechanical pulp added exceeds 20% of the total amount of pulp, it is easy to cause the surface of the paper to be rough and smooth, which is easy to cause the problem of pulling hair; at the same time, hair and powder will fall off, and the coating and fibers on the surface of the paper will be easily pulled up by the rubber cloth during printing, resulting in the inability to transfer part of the image to the paper normally, causing the problem of plate sticking; sometimes the quantitative fluctuations cause the thickness of the paper to be uniform, and it is easy to have eight-shaped wrinkles during the printing process, which is not easy to stretch, causing quality problems in market feedback. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a method for preparing offset printing paper, which aims to achieve the following invention objectives: on the basis of a high usage amount of bamboo fiber chemical mechanical pulp, no fluorescent brightener is used, the surface strength is improved, the offset printing paper surface is smooth, does not shed, does not fall off, the surface absorption amount is increased, the printing effect is good, and the fluorescence value is low.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions: Step 1: Refining The coniferous wood chemical pulp, the hardwood wood chemical pulp and the bamboo fiber chemimechanical pulp were refined respectively; the coniferous wood chemical pulp obtained by refining had a beating degree of 33-35oSR, the hardwood chemical pulp had a beating degree of 32-36oSR, and the bamboo fiber chemimechanical pulp had a beating degree of 42-45oSR.
[0007] The pulp obtained after refining is mixed according to the following weight ratio: 15-35 parts of coniferous wood chemical pulp, 30-50 parts of hardwood chemical pulp, and 30-50 parts of bamboo fiber chemical mechanical pulp.
[0008] 8-10% of broken paper can also be added to the slurry. The broken paper refers to waste paper such as paper edges generated in the subsequent production process in this technical solution, which can be recycled.
[0009] The obtained mixed slurry is introduced into a batching tank.
[0010] Step 2: Mix the slurry Add auxiliary materials into the batching tank and stir evenly to obtain the pre-papermaking slurry. The auxiliary materials used include calcium carbonate, calcium carbonate enhancer, polyaluminium chloride (PAC), retention aid, filter aid, bentonite, cationic starch, alkenyl succinic anhydride, dye yellow, bactericide and defoamer.
[0011] The amount of calcium carbonate used is 260-280 kg / ton of paper; the amount of calcium carbonate enhancer used is 1.5-1.8 kg / ton of paper; the amount of polyaluminium chloride used is 3-4 kg / ton of paper; the amount of retention agent used is 0.50-0.62 kg / ton of paper; the amount of filter aid used is 0.38-0.5 kg / ton of paper; the amount of bentonite used is 3.5-4 kg / ton of paper; the amount of cationic starch used is 5.8-6.5 kg / ton of paper; the amount of alkenyl succinic anhydride used is 1.1-1.2 kg / ton of paper; the amount of dye yellow used is 0.45-0.55 kg / ton of paper; the amount of bactericide used is 0.1-0.3 kg / ton of paper; and the amount of defoamer used is 0.1-0.3 kg / ton of paper.
[0012] The calcium carbonate enhancer is prepared by mixing sodium stearate, palmitic acid and lignin in a mass ratio of 7:3:1.
[0013] The retention aid is one or more of polyvinyl alcohol, methyl cellulose and hydroxyethyl cellulose.
[0014] The filter aid is any one of polyethyleneimine (PEI), polyacrylamide (CPAM), and polyamine (PA).
[0015] The bentonite is prepared by mixing modified bentonite, talcum powder and kaolin in a mass ratio of 3:1:0.2; the modified bentonite used is AlCl3 modified bentonite.
[0016] The bactericide is one or more of complex bromine, isothiazolinone, thiocyanate, dithiocyanomethane, 2,2-dibromo-3-cyano-acetamide and halogenated hydantoin.
[0017] The defoaming agent is one or more of polysiloxane, modified polysiloxane, silicone resin, white carbon black, dispersant and stabilizer.
[0018] The polyaluminium chloride (PAC) has a basicity of 40-85%, an insoluble matter content of ≤0.6% and a pH value of 3.5-5.0.
[0019] Step 3: Papermaking The pulp before papermaking is paper-made, and the pulp-to-wire speed ratio is controlled to be 1.012, the retention rate is 68-78%, the white water concentration is 0.2-0.3%, and the wire vacuum degree is -20 to -30 KPa to obtain wet paper.
[0020] Step 4: Pressing The wet paper is pressed to remove moisture through mechanical pressure to make the paper sheets tight and improve the paper surface; the felt tension during the pressing process is 24-28KN / M, the line pressure is 40-60KN / M, and the vacuum degree of the pressing roller is -30 to -40KPa.
[0021] Step 5: Drying The pressed paper is dried at a temperature of 80-130°C, and the moisture content of the dried paper is 6.0-8.0%.
[0022] Step 6: Gluing The dried paper sheets are sizing on the sizing roller, and the sizing amount is 1.8-2.5kg / ton of paper. The surface glue used is one or more of modified starch solution, polyvinyl alcohol PVA, carboxymethyl cellulose CMC, and polyacrylamide PAM.
[0023] Step 7: Post-drying The sizing paper sheets are introduced into a dryer for post-drying at a temperature of 80-110°C and a moisture content of 5-5.5% after drying.
[0024] Step 8: Calendering The paper sheets are introduced into the calender for two calenderings. The calender pressure of the first calendering is 30-35KN, and the calender pressure of the second calendering is 45-55KN.
[0025] The calendered paper sheets are curled and cut to obtain the finished product.
[0026] By adopting the above technical solution, the beneficial effects of the present invention are as follows: 1. The offset printing paper prepared by the present invention has good texture, light weight and thickness, high bulk, reduces the amount of wood fiber used, reduces transportation costs, and reduces production costs.
[0027] 2. The preparation of the invention does not contain fluorescent brightener, and the beige color tone can protect eyesight from harm, especially protect the elderly and children, and is convenient for readers to read and carry.
[0028] 3. The offset printing paper prepared by the present invention based on the high usage of bamboo fiber chemical mechanical pulp has the following characteristics: high smoothness, high opacity, clear printed images, and fully meets the use requirements of high-speed rotary printing presses; the surface strength of the paper is improved, the quality is stable, the thickness is uniform, and the occurrence of folding problems during printing is avoided. DETAILED DESCRIPTION
[0029] Example 1 A method for preparing offset printing paper Step 1: Refining The coniferous wood chemical pulp, the hardwood wood chemical pulp and the bamboo fiber chemimechanical pulp were refined respectively; the coniferous wood chemical pulp obtained by refining had a beating degree of 33oSR, the hardwood chemical pulp had a beating degree of 36oSR, and the bamboo fiber chemimechanical pulp had a beating degree of 42oSR.
[0030] The pulp obtained after refining is mixed according to the following weight ratio: 15 parts of coniferous wood chemical pulp, 40 parts of hardwood chemical pulp, and 35 parts of bamboo fiber chemical mechanical pulp.
[0031] The obtained mixed slurry is introduced into a batching tank.
[0032] Step 2: Mix the slurry Add auxiliary materials into the batching tank and stir evenly to obtain the pre-papermaking slurry. The auxiliary materials used include calcium carbonate, calcium carbonate enhancer, polyaluminium chloride (PAC), retention aid, filter aid, bentonite, cationic starch, alkenyl succinic anhydride, dye yellow, bactericide and defoamer.
[0033] Calculate the amount of auxiliary materials added per ton of paper produced: The amount of calcium carbonate used is 260 kg / ton of paper; the amount of calcium carbonate enhancer used is 1.5 kg / ton of paper; the amount of polyaluminium chloride used is 4 kg / ton of paper; the amount of retention aid used is 0.62 kg / ton of paper; the amount of filter aid used is 0.5 kg / ton of paper; the amount of bentonite used is 3.5 kg / ton of paper; the amount of cationic starch used is 6 kg / ton of paper; the amount of alkenyl succinic anhydride used is 1.1 kg / ton of paper; the amount of dye yellow used is 0.5 kg / ton of paper; the amount of bactericide used is 0.3 kg / ton of paper; and the amount of defoaming agent used is 0.3 kg / ton of paper.
[0034] The calcium carbonate enhancer is prepared by mixing sodium stearate, palmitic acid and lignin in a mass ratio of 7:3:1.
[0035] The retention aid is polyvinyl alcohol.
[0036] The filter aid is polyethyleneimine.
[0037] The bentonite is prepared by mixing modified bentonite, talcum powder and kaolin in a mass ratio of 3:1:0.2; the modified bentonite used is AlCl3 modified bentonite.
[0038] The bactericide is isothiazolinone.
[0039] The defoaming agent is polysiloxane.
[0040] Step 3: Papermaking The pre-papermaking pulp was papered, and the pulp-to-wire speed ratio was controlled to be 1.012, the retention rate was 68%, the white water concentration was 0.2%, and the wire vacuum degree was -20 KPa to obtain wet paper.
[0041] Step 4: Pressing The wet paper is pressed to remove moisture through mechanical pressure to make the paper sheets tight and improve the paper surface; the felt tension during the pressing process is 24KN / M, the line pressure is 40KN / M, and the vacuum degree of the pressing roller is -30KPa.
[0042] Step 5: Drying The pressed paper is dried at a temperature of 80°C, and the moisture content of the dried paper is 8.0%.
[0043] Step 6: Gluing The dried paper sheets are sizing on the sizing roller, and the sizing amount is 2.5kg / ton of paper. The surface glue used is a modified starch solution with a starch solid content of 10% (mass percentage); preparation method: starch is prepared into a solution with a mass percentage concentration of 4%, and gelatinized at a gelatinization temperature of 90°C for 30 minutes.
[0044] Step 7: Post-drying The sizing paper sheets were introduced into a dryer for post-drying at a temperature of 80°C and a moisture content of 5.5% after drying.
[0045] Step 8: Calendering The paper sheets were introduced into the calender for two calenderings. The calender pressure for the first calendering was 30 KN, and the calender pressure for the second calendering was 55 KN.
[0046] The calendered paper sheets are curled and cut to obtain the finished product.
[0047] Example 2 A method for preparing offset printing paper Step 1: Refining The coniferous wood chemical pulp, the hardwood wood chemical pulp and the bamboo fiber chemimechanical pulp were refined respectively; the coniferous wood chemical pulp obtained by refining had a beating degree of 35oSR, the hardwood chemical pulp had a beating degree of 32oSR, and the bamboo fiber chemimechanical pulp had a beating degree of 45oSR.
[0048] The pulp obtained after refining is mixed according to the following weight ratio: 35 parts of coniferous wood chemical pulp, 30 parts of hardwood chemical pulp, and 30 parts of bamboo fiber chemical mechanical pulp.
[0049] The obtained mixed slurry is introduced into a batching tank.
[0050] Step 2: Mix the slurry Add auxiliary materials into the batching tank and stir evenly to obtain the pre-papermaking slurry. The auxiliary materials used include calcium carbonate, calcium carbonate enhancer, polyaluminium chloride (PAC), retention aid, filter aid, bentonite, cationic starch, alkenyl succinic anhydride, dye yellow, bactericide and defoamer.
[0051] Calculate the amount of auxiliary materials added per ton of paper produced: The amount of calcium carbonate used is 280 kg / ton of paper; the amount of calcium carbonate enhancer used is 1.8 kg / ton of paper; the amount of polyaluminium chloride used is 3 kg / ton of paper; the amount of retention aid used is 0.5 kg / ton of paper; the amount of filter aid used is 0.38 kg / ton of paper; the amount of bentonite used is 4 kg / ton of paper; the amount of cationic starch used is 6.5 kg / ton of paper; the amount of alkenyl succinic anhydride used is 1.2 kg / ton of paper; the amount of dye yellow used is 0.45 kg / ton of paper; the amount of bactericide used is 0.1 kg / ton of paper; and the amount of defoaming agent used is 0.1 kg / ton of paper.
[0052] The calcium carbonate enhancer is prepared by mixing sodium stearate, palmitic acid and lignin in a mass ratio of 7:3:1.
[0053] The retention aid is prepared by mixing polyvinyl alcohol and hydroxyethyl cellulose in a mass ratio of 2:1.
[0054] The filter aid is polyacrylamide (CPAM).
[0055] The bentonite is prepared by mixing modified bentonite, talcum powder and kaolin in a mass ratio of 3:1:0.2; the modified bentonite used is AlCl3 modified bentonite.
[0056] The bactericide is 2,2-dibromo-3-cyano-acetamide.
[0057] The defoaming agent is polyether-modified polysiloxane.
[0058] Step 3: Papermaking The pulp before papermaking was papered, and the pulp-to-wire speed ratio was controlled to be 1.012, the retention rate to be 78%, the white water concentration to be 0.3%, the wire vacuum degree to be -30 KPa, to obtain wet paper.
[0059] Step 4: Pressing The wet paper is pressed to remove moisture through mechanical pressure to make the paper sheets tight and improve the paper surface; the felt tension during the pressing process is 28KN / M, the line pressure is 60KN / M, and the vacuum degree of the pressing roller is -40KPa.
[0060] Step 5: Drying The pressed paper is dried at a temperature of 130°C, and the moisture content of the dried paper is 6.0%.
[0061] Step 6: Gluing The dried paper sheets are sizing on the surface on a sizing roller, and the sizing amount is 1.8 kg / ton of paper. The surface glue used is a mixture of modified starch solution and carboxymethyl cellulose solution in a mass ratio of 4:1.
[0062] The modified starch solution has a starch solid content of 11% (mass percentage); the preparation method is as follows: the starch is prepared into a solution with a mass percentage concentration of 6%, and gelatinized at a gelatinization temperature of 95° C. for 20 minutes.
[0063] The concentration of the carboxymethyl cellulose solution is 0.2%.
[0064] Step 7: Post-drying The sizing paper sheets are introduced into a dryer for post-drying at a drying temperature of 110°C and a moisture content of 5% after drying.
[0065] Step 8: Calendering The paper sheets were introduced into the calender for two calenderings. The calender pressure of the first calendering was 35 KN, and the calender pressure of the second calendering was 45 KN.
[0066] The calendered paper sheets are curled and cut to obtain the finished product.
[0067] Example 3 A method for preparing offset printing paper Step 1: Refining The coniferous wood chemical pulp, the hardwood wood chemical pulp and the bamboo fiber chemimechanical pulp were refined respectively; the coniferous wood chemical pulp obtained by refining had a beating degree of 34oSR, the hardwood chemical pulp had a beating degree of 35oSR, and the bamboo fiber chemimechanical pulp had a beating degree of 43oSR.
[0068] The pulp obtained after refining is mixed according to the following weight ratio: 25 parts of coniferous wood chemical pulp, 40 parts of hardwood chemical pulp, and 40 parts of bamboo fiber chemical mechanical pulp.
[0069] The obtained mixed slurry is introduced into a batching tank.
[0070] Step 2: Mix the slurry Add auxiliary materials into the batching tank and stir evenly to obtain the pre-papermaking slurry. The auxiliary materials used include calcium carbonate, calcium carbonate enhancer, polyaluminium chloride (PAC), retention aid, filter aid, bentonite, cationic starch, alkenyl succinic anhydride, dye yellow, bactericide and defoamer.
[0071] Calculate the amount of auxiliary materials added per ton of paper produced: The amount of calcium carbonate used is 270 kg / ton of paper; the amount of calcium carbonate enhancer used is 1.6 kg / ton of paper; the amount of polyaluminium chloride used is 3.6 kg / ton of paper; the amount of retention aid used is 0.58 kg / ton of paper; the amount of filter aid used is 0.42 kg / ton of paper; the amount of bentonite used is 3.7 kg / ton of paper; the amount of cationic starch used is 5.8 kg / ton of paper; the amount of alkenyl succinic anhydride used is 1.1 kg / ton of paper; the amount of dye yellow used is 0.55 kg / ton of paper; the amount of bactericide used is 0.2 kg / ton of paper; and the amount of defoaming agent used is 0.2 kg / ton of paper.
[0072] The calcium carbonate enhancer is prepared by mixing sodium stearate, palmitic acid and lignin in a mass ratio of 7:3:1.
[0073] The retention aid is prepared by mixing polyvinyl alcohol and methyl cellulose in a mass ratio of 1:1.
[0074] The filter aid is polyethyleneimine (PEI).
[0075] The bentonite is prepared by mixing modified bentonite, talcum powder and kaolin in a mass ratio of 3:1:0.2; the modified bentonite used is AlCl3 modified bentonite.
[0076] The bactericide is isothiazolinone.
[0077] The defoaming agent is white carbon black.
[0078] Step 3: Papermaking The pulp before papermaking was papered, and the pulp-to-wire speed ratio was controlled to be 1.012, the retention rate was 72%, the white water concentration was 0.24%, and the wire vacuum degree was -25 KPa to obtain wet paper.
[0079] Step 4: Pressing The wet paper is pressed to remove moisture through mechanical pressure to make the paper sheets tight and improve the paper surface; the felt tension during the pressing process is 26KN / M, the line pressure is 50KN / M, and the vacuum degree of the pressing roller is -35KPa.
[0080] Step 5: Drying The pressed paper is dried at a temperature of 100°C, and the moisture content of the dried paper is 7.0%.
[0081] Step 6: Gluing The dried paper sheets are sizing on the sizing roller, and the sizing amount is 2.1 kg / ton of paper. The surface glue used is a mixture of modified starch solution, carboxymethyl cellulose solution and polyvinyl alcohol in a mass ratio of 4:1:0.05.
[0082] The modified starch solution has a starch solid content of 11% (mass percentage); the preparation method is as follows: the starch is prepared into a solution with a mass percentage concentration of 6%, and gelatinized at a gelatinization temperature of 95° C. for 20 minutes.
[0083] The concentration of the carboxymethyl cellulose solution is 0.2%.
[0084] Step 7: Post-drying The sizing paper sheets were introduced into a dryer for post-drying at a drying temperature of 100°C and a moisture content of 5.5% after drying.
[0085] Step 8: Calendering The paper sheets were introduced into the calender for two calenderings. The calender pressure of the first calendering was 35 KN, and the calender pressure of the second calendering was 50 KN.
[0086] The calendered paper sheets are curled and cut to obtain the finished product.
[0087] The performance of the offset printing paper prepared in Examples 1-3 was tested, and the test results are shown in Table 1: Table 1
[0088] The polyaluminium chloride (PAC) used in the present invention has a basicity of 40-85%, an insoluble matter content of ≤0.6% and a pH value of 3.5-5.0.
[0089] Unless otherwise specified, the ratios described in the present invention are all mass ratios, and the percentages described are all mass percentages.
[0090] Obviously, under the concept of the present invention, there are many specific implementation methods that can be changed. Here, it should be stated that any changes made under the inventive concept of the present invention will fall within the protection scope of the present invention.
Claims
1. A method for preparing offset printing paper, characterized in that: The invention comprises the steps of pulping, pulping, papermaking, pressing, drying, sizing, post-drying and calendering; the pulping adopts raw materials including coniferous wood chemical pulp, hardwood wood chemical pulp and bamboo fiber chemical mechanical pulp; the pulping adopts auxiliary materials including calcium carbonate, calcium carbonate enhancer, polyaluminium chloride, retention aid, filter aid, bentonite, cationic starch, alkenyl succinic anhydride, dye yellow, bactericide and defoamer.
2. The method for preparing offset printing paper according to claim 1, characterized in that: The beating degree of the softwood chemical pulp obtained by refining is 33-35 o SR, hardwood chemical pulp beating degree 32-36 o SR, bamboo fiber chemical mechanical pulp beating degree 42-45 o SR.
3. The method for preparing offset printing paper according to claim 1, characterized in that: The pulping: the pulp obtained after pulping is mixed according to the following weight ratio: 15-35 parts of coniferous wood chemical pulp, 30-50 parts of hardwood chemical pulp, and 30-50 parts of bamboo fiber chemical mechanical pulp.
4. The method for preparing offset printing paper according to claim 1, characterized in that: The retention aid is one or more of polyvinyl alcohol, methyl cellulose, and hydroxyethyl cellulose; the filter aid is any one of polyethyleneimine, polyacrylamide, and polyamine.
5. The method for preparing offset printing paper according to claim 1, characterized in that: The bactericide is one or more of complex bromine, isothiazolinone, thiocyanate, dithiocyanomethane, 2,2-dibromo-3-cyano-acetamide and halogenated hydantoin; the defoamer is one or more of polysiloxane, modified polysiloxane, silicone resin, white carbon black, dispersant and stabilizer.
6. The method for preparing offset printing paper according to claim 1, characterized in that: The polyaluminium chloride has a basicity of 40-85%, an insoluble matter content of ≤0.6% and a pH value of 3.5-5.
0.
7. The method for preparing offset printing paper according to claim 1, characterized in that: The calcium carbonate enhancer is prepared by mixing sodium stearate, palmitic acid and lignin in a mass ratio of 7:3:1; the bentonite is prepared by mixing modified bentonite, talcum powder and kaolin in a mass ratio of 3:1:0.2; the modified bentonite used is AlCl3 modified bentonite.
8. The method for preparing offset printing paper according to claim 1, characterized in that: The papermaking method controls the pulp-to-wire speed ratio to be 1.012, the retention rate to be 68-78%, the white water concentration to be 0.2-0.3%, and the vacuum degree of the wire part to be -20 to -30 KPa.
9. The method for preparing offset printing paper according to claim 1, characterized in that: The pressing: the line pressure is 40-60KN / M, and the vacuum degree of the pressing roller is -30 to -40KPa.
10. The method for preparing offset printing paper according to claim 1, characterized in that: The sizing method comprises the following steps: the sizing amount is 1.8-2.5 kg / ton of paper; the surface glue used is one or more of modified starch solution, polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC) and polyacrylamide (PAM).
Citation Information
Patent Citations
Paper preparation method using modified calcium carbonate as filler
CN107524032A
Production method of lightweight paper
CN109680536A
Raw white two-side offset paper and preparation method thereof
CN116122073A
Two-side offset paper and preparation method thereof
CN116145465A
Elegant paper and preparation method thereof
CN117265912A