Method and system for testing explosion related parameters of lithium ion battery

By testing parameters related to lithium-ion battery explosions, including the composition of explosive gases and the characteristics of mixed gases, the problem of unclear explosion mechanisms of lithium-ion batteries has been solved, safety guidelines have been provided, and the safety of lithium-ion battery storage and use has been improved.

CN118980943APending Publication Date: 2024-11-19PEOPLES POLICE UNIV OF CHINA (INT LAW ENFORCEMENT COOP INST OF THE MINISTRY OF PUBLIC SECURITY CHINA PEACEKEEPING POLICE TRAINING CENT)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411304417.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The explosion mechanism of lithium-ion batteries is unclear, making it impossible to effectively guide the safety protection of their storage and use.

Method used

A method for testing parameters related to lithium-ion battery explosions is provided, including obtaining the composition of the explosion gas and testing the combustible gas explosion characteristics of the mixed gas, determining the explosion intensity parameters and sensitive parameters, collecting thermal runaway gas and electrolyte vapor using a constant-volume pressure vessel, igniting the mixed gas and monitoring the pressure through a spherical explosion container, and precisely controlling the gas partial pressure by combining Dalton's law of partial pressure.

Benefits of technology

This study enables a detailed analysis of the lithium-ion battery explosion process, providing explosion intensity and sensitive parameters to guide the safety monitoring and protection of lithium-ion batteries during storage and use, and improving the accuracy and safety of the measurement method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980943A_ABST
    Figure CN118980943A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion battery explosion prevention and monitoring, and provides a lithium ion battery explosion parameter test method and test system. Explosion gas (thermal runaway gas and electrolyte steam) is mixed with air, and the combustible gas explosion characteristic test is carried out to obtain the explosion overpressure and the pressure rising rate. The inventor finds that the spraying process of the lithium ion battery is divided into a primary spraying stage and a main spraying stage. Primary spraying gas mainly comprises electrolyte steam with the boiling point lower than 130 DEG C, the low-boiling-point organic solvents in the electrolyte are gasified when heated and cause the internal pressure of the lithium ion battery to rise, and when the critical release pressure of a pressure relief opening is reached, the low-boiling-point organic solvents are sprayed out of the lithium ion battery. Main spraying gas is also called thermal runaway gas and mainly comes from redox reaction of positive and negative electrode materials and gas generated by reaction of the positive and negative electrode materials and ethylene carbonate. The obtained explosion overpressure and the pressure rising rate provide data support for the impact resistance of the lithium ion storage equipment and the plant wall.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery explosion prevention and monitoring, and in particular to a method and system for testing parameters related to lithium ion battery explosion. Background Art

[0002] Fuel shortage and air pollution are one of the main concerns of current and future energy issues. In order to reduce CO2 emissions and achieve sustainable development, people have been actively looking for various alternative energy sources to try to solve this problem from the root. Among them, lithium-ion batteries are widely used in consumer electronics, electric vehicles and energy storage fields because of their high energy density, long cycle life and environmental friendliness.

[0003] However, lithium-ion batteries themselves are relatively active, and related accidents occur frequently, especially accidental explosions in large energy storage power stations, which have attracted great public attention.

[0004] However, the explosion mechanism of lithium-ion batteries is still unclear, and it is impossible to provide guidance and protection for the storage and use of lithium-ion batteries. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a test method and test system for lithium ion battery explosion related parameters. The test method provided by the present invention can measure the parameters related to lithium ion explosion, and the explosion intensity obtained can provide technical guidance for the storage and use of lithium ion batteries.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for testing parameters related to lithium ion explosion, wherein the explosion related parameters include explosion intensity parameters, and the testing method comprises the following steps:

[0008] Obtaining explosion gas of the lithium-ion battery to be tested, wherein the explosion gas includes thermal runaway gas and electrolyte vapor, and analyzing to obtain the composition of the thermal runaway gas, the composition of the electrolyte vapor, and the ratio of the amount of the thermal runaway gas to the amount of the electrolyte vapor in the explosion gas;

[0009] The explosion gas and air are mixed, and the obtained mixed gas is subjected to a combustible gas explosion characteristic test to obtain the explosion intensity parameters, which include explosion overpressure and pressure rise rate.

[0010] Preferably, the lithium-ion battery to be tested is a ternary material lithium-ion battery or a lithium iron phosphate lithium-ion battery.

[0011] Preferably, the method for obtaining thermal runaway gas comprises the following steps:

[0012] In a constant volume pressure vessel, thermal runaway of the lithium-ion battery is triggered and the thermal runaway gas is collected.

[0013] Preferably, the electrolyte vapor is obtained by heating the electrolyte to initial spraying; the heating temperature range is a to 150°C, a=T+b, T is the boiling point of the low-boiling point organic solvent in the electrolyte, and the value range of b is 10 to 20°C.

[0014] Preferably, the combustible gas explosion characteristic test includes the following steps: inputting the mixed gas into a spherical explosion container, allowing it to stand for static equilibrium, igniting the mixed gas to achieve explosion, obtaining a pressure-time curve during the explosion, and obtaining the explosion overpressure and pressure rise rate based on the pressure-time curve.

[0015] Preferably, the static equilibrium time is ≥2 min; before the ignition, the pressure of the mixed gas in the spherical explosion container is normal pressure, the temperature range is a to 150°C, a=T+b, T is the boiling point of the low-boiling point organic solvent in the electrolyte, and the value range of b is 10 to 20°C.

[0016] Preferably, the partial pressures of the thermal runaway gas, electrolyte vapor and air in the mixed gas in the spherical explosion container are obtained by Dalton's law of partial pressures based on a set ratio of the amounts of the three gases in the mixed gas.

[0017] Preferably, the explosion-related parameters further include explosion-sensitive parameters, and the explosion-sensitive parameters include explosion limits, which are obtained by dichotomy.

[0018] Preferably, the dichotomy method includes: fixing the ratio of the amount of thermal runaway gas and electrolyte vapor in the explosion gas in the mixed gas, changing the ratio of the amount of the explosion gas in the mixed gas, and obtaining the explosion limit of the explosion gas.

[0019] The present invention also provides a test system for lithium-ion battery explosion-related parameters, comprising a combustible gas explosion characteristic test system and a mixed gas input system connected to the combustible gas explosion characteristic test system;

[0020] The combustible gas explosion characteristic testing system comprises a spherical explosion container;

[0021] An ignition device for igniting the gas in the spherical explosion container, the ignition device being located at the inner center of the spherical explosion container;

[0022] A vacuum pump for evacuating the spherical explosion container;

[0023] A control system for realizing the manipulation of the spherical explosion container;

[0024] A high frequency pressure sensor for realizing pressure monitoring of the spherical explosion container;

[0025] The mixed gas input system includes an evaporation premixing device;

[0026] The evaporation premixing device is provided with a gas inlet, an internal gas pipe, a gas outlet and a liquid inlet;

[0027] The gas outlet of the evaporation premixing device is connected to the first gas pipeline to realize the delivery of the gas in the evaporation premixing device to the spherical explosion container, and the first gas pipeline is provided with a solenoid valve and a pressure sensor in sequence along the air inlet direction;

[0028] The liquid inlet of the evaporation premixing device is connected to a microinjection pump to achieve the injection of electrolyte;

[0029] The gas inlet of the evaporation premixing device is connected to the second gas pipeline;

[0030] The second gas pipeline is connected to the air pump and the thermal runaway gas storage tank respectively through a three-way valve to achieve the injection of air and thermal runaway gas.

[0031] The invention provides a method for testing explosion-related parameters of a lithium-ion battery.

[0032] Beneficial effects:

[0033] 1. The inventors discovered that the eruption process of lithium-ion batteries is divided into two stages: initial spray and main spray. Therefore, the explosive gas erupted by lithium-ion batteries includes initial spray gas and main spray gas. The initial spray gas is mainly composed of electrolyte vapor with a boiling point below 130°C. The low-boiling point organic solvent in the electrolyte vaporizes when heated and causes the internal pressure of the lithium-ion battery to increase. When the critical release pressure of the pressure relief port is reached, it is ejected from the lithium-ion battery. The main spray gas, also called thermal runaway gas, mainly comes from the redox reaction of the positive and negative electrode materials and the gas generated by the reaction between the positive and negative electrode materials and ethylene carbonate. The schematic diagram of the lithium-ion battery explosion process is shown in the figure below. Figure 1 shown.

[0034] 2. The inventor mixed the explosion gas with air and conducted a combustible gas explosion characteristic test on the obtained mixed gas to obtain explosion intensity parameters, including explosion overpressure and pressure rise rate. The obtained explosion overpressure and pressure rise rate provide data support for the impact resistance of lithium-ion storage devices and factory walls.

[0035] 3. The present invention also provides the determination of explosion limits of explosion-sensitive parameters. The explosion limits can provide data support for the total concentration of thermal runaway gases and electrolyte vapor in the air of lithium-ion battery storage plants, thereby realizing safety monitoring and early prevention of lithium-ion battery storage plants.

[0036] 4. Furthermore, the present invention can accurately obtain the gas partial pressure of each gas in the mixed gas during the combustible gas explosion characteristic test through Dalton's law of partial pressure, realize precise control of the content, and thus improve the accuracy of the measurement method.

[0037] The present invention also provides a testing system for lithium-ion battery explosion-related parameters. The testing system provided by the present invention has a relatively simple structure and can achieve full mixing, explosion and detection of mixed gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of the explosion process of lithium-ion batteries;

[0039] Figure 2 A schematic diagram of a testing system for explosion-related parameters of a lithium-ion battery provided by the present invention;

[0040] Figure 3 This is a diagram showing the relationship between the explosion overpressure and the explosion gas concentration obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The present invention provides a method for testing explosion-related parameters of a lithium-ion battery, wherein the explosion-related parameters include explosion intensity parameters, and the method comprises the following steps:

[0042] Obtaining explosion gas of the lithium-ion battery to be tested, wherein the explosion gas includes thermal runaway gas and electrolyte vapor, and analyzing to obtain the composition of the thermal runaway gas, the composition of the electrolyte vapor, and the ratio of the amount of the thermal runaway gas to the amount of the electrolyte vapor in the explosion gas;

[0043] The explosion gas and air are mixed, and the obtained mixed gas is subjected to a combustible gas explosion characteristic test to obtain the explosion intensity parameters, which include explosion overpressure and pressure rise rate.

[0044] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.

[0045] The present invention obtains explosion gas of a lithium-ion battery to be tested, wherein the explosion gas includes thermal runaway gas and electrolyte vapor, and analyzes to obtain the composition of the thermal runaway gas, the composition of the electrolyte vapor, and the ratio of the amount of the thermal runaway gas to the amount of the electrolyte vapor in the explosion gas.

[0046] In the present invention, the lithium-ion battery to be tested is preferably a ternary material lithium-ion battery or a lithium iron phosphate lithium-ion battery. In the present invention, the ternary material in the ternary lithium-ion battery preferably includes lithium nickel cobalt manganese oxide. The present invention does not specifically limit the positive electrode material of the ion battery to be tested, and those skilled in the art can select it according to actual tests.

[0047] In the present invention, the explosion gas includes thermal runaway gas and electrolyte vapor.

[0048] In the present invention, the method for obtaining the thermal runaway gas preferably comprises the following steps:

[0049] In a constant volume pressure vessel, thermal runaway of the lithium-ion battery is triggered and the thermal runaway gas is collected.

[0050] In the present invention, the constant volume pressure vessel is preferably provided with a pressure sensor and a temperature sensor; the pressure sensor and the temperature sensor can record the pressure and temperature changes in the constant volume pressure vessel during the thermal runaway process. In the present invention, the constant volume pressure vessel is preferably replaced with nitrogen before the lithium-ion battery to be tested is placed therein, and the number of nitrogen replacements is preferably 4 times. The nitrogen replacement can obtain accurate components and contents of the thermal runaway gas, and can also avoid the risk of combustion and explosion of the thermal runaway gas. In the present invention, the triggering method is preferably to heat the constant volume pressure vessel, and the heated part is preferably the side of the constant volume pressure vessel. In the present invention, the collection method is preferably to collect with a gas collection bag.

[0051] In the present invention, the amount of substance of the thermal runaway gas is preferably obtained by the ideal gas equation, which is: PV=nRT, wherein P is the gas pressure in the constant volume pressure vessel, V is the volume of the constant volume pressure vessel, R is the Avogadro constant, and T is the gas temperature. Based on the parameters in the thermal runaway process, the amount of substance of the thermal runaway gas can be obtained.

[0052] In the present invention, the composition of the thermal runaway gas is preferably obtained by analyzing the thermal runaway gas; the analysis equipment is preferably a gas chromatograph. After the analysis, the present invention preferably further comprises: preparing the thermal runaway gas according to the obtained components and component contents, and the preparation preferably retains the gas components with a content of more than 1% in the thermal runaway gas. In the present invention, the prepared thermal runaway gas is preferably a standard thermal runaway gas. In the present invention, preparing the thermal runaway gas according to the analysis results can prevent the situation where the amount of thermal runaway gas directly collected is insufficient for subsequent tests.

[0053] In the present invention, the electrolyte vapor is preferably obtained by heating the electrolyte to the initial spray. In the present invention, the heating temperature range is preferably a to 150°C, a=T+b, T is the boiling point of the low-boiling organic solvent in the electrolyte, and the value range of b is 10 to 20°C. In the present invention, the electrolyte of the lithium-ion battery preferably includes an organic solvent and a lithium salt. The boiling points of the organic solvents are different, so the heating temperature for converting the organic solvent into vapor is different. In the present invention, the organic solvent preferably includes a cyclic carbonate compound and / or a chain carbonate, and is preferably a mixed solvent of a cyclic carbonate compound and a chain carbonate or a chain carbonate. In the present invention, the cyclic carbonate compound further preferably includes ethylene carbonate (EC) and / or propylene carbonate (PC). In the present invention, the chain carbonate preferably includes one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC). In the present invention, the lithium salt is preferably lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB) or lithium bis(trifluoromethanesulfonyl imide) (LiTFSI). In the present invention, the organic solvent in the electrolyte is generally a mixture of a high boiling point organic solvent and a low boiling point organic solvent, or a low boiling point organic solvent.

[0054] In the present invention, the amount of substance in the electrolyte vapor is preferably obtained by the following formula: n=Δm / M, wherein Δm is the mass loss of the electrolyte before and after heating to the initial spray, and M is the molar mass of the low boiling point organic solvent in the electrolyte.

[0055] In the present invention, the heating temperature is preferably obtained by analyzing the electrolyte components of the lithium ion battery to be tested. In a specific embodiment of the present invention, the electrolyte of the lithium iron phosphate lithium ion battery to be tested is sent for inspection, and the main components of the organic solvent in the electrolyte are EMC (boiling point 108°C) and EC (boiling point 248°C), that is, the lithium iron phosphate lithium ion battery can be initially sprayed at 120°C, at which time the low boiling point organic solvent EMC turns into steam and erupts from the battery valve, based on which the heating temperature is determined to be 120°C. In the present invention, the composition of the electrolyte vapor is preferably obtained by analyzing the electrolyte vapor; the analysis equipment is preferably a gas chromatograph. After the analysis, the present invention preferably further includes: preparing the electrolyte vapor according to the obtained components and component contents, and the preparation preferably retains the gas components with a content of more than 1% in the electrolyte vapor. In the present invention, the prepared electrolyte vapor is preferably a standard electrolyte vapor. In the present invention, the electrolyte vapor is prepared according to the analysis results, which can prevent the situation where the volume of the electrolyte vapor directly collected is insufficient for subsequent tests.

[0056] In the present invention, the ratio of the amount of the thermal runaway gas to the amount of the electrolyte vapor in the explosion gas can be calculated based on the obtained amount of the thermal runaway gas and the amount of the electrolyte vapor.

[0057] After obtaining the explosion gas of the lithium-ion battery to be tested, the present invention mixes the explosion gas with air, and performs a combustible gas explosion characteristic test on the obtained mixed gas to obtain the explosion intensity parameters, which include explosion overpressure and pressure rise rate.

[0058] In the present invention, the ratio of the amount of the explosive gas in the mixed gas is named as the concentration of the explosive gas.

[0059] In the present invention, the combustible gas explosion characteristic test preferably includes the following: inputting the mixed gas into a spherical explosion container, allowing it to stand for static equilibrium, igniting the mixed gas to achieve explosion, and obtaining a pressure-time curve during the explosion process; based on the pressure-time curve, obtaining the explosion overpressure and pressure rise rate.

[0060] In the present invention, the partial pressures of the thermal runaway gas, electrolyte vapor and air in the mixed gas in the spherical explosion container are preferably obtained by Dalton's law of partial pressures based on a set ratio of the amounts of the three gases in the mixed gas.

[0061] In the present invention, the static equilibrium time is preferably ≥ 2 min.

[0062] In the present invention, before the ignition, the pressure of the mixed gas in the spherical explosion container is preferably normal pressure, and the temperature range is a to 150° C., a=T+b, T is the boiling point of the low-boiling organic solvent in the electrolyte, and the value range of b is 10 to 20° C. In a specific embodiment of the present invention, the electrolyte organic solvent of the lithium iron phosphate lithium-ion battery preferably includes EMC, so the temperature of the mixed gas in the spherical explosion container is preferably 120° C.

[0063] In the present invention, the obtained explosion overpressure and pressure rise rate can judge the explosion hazard of lithium-ion batteries; at the same time, the explosion overpressure can guide the explosion resistance strength of protective equipment such as walls where lithium-ion batteries are stored.

[0064] In the present invention, the explosion correlation preferably further includes explosion sensitivity parameters, and the explosion sensitivity parameters preferably include explosion limits, and the explosion limits are preferably obtained by dichotomy.

[0065] In the present invention, the dichotomy preferably includes: fixing the ratio of the amount of thermal runaway gas and electrolyte vapor in the explosion gas, changing the proportion of the amount of explosion gas in the mixed gas (ie, the concentration of explosion gas), and obtaining the explosion limit of the explosion gas.

[0066] In the present invention, the explosion limit can obtain the explosion ratio of the mixed gas. This parameter can monitor and guide the environment in which the lithium-ion battery is located. Once the concentration of the explosive gas in the air (the ratio of the total amount of thermal runaway gas and electrolyte vapor to the amount of substance in the mixed gas) is found to be close to the explosion limit, some of the explosive gas can be discharged or inert gas can be filled in to reduce the concentration of the explosive gas, thereby avoiding explosion.

[0067] The present invention also provides a test system for lithium-ion battery explosion-related parameters, comprising a combustible gas explosion characteristic test system and a mixed gas input system connected to the combustible gas explosion characteristic test system;

[0068] The combustible gas explosion characteristic testing system comprises a spherical explosion container;

[0069] An ignition device for igniting the gas in the spherical explosion container, the ignition device being located at the inner center of the spherical explosion container;

[0070] A vacuum pump for evacuating the spherical explosion container;

[0071] A control system for realizing the manipulation of the spherical explosion container;

[0072] A high frequency pressure sensor for realizing pressure monitoring of the spherical explosion container;

[0073] The mixed gas input system includes an evaporation premixing device;

[0074] The evaporation premixing device is provided with a gas inlet, an internal gas pipe, a gas outlet and a liquid inlet;

[0075] The gas outlet of the evaporation premixing device is connected to the first gas pipeline to realize the delivery of the gas in the evaporation premixing device to the spherical explosion container, and the first gas pipeline is provided with a solenoid valve and a pressure sensor in sequence along the air inlet direction;

[0076] The liquid inlet of the evaporation premixing device is connected to a microinjection pump to achieve the injection of electrolyte;

[0077] The gas inlet of the evaporation premixing device is connected to the second gas pipeline;

[0078] The second gas pipeline is connected to the air pump and the thermal runaway gas storage tank respectively through a three-way valve to achieve the injection of air and thermal runaway gas.

[0079] Figure 2 A schematic diagram of a test system for lithium-ion battery explosion-related parameters provided by the present invention is shown below in conjunction with Figure 2 The test system provided by the present invention is described.

[0080] The test system provided by the invention comprises a combustible gas explosion characteristic test system.

[0081] In the present invention, the combustible gas explosion characteristic testing system comprises a spherical explosion container, and the spherical explosion container is preferably coated with a heating pipeline. In the present invention, the coating of the heating pipeline can ensure that the electrolyte vapor is in a gaseous state.

[0082] In the present invention, the combustible gas explosion characteristic test system includes an ignition device for igniting the gas in the spherical explosion container, and the ignition device is located at the inner center of the spherical explosion container. The ignition device is two tungsten needles, and the spacing between the two tungsten needles is preferably 5mm. In the present invention, the two tungsten needles can release a voltage of 5kV.

[0083] In the present invention, the combustible gas explosion characteristic testing system comprises a vacuum pump for evacuating the spherical explosion container.

[0084] In the present invention, the combustible gas explosion characteristic test system includes a control system for realizing the control of the spherical explosion container. In the present invention, the control system includes a computer, and the computer is provided with a relevant program. In the present invention, the control system can realize functions such as solenoid valve control, ignition and data recording.

[0085] In the present invention, the combustible gas explosion characteristic testing system includes a high-frequency pressure sensor for realizing pressure monitoring of the spherical explosion container.

[0086] The test system provided by the present invention comprises a mixed gas input system connected to the combustible gas explosion characteristic test system.

[0087] In the present invention, the mixed gas input system includes an evaporation premixing device.

[0088] In the present invention, the evaporation premixing device is preferably provided with a gas inlet, an internal gas pipe, a gas outlet and a liquid inlet. In the present invention, the gas outlet of the evaporation premixing device is connected to a first gas pipeline to realize the delivery of the gas in the evaporation premixing device to the spherical explosion container, and a solenoid valve and a pressure sensor are sequentially arranged on the first gas pipeline along the gas inlet direction; the first gas pipeline is preferably covered with a heating pipeline. In the present invention, the covering of the heating pipeline can ensure that the electrolyte vapor is in a gaseous state.

[0089] In the present invention, the liquid inlet of the evaporation premixing device is connected to a micro-injection pump to achieve the injection of the electrolyte.

[0090] In the present invention, the gas inlet of the evaporation premixing device is connected to the second gas pipeline.

[0091] In the present invention, the second gas pipeline is connected to the air pump and the thermal runaway gas storage tank respectively through a three-way valve to achieve the injection of air and thermal runaway gas.

[0092] Combine the following Figure 2 The test system describes the test method:

[0093] After calculating the partial pressure of the thermal runaway gas and the flow rate of the electrolyte:

[0094] The temperature in the spherical explosion container is controlled to be the set temperature through the heating pipeline, and then the spherical explosion container is evacuated by a vacuum pump; then the air pump and the micro-injection pump are closed, the input channel of the thermal runaway gas is opened, and the thermal runaway gas is introduced into the spherical explosion container. After the introduction is completed, the thermal runaway gas introduction channel is closed; the evaporation premixing device is opened, and after the temperature of the evaporation premixing device is stabilized, the micro-injection pump is opened to inject the electrolyte, and the air introduction channel is opened. The electrolyte evaporates in the evaporation premixing device to form electrolyte vapor, and is preliminarily mixed with the introduced air in the internal air pipe of the evaporation premixing device, and enters the spherical explosion container under the carry of air. After the internal pressure of the spherical explosion container reaches the set pressure (observed by a high-frequency pressure sensor), the solenoid valve is closed; it is left to stand for at least 2 minutes, and the mixed gas in the spherical explosion container is ignited by the control system, and the pressure-time curve is obtained by the control system and the high-frequency pressure sensor, and then based on the pressure-time curve, the explosion overpressure and the pressure rise rate are obtained.

[0095] The test method and system for the explosion-related parameters of a lithium-ion battery provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0096] Example 1

[0097] Taking a commercially available lithium iron phosphate lithium-ion battery as an example, the explosion intensity parameters are measured. The specific steps are as follows:

[0098] Acquisition of thermal runaway gas of lithium iron phosphate lithium-ion battery, and determination of composition and content: Before the experiment, the gas in the constant volume pressure vessel (the constant volume pressure vessel is equipped with a pressure sensor and a temperature sensor, which can record the pressure and temperature changes in the constant volume pressure vessel during thermal runaway) is replaced with nitrogen 4 times to ensure an inert gas environment, and the lithium iron phosphate lithium-ion battery to be tested is placed in the constant volume pressure vessel, and the thermal runaway of the lithium iron phosphate lithium-ion battery to be tested is triggered by side heating, and then the thermal runaway gas is collected by a gas collection bag. Based on the ideal gas deformation equation (Formula 1), the amount of substance of the generated thermal runaway gas is obtained:

[0099] n=PV / RT Formula 1.

[0100] In formula 1, P is the gas pressure in the constant volume pressure vessel, V is the volume of the constant volume pressure vessel, R is the Avogadro constant, and T is the gas temperature.

[0101] Analyze the collected thermal runaway gas: Analyze the thermal runaway gas by gas chromatography to obtain the components and component contents of the thermal runaway gas.

[0102] Since the amount of thermal runaway gas directly collected from thermal runaway is relatively small, the amount is insufficient for subsequent tests, so according to the components and contents detected by the gas chromatograph, the gas components with a content of more than 1% in the thermal runaway gas are retained to prepare the standard thermal runaway gas. Specifically, the thermal runaway gas includes the following components in volume concentration: hydrogen 54.9%, carbon dioxide 25.6%, carbon monoxide 5.2%, methane 7.3%, ethylene 5.6%, ethane 1.4%.

[0103] Determination of the vapor composition and content of the lithium iron phosphate lithium-ion battery electrolyte: The electrolyte of the lithium iron phosphate lithium-ion battery to be tested was sent for inspection, and the results were: the main components of the organic solvent in the electrolyte of the lithium iron phosphate battery are EMC (boiling point 108°C) and EC (boiling point 248°C). It is therefore believed that the lithium iron phosphate lithium-ion battery can initially spray at 120°C, at which time the low-boiling-point EMC turns into vapor and erupts from the battery valve. Based on this, it is determined that the vapor generation temperature of the lithium iron phosphate lithium-ion battery electrolyte is 120°C.

[0104] In order to accurately obtain the amount of substance in the electrolyte vapor inside the lithium iron phosphate lithium-ion battery, the lithium iron phosphate lithium-ion battery can be placed in a constant temperature box at 120°C and heated until the initial spray occurs. The mass change Δm before and after the lithium iron phosphate lithium-ion battery is heated to the initial spray occurs is weighed, and the amount of substance n of the electrolyte vapor is ele =Δm / 104 (104 is the relative molecular mass of EMC).

[0105] The final obtained ratio of the amount of explosive thermal runaway gas and electrolyte vapor in the lithium iron phosphate lithium-ion battery is 4.92:1.

[0106] use Figure 2 The test system is used to measure the explosion intensity parameters:

[0107] The concentration of the explosive gas in the mixed gas is set, and the pressure of the mixed gas in the spherical explosion container is set to normal pressure, i.e. 101 kPa, and the temperature is set to 120°C.

[0108] The concentration is determined by Dalton's law of partial pressure, and the partial pressure of each gas in the mixed gas is calculated. The specific calculation method is as follows:

[0109] 1. Fixed the ratio of the amount of thermal runaway gas and electrolyte vapor n gas / n eleIt is 4.92:1, and then the proportion of the amount of the explosive gas substance in the mixed gas is changed, that is, the concentration of the explosive gas is 5%.

[0110] 2. Under 120℃ environment, the volume of 1 mol of gas is 393 / 273×22.4=32.25L. During a single explosion test, the concentration of the explosion gas is first set to 5%, where the ratio of the amount of thermal runaway gas to the amount of electrolyte vapor is n gas / n ele =4.92:1. Among them, the partial pressure of thermal runaway gas is = (101-4) kPa × 32.25 L × c × n gas / (n gas +n ele ) / 20L=1.32(kPa); firstly, introduce thermal runaway gas, the specific steps are: control the temperature in the spherical explosion container to 120℃ through the heating pipeline, then use the vacuum pump to evacuate the spherical explosion container to 4kPa, then open the thermal runaway gas introduction pipeline to introduce thermal runaway gas, when the pressure change in the spherical explosion container reaches the other partial pressure of thermal runaway, that is, the pressure is 5.32kPa, then close the valve, at this time, the target concentration of thermal runaway gas has been reached in the 20L spherical explosion container.

[0111] 3. Then determine the electrolyte volume V = 104 × 20L × c × n corresponding to the electrolyte vapor that produces the corresponding partial pressure el e / 1.01×(n gas +n ele ) / 32.25(L / mol)=2.65mL (where 104 is the relative molecular mass of EMC and 1.01 is the density of EMC). Turn on the evaporation premixing device, and after the temperature of the evaporation premixing device is stable, turn on the microinjection pump (the microinjection pump is set with the amount of electrolyte and the introduction speed to ensure that EMC enters the spherical explosion container with a good partial pressure), inject EMC into the evaporation premixing device (120°C) for evaporation, and at the same time open the air inlet channel to let in air, and use air as a carrier gas to bring the generated electrolyte vapor into the spherical explosion container until the pressure in the spherical explosion container is 101kPa, and close the solenoid valve on the air intake pipe.

[0112] 4. The spherical explosion container is allowed to stand for 2 minutes to allow the gas in the spherical explosion container to be fully mixed, and then the mixed gas in the spherical explosion container is ignited using the control system. The pressure-time change curve during the explosion process is obtained through the control system and the high-frequency pressure sensor. Based on this pressure-change curve, the explosion overpressure and pressure rise rate when the explosion gas concentration is 5% can be obtained.

[0113] 5. Change the concentration of the explosion gas to 10%, 15%, 20%, 25% and 30%, and repeat steps 2 to 4 in sequence to obtain explosion overpressures and pressure rise rates when the explosion gas concentration is 5%, 10%, 15%, 20%, 25% and 30%.

[0114] The test was repeated with the explosion gas being pure EMC electrolyte vapor and pure thermal runaway gas as comparative examples, and the explosion overpressure and pressure rise rate were obtained when the explosion gas concentration was 5%, 10%, 15%, 20%, 25% and 30%.

[0115] The obtained explosion overpressure and explosion gas concentration data are plotted, and the results are as follows: Figure 3 shown.

[0116] from Figure 3 It can be seen that among the three media, although the explosion limit of EMC vapor is the smallest, only 2.85% to 14.25%, its explosion limit is the lowest, which indicates that EMC vapor alone is more likely to explode. The explosion limit of thermal runaway gas is the largest, 7.45% to 39.5%; the two-phase mixture is between the two, with an explosion limit range of 4.9% to 30.5%.

[0117] From the perspective of explosion intensity parameters, the peak explosion overpressure of EMC vapor is the highest, reaching 668.9 kPa. The peak explosion overpressure of thermal runaway gas is 549.2 kPa, the lowest among the three media, while the two-phase mixture is still at an intermediate level, with a peak explosion overpressure of 568.5 kPa.

[0118] The results show the explosion characteristics of EMC vapor and thermal runaway gas, that is, EMC is easy to explode and has the greatest explosion power, and although the thermal runaway gas explosion overpressure is low, it can explode in a larger concentration range. As for the explosion parameters of the two-phase mixture, they are at an intermediate level between the two, which not only expands the explosion range but also increases the explosion power. The explosion parameter results of battery ejecta tested by this method can serve the thermal runaway explosion hazard assessment of lithium-ion batteries and be used for energy storage system safety design and accident protection.

[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for testing parameters related to lithium ion explosion, characterized in that: The explosion-related parameters include explosion intensity parameters, and the testing method includes the following steps: Obtaining explosion gas of the lithium-ion battery to be tested; the explosion gas includes thermal runaway gas and electrolyte vapor, and analyzing to obtain the composition of the thermal runaway gas, the composition of the electrolyte vapor, and the ratio of the amount of thermal runaway gas and electrolyte vapor in the explosion gas; The explosion gas and air are mixed, and the obtained mixed gas is subjected to a combustible gas explosion characteristic test to obtain the explosion intensity parameters, which include explosion overpressure and pressure rise rate.

2. The testing method according to claim 1, characterized in that: The lithium-ion battery to be tested is a ternary material lithium-ion battery or a lithium iron phosphate lithium-ion battery.

3. The testing method according to claim 1, characterized in that: The method for obtaining the thermal runaway gas comprises the following steps: In a constant volume pressure vessel, thermal runaway of the lithium-ion battery is triggered and the thermal runaway gas is collected.

4. The testing method according to claim 1, characterized in that: The electrolyte vapor is obtained by heating the electrolyte to the initial spraying; the heating temperature range is a to 150°C, a=T+b, T is the boiling point of the low-boiling point organic solvent in the electrolyte, and the value range of b is 10 to 20°C.

5. The testing method according to claim 1, characterized in that: The combustible gas explosion characteristic test comprises the following steps: inputting the mixed gas into a spherical explosion container, allowing it to stand for static equilibrium, igniting the mixed gas to achieve explosion, obtaining a pressure-time curve during the explosion, and obtaining the explosion overpressure and pressure rise rate based on the pressure-time curve.

6. The testing method according to claim 5, characterized in that: The static equilibrium time is ≥2min; before the ignition, the pressure of the mixed gas in the spherical explosion container is normal pressure, the temperature range is a~150℃, a=T+b, T is the boiling point of the low-boiling point organic solvent in the electrolyte, and the value range of b is 10~20℃.

7. The testing method according to claim 6, characterized in that: The partial pressures of the thermal runaway gas, electrolyte vapor and air in the mixed gas in the spherical explosion container are obtained by Dalton's law of partial pressures based on a set ratio of the amounts of the three gases in the mixed gas.

8. The testing method according to claim 1, characterized in that: The explosion-related parameters also include explosion-sensitive parameters, and the explosion-sensitive parameters include explosion limits, which are obtained by dichotomy.

9. The testing method according to claim 8, characterized in that: The dichotomy method includes: fixing the ratio of the amount of thermal runaway gas and electrolyte vapor in the explosion gas in the mixed gas, changing the proportion of the amount of the explosion gas in the mixed gas, and obtaining the explosion limit of the explosion gas.

10. A testing system for lithium-ion battery explosion-related parameters, characterized in that: It includes a combustible gas explosion characteristic test system and a mixed gas input system connected to the combustible gas explosion characteristic test system; The combustible gas explosion characteristic testing system comprises a spherical explosion container; An ignition device for igniting the gas in the spherical explosion container, the ignition device being located at the inner center of the spherical explosion container; A vacuum pump for evacuating the spherical explosion container; A control system for realizing the manipulation of the spherical explosion container; A high frequency pressure sensor for realizing pressure monitoring of the spherical explosion container; The mixed gas input system includes an evaporation premixing device; The evaporation premixing device is provided with a gas inlet, an internal gas pipe, a gas outlet and a liquid inlet; The gas outlet of the evaporation premixing device is connected to the first gas pipeline to realize the delivery of the gas in the evaporation premixing device to the spherical explosion container, and the first gas pipeline is provided with a solenoid valve and a pressure sensor in sequence along the air inlet direction; The liquid inlet of the evaporation premixing device is connected to a microinjection pump to achieve the injection of electrolyte; The gas inlet of the evaporation premixing device is connected to the second gas pipeline; The second gas pipeline is connected to the air pump and the thermal runaway gas storage tank respectively through a three-way valve to achieve the injection of air and thermal runaway gas.