Zinc negative electrode, preparation method thereof and zinc-air battery

By using thiol compounds containing benzene rings in zinc-air batteries, the problems of hydrogen evolution and corrosion of zinc negative electrodes are solved, the stability and cycle life of the battery are improved, the preparation process is simplified, and the application scenario is expanded .

CN118983390AActive Publication Date: 2024-11-19TAN KAH KEE INNOVATION LAB

Patent Information

Application Number
CN202411058073.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Due to the problems of hydrogen evolution, corrosion, passivation, dendrite, etc. of zinc negative electrode, the Coulomb efficiency and short cycle life are caused. The existing coating methods have uniformity, adhesion, interface resistance, chemical stability and complex process. Problems, limiting their effectiveness and scope of application.

Method used

The thiol compound containing benzene ring is used as a single molecule layer to self-assemble on the surface of the zinc foil to form a Zn-S bond, inhibit dendrites' growth and improve ion conductivity, and simplify the preparation process by impregnation and self-assembly.

Benefits of technology

Effectively inhibit dendrites growth, improve battery stability and cycling efficiency, enhance electrode surface protection, reduce side reactions, simplify processes and reduce costs, extend battery service life, and improve safety and application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983390A_ABST
    Figure CN118983390A_ABST
Patent Text Reader

Abstract

The invention provides a zinc negative electrode, a preparation method thereof and a zinc-air battery, and particularly relates to the technical field of zinc-air batteries. The zinc negative electrode comprises a zinc foil and a monomolecular layer self-assembled on the surface of the zinc foil, wherein the monomolecular layer is made of a sulfhydryl compound containing a benzene ring. According to the zinc negative electrode provided by the invention, the monomolecular layer is self-assembled on the zinc foil, sulfydryl in the sulfydryl compound containing the benzene ring reacts with the zinc foil to generate a Zn-S bond so as to stably exist on the surface of the zinc foil, and meanwhile, the zinc negative electrode has a hydrophilic metal tail group-SH, and can guide zinc ions in electrochemical reaction to uniformly deposit and nucleate and isolate water molecules, so that dendritic crystal growth is effectively inhibited. Besides, the sulfhydryl compound containing the benzene ring has relatively good ionic conductivity, so that the problem of high interface resistance of the coating is effectively inhibited, and good ionic conductivity between the zinc negative electrode and the electrolyte is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal-air batteries, and in particular to a zinc negative electrode and a preparation method thereof, and a zinc-air battery. Background Art

[0002] With the intensification of energy security and energy environment issues, it is urgent to develop high energy density and high safety energy storage systems. Zinc-air batteries have attracted widespread attention due to their high energy density, high safety, and low cost. However, problems such as hydrogen evolution, corrosion, passivation, dendrites, and deformation related to the zinc negative electrode have led to low coulombic efficiency and short cycle life of zinc-air batteries, which have become the main problems restricting the development of zinc-air batteries.

[0003] At present, the common zinc negative electrode solution strategies can be divided into the design of the anode electrode structure, the construction of the interface engineering and the optimization of the electrolyte. Among them, coating modification is one of the more effective methods. The coating method in the modification of the zinc battery negative electrode has many significant advantages, including inhibiting the growth of zinc dendrites, reducing side reactions, improving interface stability, improving electrochemical performance, promoting uniform current distribution, enhancing mechanical stability and multifunctional design. The coating can form a physical barrier, effectively inhibit the growth of zinc dendrites, prevent short circuits and battery failure, prevent direct contact between zinc and the electrolyte, reduce side reactions (such as zinc corrosion and hydrogen evolution reaction), thereby improving the coulombic efficiency and cycle life of the battery; it can improve the stability of the interface between the zinc negative electrode and the electrolyte, reduce the change of the interface impedance, and maintain the stable performance of the battery; it can promote uniform current distribution and reduce the growth of dendrites and electrode loss caused by excessive local current density. These advantages significantly improve the cycle life and performance of the battery.

[0004] However, the coating method still has certain challenges, including coating uniformity problems, insufficient adhesion, increased interfacial resistance, insufficient chemical stability, and complex processes. These shortcomings may limit the effectiveness and application scope of the coating. The non-uniformity of the coating will lead to uneven current density distribution, which in turn triggers local zinc dendrite growth. Uneven coating thickness will affect the electrochemical performance and stability of the electrode; the coating material does not have strong enough adhesion to the zinc substrate, and is easy to fall off during the battery charge and discharge cycle, thus losing its protective effect. The mechanical strength and toughness of the coating are insufficient, and it is easy to crack or peel off during repeated volume changes (such as charging and discharging); the coating material may increase the interfacial resistance between the zinc negative electrode and the electrolyte, reducing the overall conductivity and power performance of the battery; the ionic conductivity of the coating material is usually lower than that of the electrolyte, which may limit the ion transmission rate and affect the battery's charge and discharge efficiency. The chemical stability of the coating material in the electrochemical environment may be insufficient, and it will degrade after long-term use, resulting in a weakened protective effect. Some coating materials have poor stability in the electrolyte and may dissolve or react, resulting in coating failure. The coating process may involve a complex manufacturing process, increasing production costs and time.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] One of the purposes of the present invention is to provide a zinc negative electrode, aiming to solve at least one of the above-mentioned technical problems in the prior art.

[0007] A second object of the present invention is to provide a method for preparing a zinc negative electrode.

[0008] A third object of the present invention is to provide a zinc-air battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A first aspect of the present invention provides a zinc negative electrode, comprising a zinc foil and a monomolecular layer self-assembled on the surface of the zinc foil;

[0011] Wherein, the material of the monomolecular layer is a thiol compound containing a benzene ring.

[0012] Furthermore, the benzene ring-containing mercapto compound includes at least one of mercaptan, thiophenol and thiocarboxylic acid.

[0013] Preferably, the thiol comprises 1,4-phenyldithiol.

[0014] Preferably, the thiophenol includes at least one of thiophenol, 4-hydroxythiophenol and 4-mercaptothiophenol.

[0015] Preferably, the thiocarboxylic acid comprises 4-mercaptobenzoic acid.

[0016] The second aspect of the present invention provides a method for preparing the zinc negative electrode according to the first aspect, comprising the following steps:

[0017] The zinc foil is immersed in a solution of a thiol compound containing a benzene ring, and the thiol compound containing a benzene ring is self-assembled on the surface of the zinc foil to obtain the zinc negative electrode.

[0018] Furthermore, the concentration of the thiol compound solution is 0.01M to 0.1M.

[0019] Preferably, the immersion time is 12 h to 48 h.

[0020] Furthermore, the preparation method further comprises pre-treating the zinc foil before impregnation;

[0021] The pretreatment includes grinding, cleaning and drying of the zinc foil.

[0022] Furthermore, sandpaper is used for the polishing.

[0023] Preferably, the roughness of the sandpaper is 800-2000 meshes.

[0024] Furthermore, the cleaning includes cleaning with an organic solvent and rinsing with deionized water in this order.

[0025] Preferably, the organic solvent comprises acetone and / or alcohol.

[0026] Preferably, the organic solvent cleaning method is ultrasonic cleaning.

[0027] Preferably, the ultrasonic cleaning time is 10 min to 20 min.

[0028] Preferably, the deionized water is rinsed 2 to 5 times.

[0029] Furthermore, the drying process is carried out under nitrogen protection.

[0030] The third aspect of the present invention provides a zinc-air battery, comprising a positive electrode, a negative electrode and an electrolyte;

[0031] Wherein, the negative electrode is the zinc negative electrode described in the first aspect.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] The zinc negative electrode provided by the present invention self-assembles a monomolecular layer on the zinc foil, and the mercapto group in the mercapto compound containing a benzene ring reacts with the zinc foil to generate a Zn-S bond and stably exists on the surface of the zinc foil. At the same time, it has a metal-philic tail group -SH, which guides the zinc ions in the electrochemical reaction to uniformly deposit and nucleate, isolates water molecules, and thus effectively inhibits the growth of dendrites. In addition, the mercapto compound containing a benzene ring has good ionic conductivity, effectively inhibits the problem of high interface resistance of the coating, and ensures good ionic conductivity between the zinc negative electrode and the electrolyte.

[0034] The preparation method of the zinc negative electrode provided by the present invention forms a monolayer on the surface of the zinc foil by impregnation and self-assembly, without the need for complex equipment or high-energy-consuming processes, making the preparation process simple and convenient. The self-assembly of the mercapto compound containing a benzene ring on the surface of the zinc foil can form a uniform and closely arranged monolayer, which helps the uniform growth of the zinc deposition layer in the electrochemical reaction, thereby improving the performance of the battery. The preparation method has good repeatability and improves the consistency and reliability of the zinc negative electrode.

[0035] The zinc-air battery provided by the present invention, in view of the advantages brought by the above-mentioned zinc negative electrode, makes the prepared zinc-air battery have better stability, efficiency and safety, expands the application field of zinc-air battery, and expands the development of downstream industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 This is the Fourier infrared characterization image obtained in Test Example 1;

[0038] Figure 2 This is a SEM image of the zinc negative electrode obtained in Example 1 after immersion;

[0039] Figure 3 Another SEM image of the zinc negative electrode obtained in Example 1 after immersion;

[0040] Figure 4 This is a SEM image of the zinc negative electrode obtained in Comparative Example 1 after immersion;

[0041] Figure 5 Another SEM image of the zinc negative electrode obtained in Comparative Example 1 after immersion;

[0042] Figure 6 The Tafel curve obtained for Test Example 3;

[0043] Figure 7 This is the SEM image of the zinc negative electrode obtained in Comparative Example 1;

[0044] Figure 8 This is a SEM image of the zinc layer deposited on the zinc negative electrode obtained in Comparative Example 1 for 5 minutes;

[0045] Fig. 9 This is a SEM image of the zinc layer deposited on the zinc negative electrode obtained in Comparative Example 1 for 10 minutes;

[0046] Fig.10 This is a SEM image of the zinc negative electrode obtained in Example 1;

[0047] Fig.11 This is a SEM image of the zinc layer deposited on the zinc negative electrode obtained in Example 1 for 5 minutes;

[0048] Fig.12 This is the SEM image of the zinc layer deposited on the zinc negative electrode obtained in Example 1 for 10 minutes. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0050] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.

[0051] A first aspect of the present invention provides a zinc negative electrode, comprising a zinc foil and a monomolecular layer self-assembled on the surface of the zinc foil;

[0052] Wherein, the material of the monomolecular layer is a thiol compound containing a benzene ring.

[0053] The zinc negative electrode provided by the present invention self-assembles a monomolecular layer on the zinc foil, and the mercapto group in the mercapto compound containing a benzene ring reacts with the zinc foil to generate a Zn-S bond and stably exists on the surface of the zinc foil. At the same time, it has a metal-philic tail group -SH, which guides the zinc ions in the electrochemical reaction to uniformly deposit and nucleate, isolates water molecules, and thus effectively inhibits the growth of dendrites. In addition, the mercapto compound containing a benzene ring has good ionic conductivity, effectively inhibits the problem of high interface resistance of the coating, and ensures good ionic conductivity between the zinc negative electrode and the electrolyte.

[0054] Specifically, the zinc negative electrode structure provided by the present invention has the following technical effects:

[0055] 1. Improve battery stability: The introduction of the monolayer reduces the uneven dissolution and deposition of the zinc negative electrode during the electrochemical reaction, thereby extending the service life of the battery.

[0056] 2. Improve battery cycle efficiency: Thiol compounds containing benzene rings as the material of the monolayer can provide better electron and ion transmission channels, promote the uniform deposition and dissolution of zinc ions, and thus improve the battery's charge and discharge efficiency.

[0057] 3. Enhance electrode surface protection: The monomolecular layer acts as a protective layer to prevent the zinc negative electrode from being directly exposed to the electrolyte, reducing the occurrence of side reactions such as hydrogen generation and excessive dissolution of zinc.

[0058] 4. Improve battery safety: By controlling the formation of zinc deposition layer in electrochemical reaction, the growth of dendrites can be reduced, the risk of battery short circuit can be reduced, and thus the safety performance of the battery can be improved.

[0059] 5. Optimize the electrode interface: The use of a monolayer can improve the interfacial compatibility between the zinc negative electrode and the electrolyte, reduce the interfacial resistance, and improve the overall performance of the battery.

[0060] Monolayer as zinc negative electrode coating can effectively avoid some disadvantages of traditional coatings, as follows:

[0061] 1. Uniformity: The monolayer can form a highly ordered and uniform monolayer structure on the zinc surface through the self-assembly process, avoiding the problem of uneven coating.

[0062] 2. Excellent adhesion: The monolayer is firmly attached to the zinc surface through chemical bonds or physical adsorption, providing strong adhesion and avoiding the problem of easy falling off of traditional coatings.

[0063] 3. Low interface resistance: The thickness of the monolayer is only a few nanometers, which does not significantly increase the interface resistance, ensuring good ion conductivity between the zinc negative electrode and the electrolyte.

[0064] 4. Chemical stability.

[0065] 5. Monolayer materials can improve the chemical stability of zinc negative electrode in electrochemical environment and reduce degradation and failure.

[0066] 6. Simplify the process and cost: The self-assembly process of the monolayer is usually simple and easy to control, which reduces the complexity and cost of the manufacturing process. Through these advantages, the monolayer as a zinc negative electrode coating performs well in inhibiting dendrite growth, reducing side reactions, and improving battery performance and cycle life, effectively overcoming many shortcomings of traditional coatings.

[0067] The benzene ring-containing mercapto compound is a compound having a mercapto group and a benzene ring.

[0068] Furthermore, the benzene ring-containing mercapto compound includes at least one of mercaptan, thiophenol and thiocarboxylic acid.

[0069] Preferably, the thiol comprises 1,4-phenyldithiol.

[0070] Preferably, the thiophenol includes at least one of thiophenol, 4-hydroxythiophenol and 4-mercaptothiophenol.

[0071] Preferably, the thiocarboxylic acid comprises 4-mercaptobenzoic acid.

[0072] The second aspect of the present invention provides a method for preparing the zinc negative electrode according to the first aspect, comprising the following steps:

[0073] The zinc foil is immersed in a thiol compound solution, and the thiol compound self-assembles on the surface of the zinc foil to obtain the zinc negative electrode.

[0074] The preparation method of the zinc negative electrode provided by the present invention forms a monolayer on the surface of the zinc foil by impregnation and self-assembly, without the need for complex equipment or high-energy-consuming processes, making the preparation process simple and convenient. The self-assembly of the mercapto compound containing a benzene ring on the surface of the zinc foil can form a uniform and closely arranged monolayer, which helps the uniform growth of the zinc deposition layer in the electrochemical reaction, thereby improving the performance of the battery. The preparation method has good repeatability and improves the consistency and reliability of the zinc negative electrode.

[0075] Furthermore, the concentration of the thiol compound solution containing a benzene ring is 0.01M to 0.1M.

[0076] When the concentration of the thiol compound solution containing a benzene ring is lower than 0.01 M, the thiol loading amount will be insufficient; when the concentration of the thiol compound solution containing a benzene ring is higher than 0.1 M, it exceeds the solubility and affects the uniform distribution of the thiol.

[0077] Typically but not limiting, the concentration of the solution of the thiol compound containing a benzene ring may be, for example, 0.01M, 0.05M, 0.1M, or any value within the range of 0.01M to 0.1M.

[0078] Preferably, the immersion time is 12 h to 48 h.

[0079] If the immersion time is less than 12 hours, the thiol loading will be insufficient and the modification effect will be affected; if the immersion time exceeds 48 hours, the production efficiency and output will be reduced and the production cost will be increased.

[0080] Typically but not limiting, the immersion time may be, for example, 12 h, 16 h, 20 h, 24 h, 28 h, 32 h, 36 h, 40 h, 44 h or 48 h, or any value within the range of 12 h to 48 h.

[0081] Furthermore, the preparation method further comprises pre-treating the zinc foil before impregnation;

[0082] The pretreatment includes grinding, cleaning and drying of the zinc foil.

[0083] Furthermore, sandpaper is used for the polishing.

[0084] Polishing can remove the oxide layer on the surface of zinc foil and expose the fresh metal surface. The freshly exposed zinc surface has higher surface energy and reactivity, which helps the self-assembled molecules to combine more stably and evenly. The polished surface can provide a more stable chemical bonding environment and enhance the interaction between the self-assembled molecules and the metal surface. The flat and fresh zinc surface helps the self-assembled molecules to arrange in order, improving the density and protection effect of the film layer.

[0085] Preferably, the roughness of the sandpaper is 800-2000 meshes.

[0086] Furthermore, the cleaning includes cleaning with an organic solvent and rinsing with deionized water in this order.

[0087] Organic solvent cleaning removes sandpaper material residues and other impurities on the surface of the zinc foil.

[0088] Preferably, the organic solvent comprises acetone and / or alcohol.

[0089] Preferably, the organic solvent cleaning method is ultrasonic cleaning.

[0090] Preferably, the ultrasonic cleaning time is 10 min to 20 min.

[0091] Typically but not limiting, the ultrasonic cleaning time may be, for example, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min or 20 min, or any value within the range of 10 min to 20 min.

[0092] Preferably, the deionized water is rinsed 2 to 5 times.

[0093] Typically but not limiting, the number of times of rinsing with deionized water may be, for example, 2 times, 3 times, 4 times or 5 times, or any value within the range of 2 to 5 times.

[0094] Furthermore, the drying process is carried out under nitrogen protection.

[0095] The third aspect of the present invention provides a zinc-air battery, comprising a positive electrode, a negative electrode and an electrolyte;

[0096] Wherein, the negative electrode is the zinc negative electrode described in the first aspect.

[0097] The zinc-air battery provided by the present invention, in view of the advantages brought by the above-mentioned zinc negative electrode, makes the prepared zinc-air battery have better stability, efficiency and safety, expands the application field of zinc-air battery, and expands the development of downstream industries.

[0098] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0099] Example 1

[0100] This embodiment provides a zinc negative electrode, and the specific preparation method is as follows:

[0101] 1. Polish the surface of a commercial zinc foil of size 1.5 cm × 1.5 cm with 1500 grit sandpaper, then clean the surface with acetone and alcohol ultrasonic for 15 min in turn to remove the sandpaper material residue on the surface and other impurities on the zinc foil, then rinse it with deionized water three times, blow dry it under nitrogen, and store it under vacuum as a substrate material for the subsequent in situ growth of a thiol monolayer.

[0102] 2. The pretreated zinc sheet was immersed in a 0.05 M 1,4-phenyldithiol ethanol solution for 36 h to obtain a zinc negative electrode.

[0103] Example 2

[0104] This embodiment provides a zinc negative electrode. The difference from Embodiment 1 is that 4-mercaptobenzenethiol is used to replace 1,4-phenyldithiol. The other methods and steps are the same as those in Embodiment 1 and will not be repeated here.

[0105] Example 3

[0106] This embodiment provides a zinc negative electrode. The difference from Embodiment 1 is that 4-mercaptobenzoic acid is used to replace 1,4-phenyldithiol. The other methods and steps are the same as those in Embodiment 1 and will not be repeated here.

[0107] Example 4

[0108] This embodiment provides a zinc negative electrode. The difference from Embodiment 1 is that the concentration of the ethanol solution of 1,4-phenyldithiol is 0.01 M. The other methods and steps are the same as those in Embodiment 1 and will not be described again.

[0109] Example 5

[0110] This embodiment provides a zinc negative electrode. The difference from Embodiment 1 is that the concentration of the ethanol solution of 1,4-phenyldithiol is 0.1 M. The other methods and steps are the same as those in Embodiment 1 and will not be described again.

[0111] Example 6

[0112] This embodiment provides a zinc negative electrode. The difference from Embodiment 1 is that the concentration of the ethanol solution of 1,4-phenyldithiol is 1 M. The other methods and steps are the same as those in Embodiment 1 and will not be described again.

[0113] Comparative Example 1

[0114] This comparative example provides a zinc negative electrode, and the preparation method is as follows:

[0115] The surface of a commercial zinc foil with a size of 1.5 cm×1.5 cm was polished with 1500 mesh sandpaper, and then the surface was cleaned with acetone and alcohol ultrasonically for 15 minutes to remove the sandpaper material residue on the surface and other impurities on the zinc sheet. After rinsing with deionized water three times, it was blown dry under nitrogen to obtain the zinc negative electrode.

[0116] Test Example 1

[0117] The commercial zinc foil, zinc negative electrode and 1,4-phenyldithiol in Example 1 were characterized by Fourier transform infrared spectroscopy. The obtained Fourier transform infrared spectroscopy characterization image is shown in the figure below. Figure 1 shown.

[0118] from Figure 1 From the gray area, we can see that the characteristic peak of 1,4-phenyldithiol appears on the self-assembled monolayer zinc foil compared with the commercial zinc foil, which proves that the zinc foil is loaded with thiol molecules.

[0119] Test Example 2

[0120] The SEM images of the commercial zinc foil and zinc negative electrode in Example 1 immersed in 6M KOH solution for 1 day are shown in the following figure. Figure 2 to Figure 5 shown.

[0121] Figure 2 and Figure 3 This is the SEM image of the zinc negative electrode obtained in Example 1. Figure 4 and Figure 5 This is a SEM image of a commercial zinc foil. It can be seen that the zinc negative electrode obtained in Example 1 is smoother and has a smaller dendrite size than the commercial zinc foil after immersion.

[0122] Test Example 3

[0123] The zinc negative electrode obtained in Comparative Example 1, Example 1, Example 4 and Example 5 was tested for Tafel curves. Hg / HgO was used as the reference electrode, platinum sheet was used as the counter electrode, the zinc negative electrode obtained in Comparative Example 1, Example 1, Example 4 and Example 5 was used as the working electrode, and the electrolyte was 6M KOH and 0.2MZn(Ac)2. The Tafel curve was tested in a three-electrode system. The results are as follows: Figure 6 shown.

[0124] from Figure 6 It can be seen that the corrosion potentials all become positive, and the potential change is the largest when the preparation condition of immersion for 36 hours at a concentration of 0.05 M is selected, which can effectively inhibit hydrogen evolution. At the same time, it can be proved that the mercapto monolayer on the zinc foil can effectively inhibit side reactions such as corrosion and hydrogen evolution.

[0125] Test Example 4

[0126] The zinc negative electrode obtained in Example 1 and Comparative Example 1 was subjected to scanning electron microscopy, and the obtained SEM images are as follows Figure 7 and Fig.10 shown.

[0127] Hg / HgO was used as the reference electrode, the zinc sheet was used as the counter electrode, the zinc negative electrode obtained in Example 1 and Comparative Example 1 was used as the working electrode, and the electrolyte was a mixed solution of 6M KOH and 0.2M Zn(Ac)2. Under the above three-electrode system, the current was 5 mA / cm 2 The zinc negative electrode after deposition was obtained by constant current deposition at a current density of 5000 nm for 5 minutes. The zinc negative electrode after deposition for 5 minutes was subjected to scanning electron microscopy and the obtained SEM image is as follows: Figure 8 and Fig.11 shown.

[0128] According to the above deposition method and deposition parameters, the zinc negative electrode obtained in Example 1 and Comparative Example 1 was deposited at a constant current for 10 minutes to obtain a deposited zinc negative electrode. The zinc negative electrode after deposition for 10 minutes was subjected to a scanning electron microscope and the obtained SEM image is as follows: Fig. 9 and Fig.12 As shown. From the deposition SEM images at the same time, it can be seen that the deposited layer of the zinc negative electrode of Example 1 has a uniform morphology, and the uneven distribution of Zn nucleation sites in Comparative Example 1 leads to a stronger tendency of Zn electrodeposition in local areas. When the electrodeposition time increases, it leads to obvious protrusion.

[0129] Experimental Example 1

[0130] The zinc negative electrodes provided in Examples 1 to 6 and Comparative Example 1 were tested for electrical performance.

[0131] 1. Preparation of zinc-air battery: The zinc negative electrode provided in Examples 1 to 6 and Comparative Example 1 is used as the negative electrode, and is assembled into a customized zinc-air battery mold in the order of mold shell, tin sheet, zinc, gasket, electrolyte cavity, gasket, positive electrode sheet, and mold shell.

[0132] The positive electrode preparation process of zinc air is as follows: RuO2 and Pt / C (Pt content is 40wt%) are mixed in a ratio of 20mg:10mg, and then 150μL of Nafion (10wt%) and 4mL of ethanol are added to mix, and then ultrasonicated for 30min to obtain a slurry. The slurry is sprayed onto a composite catalyst carrier formed by rolling a nickel mesh, a waterproof breathable membrane, and carbon paper with a spray gun, and the loading amount is: 2mg / cm 2 .

[0133] The electrolyte was a mixed solution of 12 mL of 6 M KOH and 0.2 M Zn(Ac)2.

[0134] 2. Electrical performance test

[0135] At 5mA / cm 2 The cycle curves under the cycle conditions of 10min charge and discharge are shown in Table 1 below.

[0136] Table 1

[0137] Failure time / h Example 1 432 Example 2 380 Example 3 400 Example 4 360 Example 5 380 Example 6 350 Comparative Example 1 286

[0138] As can be seen from Table 1, the battery with the negative electrode provided in Comparative Example 1 began to increase its charge and discharge voltage range after 200h, and the discharge voltage decayed significantly, and failed at 286h due to exceeding the cut-off voltage (2.5V). The battery prepared with the negative electrode provided in the example still had a relatively stable charge and discharge voltage platform up to 400h.

[0139] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A zinc negative electrode, characterized in that including a zinc foil and a monomolecular layer self-assembled on the surface of the zinc foil; Wherein, the material of the monomolecular layer is a thiol compound containing a benzene ring.

2. The zinc negative electrode according to claim 1, characterized in that The thiol compound containing a benzene ring includes at least one of thiol, thiol and thiocarboxylic acid; Preferably, the thiol comprises 1,4-phenyldithiol; Preferably, the thiophenol includes at least one of thiophenol, 4-hydroxythiophenol and 4-mercaptothiophenol; Preferably, the thiocarboxylic acid comprises 4-mercaptobenzoic acid.

3. A method for preparing a zinc negative electrode according to claim 1 or 2, characterized in that: The following steps are involved: The zinc foil is immersed in a solution of a thiol compound containing a benzene ring, and the thiol compound containing a benzene ring is self-assembled on the surface of the zinc foil to obtain the zinc negative electrode.

4. The preparation method according to claim 3, characterized in that The concentration of the thiol compound solution containing a benzene ring is 0.01M to 0.1M; Preferably, the immersion time is 12 hours to 48 hours.

5. The preparation method according to claim 3 or 4, characterized in that It also includes the pre-treatment of the zinc foil before dipping; The pretreatment includes grinding, cleaning and drying of the zinc foil.

6. The preparation method according to claim 5, characterized in that Perform the sanding using sandpaper; Preferably, the roughness of the sandpaper is 800-2000 mesh.

7. The preparation method according to claim 5, characterized in that The cleaning comprises organic solvent cleaning and deionized water rinsing in this order; Preferably, the organic solvent comprises acetone and / or alcohol; Preferably, the organic solvent cleaning method is ultrasonic cleaning; Preferably, the ultrasonic cleaning time is 10 min to 20 min; Preferably, the deionized water rinse is performed 2 to 5 times.

8. The preparation method according to claim 5, characterized in that The drying process was carried out under nitrogen protection.

9. A zinc-air battery, characterized in that including positive electrode, negative electrode and electrolyte; Wherein, the negative electrode is the zinc negative electrode according to claim 1 or 2.

Citation Information

Patent Citations

  • Modified zinc negative electrode and preparation method and application thereof

    CN113410452A

  • Method for modifying negative electrode of aqueous zinc ion battery

    CN114512630A

  • Preparation and application of zinc metal negative electrode integrated by coordination supramolecular grid material

    CN114725324A

  • Preparation method and application of aqueous zinc ion battery electrolyte containing organic sulfide additive

    CN117673521A

  • Self-assembled monomolecular film composite zinc electrode, preparation method thereof and aqueous zinc ion battery

    CN117832373A

Cited By

  • Preparation method of zinc negative electrode of hydrophobic and zinc-loving sulfydryl functionalized zinc ion energy storage device

    CN119447155A