Method for characterizing crystal quality of 3C-SiC epitaxial layer and method for characterizing crystal quality of 3C-SiC substrate

By using (112) and (113) crystal surfaces in 3C-SiC materials for X-ray diffraction testing, the accuracy problem of crystallization quality characterization of 3C-SiC epitaxial layer and substrate in the prior art is solved, and high accuracy is achieved Non-destructive testing is suitable for growth process optimization.

CN118980700AActive Publication Date: 2024-11-19SICC SHANGHAI CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411193275.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-19
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The prior art is difficult to accurately characterize the crystal quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate, especially due to the similarity to 4H-SiC, the X-ray diffractometer test results are inaccurate, and conventional polishing processes are prone to substrate cracking. .

Method used

X-rays were used to diffraction test the (112) and (113) crystal planes of the 3C-SiC epitaxial layer and the 3C-SiC substrate, and quantitatively characterized by the half-height width difference between the two crystal planes, avoiding the 4H-SiC The interference and reduces substrate damage during polishing.

Benefits of technology

Accurate quantitative characterization of the crystalline quality of 3C-SiC epitaxial layer and 3C-SiC substrate is achieved, which improves the accuracy and reliability of the test, avoids substrate damage, and is suitable for optimization of growth processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980700A_ABST
    Figure CN118980700A_ABST
Patent Text Reader

Abstract

The invention discloses a method for characterizing the crystal quality of a 3C-SiC epitaxial layer and a method for characterizing the crystal quality of a 3C-SiC substrate, and belongs to the technical field of quality characterization of 3C-SiC materials. The method comprises the following steps: (1) placing a polished 3C-SiC epitaxial layer or a polished 3C-SiC substrate on a sample table of an X-ray diffractometer; and (2) performing diffraction test on a (112) crystal face and a (113) crystal face of the 3C-SiC epitaxial layer or the 3C-SiC substrate by adopting X rays to respectively obtain full width at half maximum, and when a difference value between the full width at half maximum of the (113) crystal face and the full width at half maximum of the (112) crystal face is not greater than 40 arcsec, the full width at half maximum of the (112) crystal face and the full width at half maximum of the (113) crystal face are crystal quality parameters of the 3C-SiC epitaxial layer or the 3C-SiC substrate. The method can realize quantitative characterization of the crystal quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate, and can play a guiding role in optimization of the growth process of the 3C-SiC material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a method for characterizing the crystallization quality of a 3C-SiC epitaxial layer and a method for characterizing the crystallization quality of a 3C-SiC substrate, and belongs to the technical field of 3C-SiC material quality characterization. Background Art

[0002] Silicon carbide materials have excellent electrical and optical properties, so they have become increasingly commercialized in recent years. At the same time, silicon carbide has more than 200 crystal forms, which have different symmetries and atomic spacing, so there are also differences in physical properties.

[0003] At present, the most researched are 4H and 6H crystal forms of silicon carbide, both of which are hexagonal crystal systems. Silicon carbide has only one cubic structure, which is the 3C crystal form. Compared with hexagonal silicon carbide, 3C-SiC has higher carrier mobility and saturation velocity. At the same time, this crystal form can exist stably at around 1500°C, has a lower growth temperature, and is easier to prepare in large quantities. Therefore, it may have a wide range of applications in the new generation of devices.

[0004] At present, the growth of 3C-SiC is mainly carried out by heteroepitaxial growth using 4H-SiC as a substrate to obtain a 3C-SiC epitaxial layer. There are some potential problems with the heteroepitaxial growth method, such as the occurrence of double-positioned boundary defects, or the thickness of the growth is generally difficult to exceed 50μm. The above problems will make it difficult to characterize its crystal quality and symmetry using conventional methods.

[0005] According to the principle of minimum lattice mismatch, the surface of the 3C-SiC epitaxial layer grown by heteroepitaxial growth is the (111) plane. The conventional method of characterizing crystallization is to test the rocking curve with an X-ray diffractometer, that is, the half-peak width of the diffraction peak at a specific diffraction angle. However, the incident angle of the (111) plane of 3C-SiC under the X-ray diffractometer is 17.8°, and the incident angle of the (004) plane of 4H-SiC is also about 17.8°. The penetration depth at this diffraction angle is about 30μm, less than 50μm, so it is impossible to distinguish between the epitaxial layers 3C-SiC and 4H-SiC during the test, and it is impossible to characterize the crystallization quality of the 3C-SiC epitaxial layer.

[0006] Similarly, the 3C-SiC substrate also has a (111) crystal plane. Since 3C-SiC has poorer rigidity than 4H-SiC, multiple polishing tests are required to obtain more accurate crystal quality, but this can easily cause the substrate to crack.

[0007] And because the stacking units of 4H-SiC and 3C-SiC are similar, it is difficult to characterize whether the crystal form of the 3C-SiC epitaxial layer is single by conventional XRD characterization methods. Therefore, how to characterize the 3C-SiC epitaxial layer and 3C-SiC substrate has guiding significance for the subsequent optimization of the growth process. Summary of the invention

[0008] In order to solve the above problems, a method for characterizing the crystallization quality of a 3C-SiC epitaxial layer and a method for characterizing the crystallization quality of a 3C-SiC substrate are provided. The method uses X-rays to perform diffraction tests on the (112) crystal plane and the (113) crystal plane of the 3C-SiC epitaxial layer or the 3C-SiC substrate, and uses the half-widths obtained from the two crystal planes to compare and verify the accuracy of the test method. The method can achieve quantitative characterization of the crystallization quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate, and can play a guiding role in optimizing the growth process of the 3C-SiC material.

[0009] According to one aspect of the present application, a method for characterizing the crystalline quality of a 3C-SiC epitaxial layer is provided, comprising the following steps:

[0010] (1) Placing the polished 3C-SiC epitaxial layer on the sample stage of an X-ray diffractometer;

[0011] (2) X-ray diffraction test is performed on the (112) crystal plane and the (113) crystal plane of the 3C-SiC epitaxial layer to obtain the half-widths respectively. When the difference between the half-widths of the (113) crystal plane and the half-widths of the (112) crystal plane is no more than 40 arcsec, the half-widths of the (112) crystal plane and the half-widths of the (113) crystal plane are the crystallization quality parameters of the 3C-SiC epitaxial layer.

[0012] Based on the characteristics of different crystal planes of 3C-SiC, at the same test position of the same 3C-SiC epitaxial layer, the half-width value obtained by the (113) crystal plane is greater than the half-width value obtained by the (112) crystal plane. Therefore, when the difference between the half-width values ​​of the above two crystal planes is no more than 40 arcsec, it means that the characterization method is correct. The difference refers to the half-width value of the (113) crystal plane minus the half-width value of the (112) crystal plane.

[0013] When using the (111) crystal plane to characterize the crystal quality of the 3C-SiC epitaxial layer, firstly, it is easy to introduce the signal of the 4H-SiC substrate, thus causing inaccurate test results; secondly, the surface state of the 3C-SiC epitaxial layer after polishing will affect the test results. It is necessary to polish and correct the 3C-SiC epitaxial layer multiple times to obtain better results. However, after multiple polishing, the thickness of the 3C-SiC epitaxial layer will not meet the requirements.

[0014] Therefore, the present application uses the (112) crystal plane and the (113) crystal plane to characterize the crystal quality of the 3C-SiC epitaxial layer to solve the above problems, and the crystal quality data obtained by the (112) crystal plane and the (113) crystal plane test are the crystal quality data inside the 3C-SiC epitaxial layer, which can better reflect the crystal quality of the entire crystal compared to the test data of the (111) crystal plane. The smaller the difference between the half-height width of the (113) crystal plane and the half-height width of the (112) crystal plane, the better the crystal quality of the 3C-SiC epitaxial layer.

[0015] Optionally, the polishing in step (1) uses zirconium oxide as an abrasive for polishing. Since the Mohs hardness of zirconium oxide is about 8.5, which is close to that of 3C-SiC, and zirconium oxide is more wear-resistant, it can be reused, thereby reducing costs.

[0016] Optionally, in step (2), the incident angle of the X-ray diffraction test on the (112) crystal plane of the 3C-SiC epitaxial layer is 10.6°±0.5°, and the exit angle is 30.07°±0.5°.

[0017] Optionally, in step (2), the incident angle of the X-ray diffraction test on the (113) crystal plane of the 3C-SiC epitaxial layer is 6.36°±0.5°, and the exit angle is 35.87°±0.5°.

[0018] The incident angles of the above two crystal planes are small, and the test depth is also shallow, about 8μm, which is suitable for characterizing the epitaxial layer, but will not test the signal of the substrate 4H-SiC. The penetration depth of the incident angle of the (112) crystal plane is deeper than that of the (113) crystal plane, but its penetration depth will not exceed 10μm, so it is still suitable for characterizing the crystal quality of the 3C-SiC epitaxial layer.

[0019] Optionally, the surface Warp value of the polished 3C-SiC epitaxial layer is less than 20 μm.

[0020] Optionally, in step (2), the scanning range of the (112) and (113) surfaces is no greater than 2000 arcsec. The diffraction test is performed within 2000 arcsec, and the test data obtained has no impurity peaks except the main peak, indicating that the 3C-SiC epitaxial layer has a single crystal form.

[0021] Optionally, the diameter of the 3C-SiC epitaxial layer is greater than 6 inches, preferably greater than 8 inches.

[0022] Optionally, in step (2), at least 5 points of testing are performed on both the (112) crystal plane and the (113) crystal plane.

[0023] According to another aspect of the present application, a method for characterizing the crystalline quality of a 3C-SiC substrate is provided, comprising the following steps:

[0024] (1) Placing the polished 3C-SiC substrate on the sample stage of an X-ray diffractometer;

[0025] (2) X-ray diffraction tests are performed on the (112) crystal plane and the (113) crystal plane of the 3C-SiC substrate to obtain the half-widths respectively. When the difference between the half-widths of the (113) crystal plane and the half-widths of the (112) crystal plane is no more than 40 arcsec, the half-widths of the (112) crystal plane and the half-widths of the (113) crystal plane are the crystal quality parameters of the 3C-SiC substrate.

[0026] For 3C-SiC substrates, although there are no interference factors of 4H-SiC substrates, when the (111) crystal plane is used for crystal quality characterization, the test data will be affected by surface fluctuations, which requires repeated polishing corrections to overcome. However, after multiple polishing, the thickness of the 3C-SiC substrate will not meet the requirements, and multiple polishing is very likely to cause crystal cracking. Therefore, the (112) crystal plane and the (113) crystal plane are characterized to solve this problem, and the crystal quality data obtained by the (112) crystal plane and the (113) crystal plane test are the crystal quality data inside the 3C-SiC substrate, which can better reflect the overall crystal quality of the crystal than the test data of the (111) crystal plane. The smaller the difference between the half-height width of the (113) crystal plane and the half-height width of the (112) crystal plane, the better the crystal quality of the 3C-SiC substrate.

[0027] Optionally, the polishing in step (1) uses zirconium oxide as an abrasive for polishing. Since the Mohs hardness of zirconium oxide is about 8.5, which is close to that of 3C-SiC, and zirconium oxide is more wear-resistant, it can be reused, thereby reducing costs.

[0028] Optionally, in step (2), the incident angle of the X-ray diffraction test on the (112) crystal plane of the 3C-SiC substrate is 10.6°±0.5°, and the exit angle is 30.07°±0.5°.

[0029] Optionally, in step (2), the incident angle of the X-ray diffraction test on the (113) crystal plane of the 3C-SiC substrate is 6.36°±0.5°, and the exit angle is 35.87°±0.5°.

[0030] Optionally, the surface warpage of the polished 3C-SiC substrate is less than 20 μm.

[0031] Optionally, in step (2), the scanning range of the (112) and (113) surfaces is no greater than 2000 arcsec. The diffraction test is performed within 2000 arcsec, and the test data obtained has no impurity peaks except the main peak, indicating that the 3C-SiC substrate has a single crystal form.

[0032] Optionally, the diameter of the 3C-SiC substrate is greater than 6 inches, preferably greater than 8 inches.

[0033] Optionally, in step (2), at least 5 points of testing are performed on both the (112) crystal plane and the (113) crystal plane.

[0034] The above five test points are at least (-65,0), (65,0), (0,65), (0,-65) and (0,0).

[0035] Preferably, in step (2), at least 9 points of testing are performed on both the (112) crystal plane and the (113) crystal plane.

[0036] The above 9 test points are at least (-85,0), (85,0), (0,85), (0,-85), (-40,0), (40,0), (0,40), (0,-40) and (0,0).

[0037] Optionally, the polishing removal thickness of the 3C-SiC epitaxial layer and the 3C-SiC substrate does not exceed 1 μm. Since the thickness of the 3C-SiC epitaxial layer is usually between 10-50 μm, preferably 30-50 μm, the polishing removal thickness is less than 1 μm, which can ensure the integrity of the 3C-SiC epitaxial layer and reduce losses, and a large amount of removal will cause cracking. Although the thickness of the 3C-SiC substrate is thicker than that of the 3C-SiC epitaxial layer, usually 300-500 μm, when the removal amount is too large, it is very easy to cause cracking of the 3C-SiC substrate, so the polishing removal thickness of the 3C-SiC substrate does not exceed 1 μm. After polishing, the surface warpage of the 3C-SiC epitaxial layer and the 3C-SiC substrate is less than 20 μm, which can further improve the accuracy of the detection results.

[0038] Based on the characteristic

[111] crystal orientation property of 3C-SiC, the present application uses the (112) crystal plane and the (113) crystal plane as the crystal planes for diffraction testing, which can make the

[111] crystal orientation of 3C-SiC projected at the exact center of the (112) crystal plane and the (113) crystal plane, so as to accurately obtain the crystal quality information of 3C-SiC. And because the (112) crystal plane is closer to the cleavage plane, the half-height width value obtained by the (113) crystal plane is higher than that of the (112) crystal plane, and the displayed crystal quality is slightly worse. However, the present application uses the (112) crystal plane for testing and the (113) crystal plane for verification, or uses the (113) crystal plane for testing and the (112) crystal plane for verification, so that the test parameters of the (112) crystal plane and the test parameters of the (113) crystal plane can be mutually verified, thereby proving that the characterization method of the present application is accurate and effective.

[0039] The beneficial effects of this application include but are not limited to:

[0040] 1. The method of characterizing the crystalline quality of the 3C-SiC epitaxial layer of the present application tests the (112) crystal plane and the (113) crystal plane, has a small incident angle, and a shallow penetration depth of the X-rays. The crystalline quality of the 3C-SiC epitaxial layer can be characterized, and the signal of the substrate 4H-SiC will not be tested, and the test accuracy and reliability are high.

[0041] 2. The method of characterizing the crystalline quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate of the present application, while testing the (112) crystal plane and the (113) crystal plane can mutually verify the accuracy of the test method, and the two crystal planes can more comprehensively characterize the crystalline quality of the epitaxial layer or substrate, thereby providing guidance for the subsequent optimization of the growth process.

[0042] 3. The method of characterizing the crystal quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate of the present application can complete the detection without tilting the sample stage of the X-ray diffractometer. Therefore, the sample stability is high during the test process, which can further improve the accuracy of the test results.

[0043] 4. The method of characterizing the crystal quality of the 3C-SiC epitaxial layer and the 3C-SiC substrate of the present application is convenient and fast to test, with a short test time, and will not cause damage to the 3C-SiC epitaxial layer and the 3C-SiC substrate. It belongs to non-destructive testing and is suitable for large-scale promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0045] Figure 1 Schematic diagram of the microscopic model of 3C-SiC.

[0046] Figure 2 A test schematic diagram for determining the emission angle of the (112) crystal plane involved in Example 1 of the present application.

[0047] Figure 3 A test schematic diagram for determining the emission angle of the (113) crystal plane involved in Example 2 of the present application.

[0048] Figure 4 A test schematic diagram for determining the emission angle of the (111) crystal plane involved in Example 3 of the present application. DETAILED DESCRIPTION

[0049] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0050] Unless otherwise specified, the 3C-SiC epitaxial layer or 3C-SiC substrate in the embodiments of the present application is prepared by conventional methods or purchased through commercial channels.

[0051] Unless otherwise specified, the methods used in the embodiments of the present application are conventional methods in the prior art.

[0052] Figure 1 Schematic diagram of the microscopic model of 3C-SiC, wherein the blue line represents the (112) crystal plane, and the pink line represents the (113) crystal plane. In the following embodiments, the above two crystal planes are used to test the crystal quality of silicon carbide.

[0053] Example 1

[0054] This embodiment relates to determining the incident angle and the exit angle when performing a diffraction test on the (112) crystal plane in a 3C-SiC epitaxial layer.

[0055] In this embodiment, the incident angle of the (112) crystal plane is first determined to be 10.6° by calculation, and then the exit angle is changed to determine the angle range of the exit angle when the strongest diffraction peak exists. The results are shown in FIG. Figure 2 , so the emission angle of the (112) crystal plane is determined to be 30.07°±0.5°.

[0056] Based on the same test principle, the emission angle of the (112) crystal plane was first determined to be 30.07°, and then the incident angle was changed to determine the angle range of the incident angle when the strongest diffraction peak existed, and the emission angle of the (112) crystal plane was determined to be 10.6°±0.5°.

[0057] Example 2

[0058] This embodiment relates to determining the incident angle and the exit angle when performing a diffraction test on the (113) crystal plane in a 3C-SiC epitaxial layer.

[0059] In this embodiment, the incident angle of the (113) crystal plane is first determined to be 6.36° by calculation, and then the exit angle is changed to determine the angle range of the exit angle when the strongest diffraction peak exists. The results are shown in FIG. Figure 3 , so the emission angle of the (112) crystal plane is determined to be 35.87°±0.5°.

[0060] Based on the same test principle, the emission angle of the (113) crystal plane was first determined to be 35.87°, and then the incident angle was changed to determine the angle range of the incident angle when the strongest diffraction peak existed, and the emission angle of the (113) crystal plane was determined to be 6.36°±0.5°.

[0061] Example 3

[0062] This embodiment relates to determining the incident angle and the exit angle when performing a diffraction test on the (111) crystal plane in a 3C-SiC epitaxial layer.

[0063] In this embodiment, the incident angle of the (111) crystal plane is first determined to be 17.8° by calculation, and then the exit angle is changed to determine the angle range of the exit angle when the strongest diffraction peak exists. The results are shown in FIG. Figure 4 It can be seen that when the (111) crystal plane is used to test the 3C-SiC epitaxial layer, the range of its emission angle is relatively large, roughly in the large range of 35°-36.5°, and there are two main peaks, proving that the signals of 3C-SiC and 4H-SiC as well as lattice mismatch can be tested.

[0064] Example 4

[0065] This embodiment relates to a method for characterizing the crystal quality of a 6-inch 3C-SiC epitaxial layer, wherein the 3C-SiC epitaxial layer includes both a 4H-SiC substrate and 3C-SiC generated on the surface of the 4H-SiC substrate, and comprises the following steps:

[0066] (1) placing the polished 3C-SiC epitaxial layer on a sample stage of an X-ray diffractometer, wherein the surface Warp value of the polished 3C-SiC epitaxial layer is less than 20 μm;

[0067] (2) X-rays were used to perform 5-point diffraction tests on the (112) and (113) crystal planes of the 3C-SiC epitaxial layer to obtain the half-height widths, where the incident angle for the diffraction test on the (112) crystal plane was 10.6°, and the exit angles were shown in Table 1; the incident angle for the diffraction test on the (113) crystal plane was 6.36°, and the exit angles were shown in Table 1; the scanning ranges of the (112) and (113) planes were no greater than 2000 arcsec. The test results of the half-height widths of the two crystal planes are shown in Table 1.

[0068] In addition, for the same 3C-SiC epitaxial layer, a 5-point diffraction test was performed using the (111) crystal plane as a control test, and the incident angle of the (111) crystal plane diffraction test was 17.8°. The test results of the half-height width of the (111) crystal plane are shown in Table 1.

[0069] Table 1

[0070]

[0071] According to the test results in Table 1, the difference between the half-width of the (113) crystal plane and the half-width of the (112) crystal plane is no more than 40 arcsec, so the half-width of the (112) crystal plane and the half-width of the (113) crystal plane are the crystal quality parameters of the 3C-SiC epitaxial layer. The half-width data of the (111) crystal plane fluctuates greatly, proving that it is easy to introduce the signal of 4H-SiC at the test point, and the difference between the half-width of the (112) crystal plane and the (111) crystal plane is greater than 90 arcsec, and the difference between the half-width of the (113) crystal plane and the (111) crystal plane is greater than 60 arcsec, proving that the use of the (111) crystal plane to test the 3C-SiC epitaxial layer is easy to introduce the test signal of 4H-SiC, thereby failing to accurately characterize the crystal quality of the 3C-SiC epitaxial layer.

[0072] Example 5

[0073] This embodiment relates to a method for characterizing the crystal quality of an 8-inch 3C-SiC substrate, wherein the 3C-SiC substrate is prepared by a conventional preparation method, and comprises the following steps:

[0074] (1) placing the polished 3C-SiC substrate on the sample stage of an X-ray diffractometer, wherein the surface Warp value of the polished 3C-SiC substrate is less than 20 μm;

[0075] (2) X-rays were used to perform 9-point diffraction tests on the (112) and (113) crystal planes of the 3C-SiC substrate to obtain the half-height widths, where the incident angle for the diffraction test on the (112) crystal plane was 10.6°, and the exit angles were shown in Table 2; the incident angle for the diffraction test on the (113) crystal plane was 6.36°, and the exit angles were shown in Table 2; the scanning ranges of the (112) and (113) planes were no more than 2000 arcsec. The test results of the half-height widths of the two crystal planes are shown in Table 2.

[0076] In addition, for the same 3C-SiC substrate, a 9-point diffraction test was performed using the (111) crystal plane as a control test, and the incident angle of the (111) crystal plane diffraction test was 17.8°. The test results of the half-height width of the (111) crystal plane are shown in Table 2.

[0077] Table 2

[0078]

[0079]

[0080] According to the test results in Table 2, the difference between the half-width at half-height of the (113) crystal plane and the half-width at half-height of the (112) crystal plane of the 3C-SiC substrate tested is no more than 40 arcsec, which proves that the method of this embodiment can characterize the crystallization quality of the 3C-SiC substrate. Therefore, at this time, the half-width at half-height of the (112) crystal plane and the half-width at half-height of the (113) crystal plane are the crystallization quality parameters of the 3C-SiC epitaxial layer. According to the test data of the (111) crystal plane, when the 3C-SiC substrate is tested using the (111) crystal plane, although there is no test signal introduced into the 3C-SiC epitaxial layer like the 4H-SiC substrate, the half-width data obtained from the test at different test points are very different, which proves that the use of the (111) crystal plane for testing will be affected by the undulations of the substrate surface, resulting in a decrease in detection accuracy. In order to improve the detection accuracy, multiple polishing corrections are required. However, the 3C-SiC substrate after multiple polishing corrections cannot meet the use requirements. Therefore, the (111) crystal plane cannot be used to accurately characterize the crystal quality of the 3C-SiC substrate.

[0081] Example 6

[0082] This embodiment relates to a method for characterizing the crystal quality of a 6-inch 3C-SiC substrate, wherein the 3C-SiC substrate is prepared by a conventional preparation method, and comprises the following steps:

[0083] (1) placing the polished 3C-SiC substrate on the sample stage of an X-ray diffractometer, wherein the surface Warp value of the polished 3C-SiC substrate is less than 20 μm;

[0084] (2) X-rays were used to perform 5-point diffraction tests on the (112) and (113) crystal planes of the 3C-SiC substrate to obtain the half-height widths, where the incident angle for the diffraction test on the (112) crystal plane was 10.1°, and the exit angles were shown in Table 3; the incident angle for the diffraction test on the (113) crystal plane was 5.86°, and the exit angles were shown in Table 3; the scanning ranges of the (112) and (113) planes were no more than 2000 arcsec. The test results of the half-height widths of the two crystal planes are shown in Table 3.

[0085] Table 3

[0086]

[0087]

[0088] Example 7

[0089] This embodiment relates to a method for characterizing the crystal quality of an 8-inch 3C-SiC epitaxial layer, wherein the 3C-SiC epitaxial layer includes both a 4H-SiC substrate and 3C-SiC generated on the surface of the 4H-SiC substrate, and comprises the following steps:

[0090] (1) placing the polished 3C-SiC epitaxial layer on a sample stage of an X-ray diffractometer, wherein the surface Warp value of the polished 3C-SiC epitaxial layer is less than 20 μm;

[0091] (2) X-rays were used to perform 9-point diffraction tests on the (112) and (113) crystal planes of the 3C-SiC epitaxial layer to obtain the half-height widths, where the incident angle for the diffraction test on the (112) crystal plane was 11.1°, and the exit angles were shown in Table 4; the incident angle for the diffraction test on the (113) crystal plane was 6.86°, and the exit angles were shown in Table 4; the scanning ranges of the (112) and (113) planes were no greater than 2000 arcsec. The test results of the half-height widths of the two crystal planes are shown in Table 4.

[0092] Table 4

[0093]

[0094] According to the test results in Table 3 and Table 4, when the incident angle of the (112) crystal plane is 10.6°±0.5°, the exit angle of the (112) crystal plane in Table 1 and Table 2 is still within the range of 30.07°±0.5°, and when the incident angle of the (113) crystal plane changes from 6.36°±0.5°, the exit angle of the (112) crystal plane in Table 1 and Table 2 is still within the range of 35.87°±0.5°. And for the same test object, the difference between the half-height width of the (113) crystal plane and the half-height width of the (112) crystal plane is no more than 40 arcsec, proving that the accuracy of the crystal quality test of the (112) crystal plane and the (113) crystal plane is high.

[0095] The above are only embodiments of the present application. The protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for characterizing the crystalline quality of a 3C-SiC epitaxial layer, characterized in that: The steps include: (1) Placing the polished 3C-SiC epitaxial layer on the sample stage of an X-ray diffractometer; (2) X-ray diffraction test is performed on the (112) crystal plane and the (113) crystal plane of the 3C-SiC epitaxial layer to obtain the half-widths respectively. When the difference between the half-widths of the (113) crystal plane and the half-widths of the (112) crystal plane is no more than 40 arcsec, the half-widths of the (112) crystal plane and the half-widths of the (113) crystal plane are the crystallization quality parameters of the 3C-SiC epitaxial layer.

2. The method according to claim 1, characterized in that In step (2), the incident angle of the X-ray diffraction test on the (112) crystal plane of the 3C-SiC epitaxial layer is 10.6°±0.5°, and the exit angle is 30.07°±0.5°.

3. The method according to claim 1, characterized in that In step (2), the incident angle of the X-ray diffraction test on the (113) crystal plane of the 3C-SiC epitaxial layer is 6.36°±0.5°, and the exit angle is 35.87°±0.5°.

4. The method according to claim 1, characterized in that The surface Warp value of the polished 3C-SiC epitaxial layer is less than 20 μm; and / or In step (2), the scanning range of surfaces (112) and (113) is no more than 2000 arcsec.

5. The method according to claim 1, characterized in that The diameter of the 3C-SiC epitaxial layer is greater than 6 inches, preferably greater than 8 inches; and / or In step (2), at least 5 points of testing are performed on both the (112) crystal plane and the (113) crystal plane.

6. A method for characterizing the crystalline quality of a 3C-SiC substrate, characterized in that: The steps include: (1) Placing the polished 3C-SiC substrate on the sample stage of an X-ray diffractometer; (2) X-ray diffraction tests are performed on the (112) crystal plane and the (113) crystal plane of the 3C-SiC substrate to obtain the half-widths respectively. When the difference between the half-widths of the (113) crystal plane and the half-widths of the (112) crystal plane is no more than 40 arcsec, the half-widths of the (112) crystal plane and the half-widths of the (113) crystal plane are the crystal quality parameters of the 3C-SiC substrate.

7. The method according to claim 6, characterized in that In step (2), the incident angle of the X-ray diffraction test on the (112) crystal plane of the 3C-SiC substrate is 10.6°±0.5°, and the exit angle is 30.07°±0.5°.

8. The method according to claim 6, characterized in that In step (2), the incident angle of the X-ray diffraction test on the (113) crystal plane of the 3C-SiC substrate is 6.36°±0.5°, and the exit angle is 35.87°±0.5°.

9. The method according to claim 6, characterized in that The surface warpage of the polished 3C-SiC substrate is less than 20 μm.

10. The method according to claim 6, characterized in that The diameter of the 3C-SiC substrate is greater than 6 inches, preferably greater than 8 inches; and / or In step (2), at least 5 points of testing are performed on both the (112) crystal plane and the (113) crystal plane.

Citation Information

Patent Citations

  • Feed material for epitaxial growth of monocrystalline silicon carbide, and method for epitaxial growth of monocrystalline silicon carbide

    CN103270203A

  • Unit for liquid phase epitaxial growth of monocrystalline silicon carbide, and method for liquid phase epitaxial growth of monocrystalline silicon carbide

    CN103282557A

  • Method for detecting silicon carbide defects by X-ray diffractometer

    CN114778577A

  • Silicon carbide wafer with uniformly distributed stress and method for lossless and accurate determination of stress in each direction of wafer

    CN116657249A