Composite pipeline resistant to high temperature and high pressure and forming process

Through double-layer structure design and multi-angle wire laying technology, combined with low-temperature assembly, the problem of degradation of heat dissipation and mechanical properties of composite pipes under high temperature and high pressure is solved, and the excellent performance and weight reduction in high temperature and high pressure conditions is achieved. It is suitable for more Wide application of high temperature and high pressure conditions.

CN118980000APending Publication Date: 2024-11-19ZHEJIANG UNIV +1

Patent Information

Application Number
CN202410958559.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The heat dissipation and mechanical properties of existing composite pipes under high temperature and high pressure conditions have decreased, which affects service life and production safety. The weight loss process is complex and is not suitable for high temperature and high pressure applications. The weight of steel pipes limits its further development.

Method used

The composite pipeline design adopts a double-layer structure, the steel lining layer and the carbon fiber reinforced epoxy resin material cover layer are designed through multi-angle wire laying and heat dissipation groove design, combined with low-temperature assembly technology, to improve the axial stiffness and heat dissipation ability of the pipeline and reduce weight .

Benefits of technology

On the premise of ensuring high-temperature and high-pressure performance, significantly reduce the weight of the pipeline, improve axial stiffness and heat dissipation capabilities, extend service life, and reduce production costs. It is suitable for a wider application of high-temperature and high-pressure working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980000A_ABST
    Figure CN118980000A_ABST
Patent Text Reader

Abstract

The invention discloses a composite pipeline resistant to high temperature and high pressure. The composite pipeline is sequentially provided with a steel lining layer and a composite outer cover layer from inside to outside. A heat dissipation groove with openings in the two ends is formed in the contact surface of the steel lining layer and the composite material outer cover layer in the axis direction, and the heat dissipation groove is used for introducing cooling liquid for absorbing heat in the composite pipeline; the composite material outer cover layer is prepared in a multi-angle fiber placement mode. The invention further provides a forming process. The composite pipeline provided by the invention gives full play to the advantage of light weight of a composite material, and the overall weight of the pipeline is effectively reduced on the premise of ensuring high-temperature and high-pressure resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite pipes, and in particular relates to a composite pipe resistant to high temperature and high pressure and a molding process. Background Art

[0002] Composite pipes are special pipes that are assembled from multiple layers of different materials such as metal, plastic, ceramic, and composite materials. Due to the combination of the advantages of various materials, they usually exhibit excellent properties such as high strength, heat resistance, corrosion resistance, and light weight. They are currently widely used in fire protection, chemical industry, oil and gas transportation and other fields.

[0003] The laying of pipelines often requires crossing long distances, and reducing the weight of the pipelines themselves will greatly reduce the cost of pipeline transportation and the difficulty of laying operations. However, reducing the weight of pipelines is often accompanied by a decrease in service performance, especially in the face of high temperature and high pressure conditions. The decline in the heat dissipation and mechanical properties of the pipeline will greatly affect its service life, which is actually related to production safety and production costs.

[0004] Patent document CN117901462A discloses a method for manufacturing a fully composite pressure-bearing device, including the steps of preparing an ultra-thin gas-barrier film whose surface is uniformly covered with nanosheets; performing a filament spreading treatment on carbon fiber, laminating, hot pressing and cooling the carbon fiber and the gas-barrier film after the filament spreading to form a carbon fiber-gas-barrier film material, and coating the remaining part with resin to form a prepreg material; performing a layup design on the pressure-bearing device to obtain the number of layup layers and the layup angle; performing carbon fiber layup on the pressure-bearing device, the pressure-bearing device has a gradient structure after layup, the inner side of the device is a carbon fiber-gas-barrier film material layup to form an gas-barrier functional area, and the outer side is a pure carbon fiber layup to form a pressure-bearing functional area; adding a head for the pressure-bearing device, and adding an inner head and an inner rubber gasket to the inner surface of the carbon fiber composite material of the head part of the pressure-bearing device in turn, and adding an outer rubber gasket and an outer head to the outer surface in turn, and connecting them by bolts; performing integrated vacuum curing on the pressure-bearing device.

[0005] Patent document CN117267482A discloses a molding process for a fiber-reinforced large-diameter composite pipe, which includes the following steps: S1, preheating a metal mold, extruding a PE thin strip onto the metal mold through an extruder, and forming a PE liner after cooling; S2, winding an inner link rib on the outer surface of the liner at an 89° winding angle, and blowing hot air at the same time, hot-melt welding the inner link rib on the outer surface of the liner; S3, winding a glass fiber yarn impregnated with thermosetting resin on the outer surface of the liner at an 89° winding angle, with a thickness of 3 mm, and then continuing to use a 55.45° winding angle. S4, then wind the external link ribs at an 89° winding angle on the glass fiber reinforcement layer, and then continue to wind the glass fiber yarn impregnated with thermosetting resin at an 89° winding angle on the reinforcement layers spaced on both sides of the external link ribs, with a thickness of 2mm; S5, after the glass fiber reinforcement layer is solidified, the PE thin tape is wrapped around the outside of the pipe through an extruder, and the molten PE tape is welded to the external link ribs through an extrusion roller to form a PE protective layer; S6, wind an "O"-shaped PP reinforced rib tube around the outside of the PE protective layer, and hot-melt weld it to the PE protective layer.

[0006] The above process is complicated and is not suitable for pipelines used in high temperature and high pressure conditions. Currently, the pipelines used in high temperature and high pressure conditions are mainly steel pipes, but their large weight limits their further development in high temperature and high pressure pipeline applications. Summary of the invention

[0007] The purpose of the present invention is to provide a high temperature and high pressure resistant composite pipe and a molding process. The composite pipe fully utilizes the advantages of lightweight composite materials, effectively reduces the overall weight of the pipe while ensuring high temperature and high pressure resistance, so that it has broader application prospects in high temperature and high pressure working conditions such as gas and oil transmission.

[0008] In order to achieve the first object of the present invention, the following technical solution is provided: a composite pipe resistant to high temperature and high pressure, wherein the pipe wall of the composite pipe is provided with a steel lining layer and a composite material outer cover layer in sequence from the inside to the outside;

[0009] The contact surface between the steel lining layer and the composite material outer cover layer is provided with a heat dissipation groove with two ends opened along the axial direction, and the heat dissipation groove is used to pass a coolant that absorbs the heat of the liquid in the composite pipe;

[0010] The composite material outer cover layer is prepared by a multi-angle wire laying method.

[0011] The present invention adopts a composite material with high strength and low specific gravity as the outer layer, and arranges an inner lining to absorb the heat in the pipeline, thereby avoiding the problems of high cost and high temperature softening of thermoplastic composite materials.

[0012] Specifically, the composite material outer cover layer is obtained by laying out carbon fiber reinforced epoxy resin material, which breaks through the problem of limited winding angle in traditional methods, and effectively reduces the stress concentration of the composite material outer cover by adjusting the arrangement order of the laying angles, thereby greatly improving the axial stiffness of the composite material pipe.

[0013] Specifically, the multiple angles include ply angles of -45°, 0°, 45° and 90°.

[0014] Specifically, there are a plurality of heat dissipation grooves, and the plurality of heat dissipation grooves are arranged at intervals on the outer peripheral surface of the steel lining layer along the circumference of the steel lining layer.

[0015] Specifically, the heat dissipation groove is an arc groove.

[0016] Specifically, the ratio of the depth of the heat dissipation groove to the thickness of the steel lining layer is in the range of 1:2-3.

[0017] In order to achieve the second object of the present invention, the following technical solution is provided: a molding process for preparing the above-mentioned high temperature and high pressure resistant composite pipe comprises the following steps:

[0018] Preheating the forming mold and laying the composite material in the forming mold in a specific arrangement order, and demoulding after multiple hot pre-pressing processes and multiple curing processes to obtain the corresponding composite material outer cover layer;

[0019] Obtain a prefabricated pipe body, and process the outer peripheral surface of the pipe body according to the preset heat dissipation groove depth to obtain a steel lining layer with multiple heat dissipation grooves;

[0020] The composite outer cover layer and steel inner lining layer obtained by processing are placed in an ultra-low temperature environment of liquid nitrogen, the shrunk steel inner lining layer is placed in the composite outer cover layer, and then the ambient temperature is restored to room temperature to complete the self-tightening of the composite pipe.

[0021] Specifically, the specific arrangement order is:

[0022] The arrangement order of the ply angles is [45°, 0°, -45°, 90°, 0°, 0°, 90°, -45°, 0°, 45°].

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention adopts a double-layer structure design. The carbon fiber reinforced epoxy resin material used in the outer cover is a thermosetting material, which avoids the high-temperature softening and high-cost problems of thermoplastic materials. The outer cover is prepared by wire laying technology to reduce stress concentration while ensuring the precise size of the outer cover structure, thereby improving the axial stiffness. Multiple hot pre-pressing processes and multiple curing processes suppress and eliminate the superposition and amplification effects of defects in the manufacturing process of the thick carbon fiber outer cover structure. At the same time, the steel lining is designed with a heat dissipation structure while ensuring the structural strength, and the heat dissipation capacity is improved by means of coolant, thereby alleviating the problem of poor high-temperature resistance of thermosetting composite materials.

[0025] In addition, by utilizing the different physical properties of the two layers of materials, low-temperature assembly is used to improve the assembly accuracy between the two layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic cross-sectional view of the composite pipeline provided in this embodiment;

[0027] Figure 2 A schematic diagram of the structure of the composite material outer cover provided in this embodiment;

[0028] Figure 3 A schematic diagram of the structure of the steel liner provided in this embodiment;

[0029] Figure 4 A comparison diagram of stress distribution of composite material outer cover layers with different interference fits under high temperature and high pressure conditions provided in this embodiment;

[0030] Figure 5 A comparison diagram of stress distribution of steel lining layers with different interference fits under high temperature and high pressure conditions provided in this embodiment;

[0031] In the figure, 1. Composite material outer cover; 2. Steel lining. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0033] like Figure 1As shown, a high temperature and high pressure resistant composite pipe is provided in this embodiment. The pipe wall of the composite pipe is composed of two parts, including a steel lining 2 and a composite material outer cover 1.

[0034] like Figure 2 As shown, the composite outer cover 1 is made of carbon fiber reinforced epoxy resin material. The carbon fiber reinforced epoxy resin material has the characteristics of small specific gravity, high strength and modulus, good dimensional stability, etc. It is suitable for developing various components with high load-bearing capacity. As a thermosetting material, it avoids the high cost and high temperature softening problems of thermoplastic composite materials.

[0035] The composite material cover 1 selected in this embodiment has a structural dimension of 3000mm in length, 210mm in outer diameter, 140mm in inner diameter, and 35mm in wall thickness. It is prepared by an automatic wire laying process, which breaks through the problem of limited winding angles and adopts the arrangement sequence of [45°, 0°, -45°, 90°, 0°, 0°, 90°, -45°, 0°, 45°] layer angles, effectively reducing the stress concentration of the composite material cover 1 and greatly improving the axial stiffness of the composite material cover 1. Multiple hot pre-pressing processes and multiple curing processes suppress and eliminate the superposition and amplification effects of defects in the manufacturing process of the composite material cover 1, thereby ensuring stable and controllable molding quality and realizing precise manufacturing of the composite material cover 1.

[0036] like Figure 3 As shown, the steel lining 2 is made of high-strength steel, has high strength, plasticity and wear resistance under high temperature and high pressure conditions, and is suitable for the manufacture of pipe inner linings.

[0037] The structural dimensions of the steel liner 2 in this embodiment are 3000 mm long, 140 mm outer diameter, 120 mm inner diameter, and 10 mm thick. On the premise of meeting the structural strength requirements of the composite pipeline, in order to enhance the heat dissipation performance of the pipeline, the stability of the thermosetting composite material cover 1 is ensured.

[0038] At the same time, a heat dissipation structure is designed on the steel lining 2, that is, straight arc grooves are cut along the axis on the outer periphery of the steel lining 2, totaling 10 to 25, and the radius of the arc groove is R. In this embodiment, the radius of the arc groove is selected in the range of 1mm≤R≤5mm, and coolant is passed into the heat dissipation structure to reduce the temperature of the contact interface between the steel lining and the composite material outer cover, thereby ensuring the working stability of the composite material outer cover.

[0039] In this embodiment, a simulation analysis of the heat dissipation structure is also performed on the above-mentioned steel liner 2. At the same time, the composite material cover 1 is taken as an insulating material with no thermal expansion. When conveying a high-temperature material at 300°C, it is calculated that the temperature of the contact interface between the steel liner 2 without an active heat dissipation structure and the composite material cover 1 is 300°C in a steady state. At this temperature, the composite material will fail, and its mechanical properties will be greatly reduced, and it will be unable to continue to withstand high-pressure conditions. Under the same conditions, the internal temperature distribution of the composite channel with an active heat dissipation structure presents a good gradient distribution from the inside to the outside, and the interface temperature in contact with the composite material cover 1 is about 100°C, which is much lower than the failure temperature of the composite material cover 1. It can be seen that the heat dissipation structure can effectively alleviate the problem of the composite material cover 1 being sensitive to high temperatures by quickly dissipating the heat of the steel liner, thereby ensuring its working performance in a high-temperature environment.

[0040] The composite material outer cover 1 mentioned in this embodiment can be made of carbon fiber reinforced epoxy resin material, and is also suitable for other thermosetting resins and thermoplastic resins.

[0041] The steel lining 2 can be steel lining or ceramic lining.

[0042] In order to improve the assembly accuracy of the composite pipe, this embodiment provides a molding process for preparing the composite pipe provided in the above embodiment, which is specifically as follows:

[0043] Preheating the forming mold and laying the composite material in the forming mold in a specific arrangement order, and demoulding after multiple hot pre-pressing processes and multiple curing processes to obtain the corresponding composite material outer cover layer;

[0044] Obtain a prefabricated pipe body, and process the outer peripheral surface of the pipe body according to the preset heat dissipation groove depth to obtain a steel lining layer with multiple heat dissipation grooves;

[0045] The composite outer cover layer and steel inner lining layer obtained by processing are placed in an ultra-low temperature environment of liquid nitrogen, the shrunk steel inner lining layer is placed in the composite outer cover layer, and then the ambient temperature is restored to room temperature to complete the self-tightening of the composite pipe.

[0046] According to the cold brittleness of metal in ultra-low temperature environment, this embodiment determines to use liquid nitrogen to form an ultra-low temperature assembly environment of -120℃~-200℃ to ensure that its mechanical properties are not affected. The composite outer cover 1 and the steel liner 2 are placed in this environment. Due to the different thermal expansion coefficients of steel and carbon fiber reinforced epoxy resin materials, the steel liner 2 is much smaller in size due to low temperature than the composite outer cover 1. The two are assembled, and the interference fit is 0.2mm~0.12mm. After assembly, the composite pipe is restored to room temperature, and at this time, the composite outer cover 1 and the steel liner 2 are self-tightened.

[0047] like Figure 4 and Figure 5 As shown in the figure, the above molding process not only effectively avoids the gap problem caused by the thermosetting composite material outer cover wrapping the steel liner and curing process, but also realizes the self-tightening of the composite pipe. At the same time, due to the interference fit between the outer cover and the liner, the composite material outer cover 1 generates an inward pressure on the steel liner 2. Although the stress of the composite material outer cover 1 will be slightly increased, the tensile stress of the steel liner can be reduced, which is equivalent to sharing the load of the liner through the outer cover, alleviating the stress of the steel liner 2, improving the internal pressure resistance of the pipeline, and better adapting to the working conditions of high internal pressure. The composite pipelines with and without low-temperature interference assembly are simulated and modeled, and their working performance under high temperature and high pressure is analyzed. The internal temperature of the pipeline is set to 300℃, the pressure is set to 200MPa, the carbon fiber stress verification strength standard is set to 1347MPa, and the steel stress verification standard is set to 842MPa.

[0048] The inner wall stress of the composite cover 1 without low-temperature interference fitting is about 1072MPa, while the inner wall stress of the composite cover 1 with low-temperature interference fitting is about 1183MPa. At the same time, the stress at other positions increases slightly due to interference fitting. Since the stress on the composite cover 1 decreases from the inside to the outside, the stress on the inner wall is the largest, and the inner wall stress of the composite cover 1 with low-temperature interference fitting is lower than the strength verification standard. Therefore, although the stress has increased, the design still meets the strength requirements. The maximum stress of the steel lining is also at the inner wall. The inner wall stress of the steel lining 2 without low-temperature interference fitting is 865MPa, which does not meet the strength verification standard and is prone to safety hazards. The inner wall stress of the steel lining 2 with low-temperature interference fitting is 793MPa, which meets the strength verification standard. That is, through the stress sharing of the composite cover 1, the stress of the steel lining 2 is effectively reduced, ensuring the safety performance of the pipeline under high temperature and high pressure conditions.

[0049] In summary, the composite pipe made and assembled by the above specific implementation method ensures that it still has excellent performance under high temperature and high pressure conditions. At the same time, due to the use of composite materials, the total weight is greatly reduced compared with the full steel pipe of the same size. Under the above dimensions, the weight of the composite outer cover 1 is about 92kg, the weight of the steel lining 2 is about 88kg, and the total weight is about 180kg, while the total weight of the full steel pipe of the same size is about 550kg, and the overall weight is reduced by about 67%, which provides a lighter advantage for the transportation and laying of the pipeline in practical applications.

[0050] In addition, the terms "upper", "lower", "inner", "outer", "front", "rear" are used for descriptive purposes only and should not be understood as indicating or implying relative importance. Unless otherwise specifically stated, the relative steps, numerical expressions and values ​​of the components and steps described in these embodiments do not limit the scope of the present invention.

[0051] Of course, the above description is only a specific embodiment of the present invention and is not intended to limit the scope of implementation of the present invention. All equivalent changes or modifications made according to the structure, characteristics and principles described in the patent application scope of the present invention should be included in the patent application scope of the present invention.

[0052] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A composite pipe resistant to high temperature and high pressure, characterized in that: The pipe wall of the composite pipe is provided with a steel inner lining layer and a composite material outer covering layer in sequence from the inside to the outside; The contact surface between the steel lining layer and the composite material outer cover layer is provided with a heat dissipation groove with two ends opened along the axial direction, and the heat dissipation groove is used to pass a coolant that absorbs heat in the composite pipe; The composite material outer cover layer is prepared by a multi-angle wire laying method.

2. The high temperature and high pressure resistant composite pipe according to claim 1, characterized in that: The composite material outer cover layer is obtained by laying out carbon fiber reinforced epoxy resin material.

3. The high temperature and high pressure resistant composite pipe according to claim 1, characterized in that: The multiple angles include ply angles of -45°, 0°, 45° and 90°.

4. The high temperature and high pressure resistant composite pipe according to claim 1, characterized in that: There are a plurality of heat dissipation grooves, which are arranged at intervals on the outer peripheral surface of the steel lining layer along the circumference of the steel lining layer.

5. The high temperature and high pressure resistant composite pipe according to claim 1 or 4, characterized in that: The heat dissipation groove is a circular arc groove.

6. The high temperature and high pressure resistant composite pipe according to claim 1 or 4, characterized in that: The ratio of the depth of the heat dissipation groove to the thickness of the steel lining layer is in the range of 1:2 to 3.

7. A molding process, characterized in that: The method for preparing the high temperature and high pressure resistant composite pipe according to any one of claims 1 to 7 comprises the following steps: Preheating the forming mold and laying the composite material in the forming mold in a specific arrangement order, and demoulding after multiple hot pre-pressing processes and multiple curing processes to obtain the corresponding composite material outer cover layer; Obtain a prefabricated pipe body, and process the outer peripheral surface of the pipe body according to the preset heat dissipation groove depth to obtain a steel lining layer with multiple heat dissipation grooves; The composite outer cover layer and steel inner lining layer obtained by processing are placed in an ultra-low temperature environment of liquid nitrogen, the shrunk steel inner lining layer is placed in the composite outer cover layer, and then the ambient temperature is restored to room temperature to complete the self-tightening of the composite pipe.

8. The molding process according to claim 7, characterized in that: The specific arrangement order is specifically: The arrangement order of the ply angles is [45°, 0°, -45°, 90°, 0°, 0°, 90°, -45°, 0°, 45°].

Citation Information

Patent Citations

  • High-pressure fuel pipe for hydraulic system with self cooling device

    CN101629667A

  • Carbon fiber composite barrel containing metal liner and cold assembly manufacturing method of carbon fiber composite barrel

    CN106705748A

  • Composite material rotation structure and forming method thereof

    CN107696523A

  • Preparation and application of two-dimensional multi-directional cloth for flanged containment case

    CN108466437A

  • Low-temperature-resistant high-heat-dissipation aluminum pipe

    CN213452401U

Cited By

  • Compound gear, speed reduction transmission assembly and aircraft

    CN119308987A

  • Compound gear, speed reduction transmission assembly and aircraft

    CN119308988A