THBC solar cell structure and preparation method thereof
By using p+hydrogenated amorphous silicon or microcrystalline silicon and front surface field or floating junction layer in TBC solar cells, the problem of preparation difficulty and carrier transmission of the back surface p+ polysilicon is solved, and the short-circuit current density and open circuit voltage of the solar cell are improved. .
Patent Information
- Application Number
- CN202411041213.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing tunnel oxide passivation contact back contact (TBC) solar cells are difficult to prepare p+ polysilicon on the back, limiting the interfacial passivation and carrier collection effects, and the electrodelessness on the front increases the difficulty of photogenerated carrier collection.
Use p+hydrogenated amorphous silicon or p+hydrogenated microcrystalline silicon to replace the p+ polysilicon with poor passivation in TBC, and insert the front surface field (FSF) or front floating junction (FFE) layer on the front surface of the battery to improve photogenerating carriers Transmission distance to the back.
The passivation and carrier transmission performance of the p+ area on the back of the TBC solar cell is significantly improved, the short-circuit current density JSC is increased by 0.2~0.7mA/cm2, and the open-circuit voltage VOC is increased by 10~20mV, enhancing the photoelectric conversion efficiency of the battery.
Smart Images

Figure CN118983365A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of solar cells, in particular to a tunneling oxide passivated heterojunction back contact (THBC) solar cell structure and a preparation method thereof. Background Art
[0002] Tunnel oxide passivated back contact (TBC) solar cells combine interdigitated back contact (IBC) cells with TOPCon cell technology, taking advantage of the low cost and high efficiency potential of the TOPCon structure. However, the p-type back contact of TBC solar cells is currently limited. + The difficulty of preparing polycrystalline silicon limits the full play of the interface passivation and carrier collection effects; and since there is no electrode on the front side, all photogenerated carriers on the crystalline silicon substrate need to be transferred to the back side to be collected by the electrode, which increases the difficulty of collecting photogenerated carriers near the front surface of the cell. The carrier transmission distance of existing crystalline silicon heterojunction solar cells is long, and the quality requirements of silicon substrates and passivation films are high, while existing heterojunction back contact (HBC) solar cells can only realize the passivation function and cannot transmit carriers. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, the present invention proposes a THBC solar cell structure and a preparation method thereof, which utilizes the superior interface passivation characteristics of heterojunction (SHJ) solar cells to passivate the poorly passivated p-type TBC solar cells. + Polysilicon is replaced by p + Hydrogenated amorphous silicon or p + Hydrogenated microcrystalline silicon; at the same time, the front surface field (FSF) or front floating junction (FFE) is inserted on the front surface of the cell to increase the transmission distance of photogenerated carriers from the front surface of the crystalline silicon substrate to the back surface, thereby significantly improving the back surface p of the TBC solar cell. + Regional interface passivation and carrier transport properties.
[0004] The present invention is achieved through the following technical solutions:
[0005] The present invention relates to a THBC solar cell structure, comprising: a substrate, n + Front surface field layer or p + The front floating junction layer, the aluminum oxide passivation layer and the hydrogenated silicon nitride anti-reflection layer are sequentially arranged on the back surface side of the substrate, the tunneling oxide layer, the phosphorus-doped n + Polysilicon layer, boron-doped p + Amorphous silicon layer or microcrystalline silicon layer, hydrogenated silicon nitride passivation layer and metal electrode.
[0006] The substrate is an industrial-grade n-type Cz single-crystal silicon wafer with a crystal orientation of (100).
[0007] The present invention relates to a method for preparing the above-mentioned THBC solar cell structure, wherein the pre-treated substrate is subjected to high temperature diffusion to form n + After the front surface field FSF layer, SiO is formed on the back by high temperature thermal oxidation. 2 layer; then through the mask method on the SiO 2 Phosphorus-doped n + Polysilicon layer and boron-doped p + After the amorphous silicon layer, a hydrogenated silicon nitride passivation layer is further deposited. + Al is deposited on the front surface field layer 2 O 3 Passivation layer and SiN x :H anti-reflection layer; finally, Ag / Al and Ag electrodes are prepared on the hydrogenated silicon nitride passivation layer by screen printing.
[0008] The front surface FFE layer and the front surface FSF layer are both realized by high temperature diffusion doping.
[0009] The boron doping concentration range of the front surface FFE layer is 8×10 18 ~1×10 20 cm -3 , the doping junction depth ranges from 0.8 to 2.0 μm.
[0010] The phosphorus doping concentration of the front surface FSF layer is in the range of 5×10 19 ~1×10 21 cm -3 , the doping junction depth ranges from 1.0 to 2.5μm. Technical Effects
[0011] The present invention adopts p + Hydrogenated amorphous silicon or p + Hydrogenated microcrystalline silicon enhances the back surface of TBC solar cells + The front surface field FSF or front floating junction FFE is inserted on the front side, where the FSF layer has the function of field effect passivation and the FFE layer has the effect of "pumping effect" generated by the voltage gradient, both of which can increase the transmission distance of photogenerated carriers from the front surface of the crystalline silicon substrate to the back side, thereby improving the short-circuit current density of the battery. Compared with the prior art, the present invention makes the short-circuit current density J SC Increase 0.2~0.35mA / cm 2 , open circuit voltage V OC Increase 10~20mV; p + Hydrogenated microcrystalline silicon can make J SC Increase 0.3~0.48mA / cm 2 , V OCIncrease by 3~7mV; the use of the front surface field FSF layer can make J SC Increase 0.25~0.35mA / cm 2 , the front floating junction FFE layer can make J SC Increase 0.5~0.7mA / cm 2 , V OC All remain unchanged. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1-Figure 3 Flow chart of the present invention, wherein:
[0013] Figure 1 This is a schematic diagram of the silicon wafer after texturing;
[0014] Figure 2 Schematic diagram of a silicon wafer with a front surface field FSF or floating junction FFE layer prepared on the front side and a tunnel oxide layer, p+ amorphous silicon or p+ microcrystalline silicon layer, and n+ polycrystalline silicon covered on the back side;
[0015] Figure 3 This is a schematic diagram of the final THBC crystalline silicon solar cell structure;
[0016] In the figure: 1-n type crystalline silicon substrate, 2-n + Front surface field FSF or p + Front floating junction FFE layer, 3-tunneling oxide layer, 4-n + Polysilicon layer, 5-p + Amorphous silicon or microcrystalline silicon layer, 6-aluminum oxide passivation layer, 7 and 8-hydrogenated silicon nitride anti-reflection layer, 9-metal electrode;
[0017] Figure 4 Schematic diagram of the mask. DETAILED DESCRIPTION
[0018] like Figure 1-Figure 3 As shown, this embodiment relates to a method for preparing a THBC solar cell structure, comprising:
[0019] Step 1, prepare an industrial-grade n-type Cz single crystal silicon wafer with a crystal orientation of (100) as a crystalline silicon substrate, the thickness of the silicon wafer is 110 μm, and the resistivity is 0.5 Ω·cm; use an alkaline solution to remove the cutting damage layer on the silicon surface;
[0020] Step 2, using a 1% KOH solution to texturize the n-type silicon wafer obtained in step 1 at a texturizing temperature of 80° C., and then performing standard RCA cleaning to obtain a pre-treated silicon wafer;
[0021] Step 3: Place the n-type silicon wafer obtained in step 2 into a high temperature diffusion furnace for P 2 O 5 Phosphorus diffuses to form n on the front side+ Front surface field FSF layer.
[0022] Step 4: After the silicon wafer obtained in step 3 is etched around the edges, the back surface of the silicon wafer is polished with a 15% KOH solution at a solution temperature of 90°C for 15 minutes; then a SiO2 layer with a thickness of 1 nm is grown on the back surface by high temperature thermal oxidation. 2 layer, thermal oxidation temperature 650℃.
[0023] Step 5: insert the first mask on the back of the silicon wafer obtained in step 4, use PECVD equipment to deposit phosphorus-doped amorphous silicon, introduce silane, phosphine and hydrogen gas, wherein the phosphine gas flow ratio is 4%, and deposit n-doped silicon with a thickness of 70nm. + Amorphous silicon; then n + Amorphous silicon is annealed at high temperature to form n + Polysilicon, phosphorus doping concentration is 2×10 20 cm -3 .
[0024] Step 6, take out the first mask from the back of the silicon wafer obtained in step 5 and insert the second mask, use the same PECVD equipment as step 5 to deposit boron-doped amorphous silicon, wherein the power supply power is 4kW, the deposition temperature is 250°C, and the deposition pressure is 300Pa; introduce silane, borane and hydrogen gases, wherein the borane gas flow ratio is 2.5%, and the p-type silicon with a deposition thickness of 50nm is deposited. + Amorphous silicon, doping concentration 5.5×10 19 ;
[0025] The first and second masks have the same structure and are centrally symmetrically arranged so that their holes are distributed in an interdigitated manner. Figure 4 As shown, the first mask covers all areas except the red area, and n + Polysilicon; the second mask covers all areas except the blue area, and p is prepared in the blue area + Amorphous silicon.
[0026] Step 7, after removing the back borosilicate glass and phosphosilicate glass from the silicon wafer obtained in steps 5 and 6 and cleaning it, a hydrogenated silicon nitride passivation layer with a thickness of 100 nm is deposited on the corresponding area.
[0027] Step 8: After removing the phosphosilicate glass from the front side of the silicon wafer obtained in step 7 and cleaning it, Al is deposited by using an ALD device and a PECVD device respectively. 2 O 3 Passivation layer and SiN x :H anti-reflection layer, with thicknesses of 2nm and 75nm respectively.
[0028] Step 9: The back side of the silicon wafer obtained in step 8 + and n + The regions were covered with Ag / Al paste and Ag paste by screen printing, and finally co-sintered in an infrared belt sintering furnace to obtain metal electrodes.
[0029] like Figure 3 As shown in the figure, the THBC solar cell prepared according to the above method in this embodiment comprises: an n-type crystalline silicon substrate 1, n-type crystalline silicon substrates 1 and n-type crystalline silicon substrates 1 and 1 + Front surface field FSF or p + The front floating junction FFE layer 2, the aluminum oxide passivation layer 6, the hydrogenated silicon nitride anti-reflection layer 7 and the tunneling oxide layer 3, n type crystalline silicon substrate 1 are sequentially located on the back surface + Polysilicon layer 4, p + Amorphous silicon or microcrystalline silicon layer 5 , metal electrode 9 of hydrogenated silicon nitride passivation layer 8 .
[0030] After specific practical experiments, the solar cells prepared under the specific environment setting at room temperature were tested for short-circuit current density J SC Increase 0.25mA / cm 2 , open circuit voltage V OC Increase 16mV; p + Hydrogenated microcrystalline silicon can make J SC Increase 0.4mA / cm 2 , V OC Increase 5mV; the use of the front surface field FSF layer can make J SC Increase 0.3mA / cm 2 , the front floating junction FFE layer can make J SC Increase 0.55mA / cm 2 , V OC All remain unchanged.
[0031] Compared with the prior art, the back of the battery of the present invention no longer uses the p-type + Polysilicon, and use p-type silicon with better passivation performance and simpler process + Amorphous silicon or p + Microcrystalline silicon; and doping is performed on the front surface of the THBC solar cell to prepare a phosphorus-doped FSF layer or a boron-doped FFE layer that can enhance carrier transport performance.
[0032] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A THBC solar cell structure, characterized in that: include: a substrate, and n + Front surface field layer or p + The front floating junction layer, the aluminum oxide passivation layer and the hydrogenated silicon nitride anti-reflection layer are sequentially arranged on the back surface side of the substrate, the tunneling oxide layer, the phosphorus-doped n + Polysilicon layer, boron-doped p + Amorphous silicon layer or microcrystalline silicon layer, hydrogenated silicon nitride passivation layer and metal electrode.
2. The THBC solar cell structure according to claim 1, characterized in that: The substrate is an industrial-grade n-type Cz single-crystal silicon wafer with a crystal orientation of (100).
3. The THBC solar cell structure according to claim 1, characterized in that: The boron doping concentration range of the front surface FFE layer is 8×10 18 ~1×10 20 cm -3 , the doping junction depth range is 0.8~2.0μm; the phosphorus doping concentration range of the front surface FSF layer is 5×10 19 ~1×10 21 cm -3 , the doping junction depth ranges from 1.0 to 2.5μm.
4. A method for preparing the THBC solar cell structure according to any one of claims 1 to 3, characterized in that: The pre-treated substrate is diffused at high temperature to form n + After the front surface field FSF layer, a SiO2 layer is formed on the back by high temperature thermal oxidation; then phosphorus-doped n-type + Polysilicon layer and boron-doped p + After the amorphous silicon layer, a hydrogenated silicon nitride passivation layer is further deposited. + Al2O3 passivation layer and SiN are deposited on the front surface field layer in sequence. x :H anti-reflection layer; finally, Ag / Al and Ag electrodes are prepared on the back hydrogenated silicon nitride passivation layer by screen printing.
5. The preparation method according to claim 4, characterized in that include: Step 1, prepare an industrial-grade n-type Cz single crystal silicon wafer with a crystal orientation of (100) as a crystalline silicon substrate, the thickness of the silicon wafer is 110 μm, and the resistivity is 0.5 Ω·cm; use an alkaline solution to remove the cutting damage layer on the silicon surface; Step 2, using a 1% KOH solution to texturize the n-type silicon wafer obtained in step 1 at a texturizing temperature of 80° C., and then performing standard RCA cleaning to obtain a pre-treated silicon wafer; Step 3: Place the n-type silicon wafer obtained in step 2 into a high-temperature diffusion furnace for P2O5 phosphorus diffusion to form n-type silicon wafer on the front side. + Front surface field FSF layer; Step 4: After the silicon wafer obtained in step 3 is etched around the edges, the back surface of the silicon wafer is polished using a 15% KOH solution at a solution temperature of 90°C for 15 minutes; then a SiO2 layer with a thickness of 1 nm is grown on the back by high-temperature thermal oxidation at a thermal oxidation temperature of 650°C; Step 5: insert the first mask on the back of the silicon wafer obtained in step 4, use PECVD equipment to deposit phosphorus-doped amorphous silicon, introduce silane, phosphine and hydrogen gas, wherein the phosphine gas flow ratio is 4%, and deposit n-doped silicon with a thickness of 70nm. + Amorphous silicon; then + Amorphous silicon is annealed at high temperature to form n + Polysilicon, phosphorus doping concentration is 2×10 20 cm -3 ; Step 6, take out the first mask from the back of the silicon wafer obtained in step 5 and insert the second mask, use the same PECVD equipment as step 5 to deposit boron-doped amorphous silicon, wherein the power supply power is 4kW, the deposition temperature is 250°C, and the deposition pressure is 300Pa; introduce silane, borane and hydrogen gases, wherein the borane gas flow ratio is 2.5%, and the p-type silicon with a deposition thickness of 50nm is deposited. + Amorphous silicon, doping concentration 5.5×10 19 ; Step 7, after removing the back borosilicate glass and phosphosilicate glass from the silicon wafer obtained in steps 5 and 6 and cleaning it, a hydrogenated silicon nitride passivation layer with a thickness of 100 nm is deposited on the corresponding area; Step 8: After removing the phosphosilicate glass from the front side of the silicon wafer obtained in step 7 and cleaning it, an Al2O3 passivation layer and a SiN x :H anti-reflection layer, thickness is 2nm and 75nm respectively; Step 9: The back side of the silicon wafer obtained in step 8 + and n + The regions were covered with Ag / Al paste and Ag paste by screen printing, and finally co-sintered in an infrared belt sintering furnace to obtain metal electrodes.
6. The preparation method according to claim 4 or 5, characterized in that: The front surface FFE layer and the front surface FSF layer are both realized by high temperature diffusion doping.
7. The preparation method according to claim 4 or 5, characterized in that: The first and second mask plates have the same structure and are centrally symmetrically arranged so that their holes are distributed in an interdigitated manner, wherein: the uncovered area of the first mask plate is used to prepare n + Polysilicon; the area not covered by the second mask is used to prepare p + Amorphous silicon.
Citation Information
Patent Citations
Solar cell and method for manufacturing the same
CN104282782A
Back-surface tunnel oxidation and passivation inter-digitated type back-to-back contact battery production method
CN106784069A
Double-sided passivation back contact heterojunction solar cell and manufacturing method thereof
CN110634961A
Interdigital back contact solar cell structure and manufacturing method thereof
CN111613688A
Cited By
Back contact cell and etching‑free manufacturing method therefor, and cell assembly