Titanium-doped high-nickel layered oxide positive electrode material fluorine-doped mesoporous titanium dioxide and preparation method thereof
Through the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, the structural evolution and interface side reaction problems of high-nickel layered oxide at high voltage are solved, and high-voltage stability and cycle life are achieved. Improved, suitable for high energy density applications of lithium-ion batteries.
Patent Information
- Application Number
- CN202411065885.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The high-nickel layered oxide positive electrode material has structural evolution and electrode/electrolyte interface side reactions at high voltages, limiting the energy density improvement and cycling stability of lithium-ion batteries.
Using titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, the surface of the Ti element is coated by bulk doping and fluorine-doping mesoporous titanium dioxide, forming a protective film to stabilize the crystal structure and suppress the side. reaction.
It significantly improves the high-voltage working stability of high-nickel ternary layered oxide materials, extends the cycle life, and maintains a capacity of more than 80% at a voltage above 4.5V, reduces the preparation cost, and is suitable for large-scale production.
Smart Images

Figure CN118983434A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion battery positive electrode materials, and relates to a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide and a preparation method thereof. Background Art
[0002] In order to meet the challenges brought by global climate change, it is necessary to reduce carbon emissions, which has promoted the transformation of the energy structure dominated by fossil energy and promoted the development of new clean energy. Lithium-ion batteries have the advantages of high energy density, long cycle life and wide operating temperature range. They have become a feasible way to generate new clean energy and an important carrier for the development of new energy vehicles. In the entire lithium-ion battery system, the disadvantage of low mass-to-capacity of the positive electrode material has always been an important factor limiting the improvement of the energy density of lithium-ion batteries. High nickel layered oxide positive electrode material LiNi x Co y Mn 1-x-y O2 has high reversible specific capacity and high working voltage (3.8V vs Li / Li + ), is considered to be the most promising high-energy-density electrode material. In order to meet the growing demand for high energy density of lithium-ion batteries, it is very necessary to further increase the charge cutoff voltage to 4.5V. However, high-nickel layered oxide cathode materials still face structural evolution during long cycles and electrode / electrolyte interface side reactions at high voltages, which limits their practical applications.
[0003] In order to make high-nickel layered oxide cathode materials have excellent cycle stability at high charge cut-off voltage, domestic and foreign scholars have done a lot of work, such as gradient microstructure design, doping modification and surface coating modification. Doping can stabilize the crystal structure, but it cannot avoid the chemical reaction between the surface and the electrode liquid. Surface coating treatment can improve the interface between the electrolyte and high-nickel layered oxide cathode materials, inhibit the generation of interface side reactions, and achieve the purpose of improving the cycle stability at high charge cut-off voltage.
[0004] Patent CN 113809329 A reports a method for surface coating modification of high-nickel positive electrode materials. The coating layer is selected from at least one of Li2ZrO3, Li4ZrO4, Li6Zr2O7 and Li8ZrO6, which optimizes the structural stability of the prepared positive electrode material and improves the cycle stability of the material under high cut-off voltage. However, the preparation process of this invention is complicated. It is necessary to first synthesize a zirconium precursor (UiO-66), and then blend it with a high-nickel layered material precursor powder and sinter it. Patent CN 114171733B reports a coated lithium-ion battery positive electrode material and its preparation method. The coating layer includes Li4Ti5O 12, TiO2 and Ti4O7, deposited on the surface of high nickel layered oxide through deposition source, and the coordination between the three substances in the coating layer is used to improve the electronic conductivity and ionic conductivity of the positive electrode material of lithium ion battery, thereby improving the specific capacity and rate performance of the positive electrode material of lithium ion battery, and extending its cycle life. However, the preparation conditions of this process are harsh and need to be in a high vacuum environment. Patent CN 111342012 B discloses a preparation method of mesoporous spherical titanium dioxide coated ternary high nickel material. The coating of the mesoporous layer is conducive to the penetration of the electrode liquid without direct contact with the ternary high nickel material, shortening the transmission distance of lithium ions and improving its electrochemical performance. However, its electrochemical performance at high cut-off voltage is not reported. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention proposes a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide and a preparation method, which realizes the surface coating of the high-nickel layered oxide by fluorine-doped mesoporous TiO2, and at the same time realizes the bulk doping of the high-nickel layered oxide by Ti element. With the help of surface coating and doping modification, the electrochemical stability of the positive electrode material under high voltage is greatly improved.
[0006] The present invention is achieved through the following technical solutions:
[0007] A titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, comprising a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped high-nickel layered oxide, the high-nickel layered oxide is LiNi x Co y Mn 1-x-y O2, the coating layer is fluorine-doped mesoporous titanium dioxide.
[0008] Preferably, the average particle size of the inner core is 1.5 to 5 μm, wherein 0.5≤x<1, 0≤y≤0.2.
[0009] A method for preparing any of the above-mentioned titanium-doped high-nickel layered oxide positive electrode materials @ fluorine-doped mesoporous titanium dioxide comprises the following steps:
[0010] Step 1, grinding the high nickel layered oxide powder with tetrabutyl titanate, polyethyleneimine and acetic acid, wherein the mass ratio of the high nickel layered oxide powder to tetrabutyl titanate is 1:(0.002-0.02), to obtain a gel-like mixed system;
[0011] Step 2, calcining the mixed system at 300-600° C. to obtain titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide powder;
[0012] Step 3, mixing the powder and ammonium fluoride uniformly at a molar ratio of 1: (0.01-0.04) to obtain a mixture, and calcining the mixture at 300-600° C. to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide.
[0013] Preferably, in step 1, the mass ratio of high nickel layered oxide powder to polyethyleneimine and acetic acid is 1:(0.001-0.02):(0.1-0.4).
[0014] Preferably, in step 1, the high-nickel layered oxide powder is ground with tetrabutyl titanate, polyethyleneimine and acetic acid for 20 to 30 minutes to obtain a gel-like mixed system.
[0015] Preferably, in step 2, the temperature of the mixed system is raised from room temperature to 300-600° C. at a heating rate of 2-10° C. / min.
[0016] Preferably, in step 2, the mixed system is calcined at 300-600° C. for 2-10 hours to obtain titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide powder.
[0017] Preferably, in step 3, the powder and ammonium fluoride are first dispersed in ethanol or deionized water, and then stirred under heating until the ethanol or deionized water is completely volatilized to obtain a mixture.
[0018] Preferably, in step 3, the mixture is heated from room temperature to 300-600° C. at a heating rate of 2-10° C. / min.
[0019] Preferably, in step 3, the mixture is calcined at 300-600° C. for 2-10 hours to obtain titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide.
[0020] Compared with the prior art, the present invention has the following beneficial technical effects:
[0021] The present invention discloses a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, by x Co y Mn 1-x-y O2 Bulk Doping Ti 4+ The two modification methods of surface coating with fluorine-doped mesoporous titanium dioxide can not only stabilize the crystal structure of the positive electrode material, but also effectively reduce the mixing of lithium and nickel, thereby inhibiting the irreversible phase change of the positive electrode material at high voltage; fluorine-doped mesoporous titanium dioxide can be doped with Ti in the bulk phase. 4+ LiNi x Co y Mn 1-x-yA protective film is formed on the surface of O2, which can provide a physical barrier, inhibit the occurrence of side reactions, and effectively avoid the decomposition of the electrolyte under high voltage to the active material LiNi x Co y Mn 1-x-y O2 causes chemical corrosion on the surface, reduces the dissolution of transition metals, and has a certain electronic conductivity, which greatly improves the high-voltage working stability of high-nickel ternary layered oxide materials and inhibits the continuous increase of the interface impedance between high-nickel ternary layered oxide materials and electrolytes. The coating layer formed by fluorine-doped mesoporous titanium dioxide improves the conductivity and stability of the material, thereby improving the specific capacity of the material and extending the cycle life of the material. Bulk doping of titanium elements can stabilize the lattice structure, increase the transmission channel of lithium ions, and improve the ionic conductivity of lithium ions. The coated doped modified lithium ion battery positive electrode material obtained by the present invention can be charged at a high voltage exceeding 4.5V, and the capacity retention rate of 200 cycles at a high voltage of 2.7 to 4.5V is as high as 80% or more, which has broad market prospects.
[0022] The invention discloses a method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide. The method adopts a grinding method to coat the precursor of the mesoporous titanium dioxide on the surface of the high-nickel layered oxide positive electrode material powder, thereby saving the time of pretreatment, improving the preparation efficiency, and facilitating the subsequent calcination at 300-600° C., which can not only ensure the formation of a uniform mesoporous titanium dioxide coating layer, but also ensure that the protective film formed by the mesoporous titanium dioxide does not affect the good structure of the high-nickel layered oxide positive electrode material after being coated on the surface of the positive electrode material, and realize the Ti 4+ When the calcination temperature is lower than 300°C, the calcination temperature is too low to form a stable titanium dioxide crystal phase. When the calcination temperature is higher than 600°C, the titanium dioxide particles grow and agglomerate seriously due to the high temperature, which hinders the diffusion of lithium ions and further aggravates the lithium-nickel mixed arrangement phenomenon. Finally, ammonium fluoride is calcined at 300-600°C to achieve fluorine doping in mesoporous titanium dioxide. The present invention has low equipment requirements, no special conditions, is simple and easy to control, can be mass-produced, greatly reduces costs, and the obtained modified material has good high-voltage working stability, which is conducive to the improvement of energy density. At the same time, it has a suitable charge and discharge voltage platform, can work under high voltage, exerts a higher capacity, has energy density advantages, and can be used in lithium-ion batteries. The composite positive electrode material obtained by the present invention, when used as a positive electrode material for a lithium ion battery, shows good cycle stability at a high charging cut-off voltage (2.7-4.5V), has better conductivity, specific capacity and longer cycle life, and provides a new approach and method for the coating modification of high-nickel layered oxide positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1This is a SEM image of the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide prepared in Example 3 of the present invention.
[0024] Figure 2 This is a constant current charge and discharge curve of the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide prepared in Example 3 of the present invention at a high voltage of 2.7-4.5V.
[0025] Figure 3 This is a SEM image of the titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide prepared in Comparative Example 1 of the present invention.
[0026] Figure 4 This is a constant current charge and discharge curve of the titanium-doped high-nickel layered oxide positive electrode material @mesoporous titanium dioxide prepared in Comparative Example 1 of the present invention at a high voltage of 2.7-4.5V.
[0027] Figure 5 The cycle-capacity diagram of the coated lithium-ion battery positive electrode material prepared in Example 3 of the present invention and Comparative Example 1 after a long cycle of 200 cycles at a high voltage of 2.7 to 4.5 V. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.
[0029] The present invention discloses a method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide (coated doped modified lithium ion battery positive electrode material), which specifically includes the following steps:
[0030] Step 1: Prepare high nickel layered oxide positive electrode material powder (chemical formula is LiNi x Co y Mn 1-x-y O2, wherein 0.5≤x<1, 0≤y≤0.2, 0<z≤0.3, x+y+z=1) is ground with tetrabutyl titanate, polyethyleneimine and acetic acid in a certain mass ratio for 20 to 30 minutes, and the specific mass ratio range is 1:(0.002~0.02):(0.001~0.02):(0.1~0.4) to form a gel-like mixed system, and the precursor of mesoporous titanium dioxide is coated on the surface of the high nickel layered oxide positive electrode material powder;
[0031] Step 2, placing the mixed system ground in step 1 into a muffle furnace, heating from room temperature to 300-600°C, controlling the rate at 2-10°C / min, and then calcining at 300-600°C for 2-10h to obtain a titanium-doped high-nickel layered oxide positive electrode material @mesoporous titanium dioxide.
[0032] Step 3, dispersing the powder obtained in step 2) and ammonium fluoride in ethanol or deionized water at a molar ratio of 1: (0.01-0.04), and continuously heating and stirring until the ethanol or deionized water is completely volatilized to achieve the purpose of mixing the two and obtain a mixture.
[0033] Step 4, placing the mixture obtained in step 3 into a muffle furnace, heating from room temperature to 300-600°C, controlling the rate to be 2-10°C / min, and then calcining at 300-600°C for 2-10h to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, which is a coated doped modified lithium-ion battery positive electrode material.
[0034] The modified lithium ion battery positive electrode material comprises a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped LiNi x Co y Mn 1-x-y O2 (wherein 0.5≤x<1, 0≤y≤0.2), the average particle size is 1.5~5μm; the coating layer is F-doped TiO2 (F-TiO2).
[0035] Example 1
[0036] A titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide as a positive electrode material for lithium-ion batteries, comprising a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), with an average particle size of 2.5 μm; the coating layer is F-doped TiO2 (F-TiO2).
[0037] The present invention discloses a method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide (i.e., a coated lithium-ion battery positive electrode material), which specifically comprises the following steps:
[0038] Step 1: Grind high nickel layered oxide positive electrode material powder NCM622 with tetrabutyl titanate, polyethyleneimine and acetic acid in a mass ratio of 1:0.002:0.004:0.1 using an agate mortar for 25 minutes to form a gel-like mixed system.
[0039] Step 2, placing the mixed system ground in step 1 into a muffle furnace, heating from room temperature to 300°C, controlling the rate at 10°C / min, and then calcining at 300°C for 2h to obtain a titanium-doped high-nickel layered oxide positive electrode material @mesoporous titanium dioxide.
[0040] Step 3, dispersing the powder obtained in step 2 and ammonium fluoride in 50 ml of ethanol at a molar ratio of 1:0.01, wherein the ammonium fluoride is 0.0002 mol, and continuing heating and stirring until the ethanol is completely volatilized to obtain a powder.
[0041] Step 4, placing the mixture obtained in step 3 into a muffle furnace, heating from room temperature to 300°C, controlling the rate to be 10°C / min, and then calcining at 300°C for 2h to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, which is a coated lithium-ion battery positive electrode material.
[0042] The electrochemical performance test of the coated doped modified lithium ion battery positive electrode material obtained in this embodiment was carried out, wherein the lithium ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1 constituted the pole piece; the counter electrode was a lithium sheet, the diaphragm was a polypropylene microporous membrane Celgard2400, the electrolyte was a 1 mol / L LiPF6 aqueous solution, and EC, DEC and DMC were dissolved in a volume ratio of 1:1:1. A CR2032 button battery was prepared from the above-mentioned pole piece, counter electrode, diaphragm and electrolyte.
[0043] In this embodiment, the LAND battery test system is used to perform constant current charge and discharge tests on CR2032 button batteries. In the voltage window of 2.7-4.5V and the current density of 0.1C, the first cycle discharge capacity is 176mAh / g. At the current density of 1C, the capacity retention rate after 200 cycles is 75.28%.
[0044] Example 2
[0045] A titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide as a positive electrode material for lithium-ion batteries, comprising a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), with an average particle size of 5 μm; the coating layer is F-doped TiO2 (F-TiO2).
[0046] The present invention discloses a method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide (i.e., a coated lithium-ion battery positive electrode material), which specifically includes the following steps:
[0047] Step 1: Grind high nickel layered oxide positive electrode material powder NCM811 with tetrabutyl titanate, polyethyleneimine and acetic acid in a mass ratio of 1:0.02:0.04:0.4 using an agate mortar for 20 minutes to form a gel-like mixed system.
[0048] Step 2, putting the mixed system ground in step 1 into a muffle furnace, heating from room temperature to 600°C, controlling the rate at 5°C / min, and then calcining at 600°C for 10 hours to obtain a titanium-doped high-nickel layered oxide positive electrode material @mesoporous titanium dioxide.
[0049] Step 3, dispersing the powder obtained in step 2 and ammonium fluoride in 50 ml of ethanol at a molar ratio of 1:0.03, wherein the ammonium fluoride is 0.0006 mol, and continuing heating and stirring until the ethanol is completely volatilized to obtain a powder.
[0050] Step 4, placing the mixture obtained in step 3 into a muffle furnace, heating from room temperature to 600°C, controlling the rate to 5°C / min, and then calcining at 600°C for 10 hours to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, which is a coated lithium-ion battery positive electrode material.
[0051] The electrochemical performance test of the coated doped modified lithium ion battery positive electrode material obtained in this embodiment was carried out, wherein the lithium ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1 constituted the pole piece; the counter electrode was a lithium sheet, the diaphragm was a polypropylene microporous membrane Celgard2400, the electrolyte was a 1 mol / L LiPF6 aqueous solution, and EC, DEC and DMC were dissolved in a volume ratio of 1:1:1. A CR2032 button battery was prepared from the above-mentioned pole piece, counter electrode, diaphragm and electrolyte.
[0052] In this embodiment, the LAND battery test system is used to perform constant current charge and discharge tests on CR2032 button batteries. In the voltage window of 2.7-4.5V and the current density of 0.1C, the first cycle discharge capacity is 203mAh / g. At the current density of 1C, the capacity retention rate after 200 cycles is 78.75%.
[0053] Example 3
[0054] A titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide as a positive electrode material for lithium-ion batteries, comprising a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), with an average particle size of 1.5 μm; the coating layer is F-doped TiO2 (F-TiO2).
[0055] The present invention discloses a method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide (i.e., a coated lithium-ion battery positive electrode material), which specifically includes the following steps:
[0056] Step 1: Grind high nickel layered oxide positive electrode material powder NCM523 with tetrabutyl titanate, polyethyleneimine and acetic acid in a mass ratio of 1:0.005:0.001:0.2 using an agate mortar for 30 minutes to form a gel-like mixed system.
[0057] Step 2, placing the mixed system ground in step 1 into a muffle furnace, heating from room temperature to 450°C, controlling the rate at 2°C / min, and then calcining at 450°C for 3 hours to obtain a titanium-doped high-nickel layered oxide positive electrode material @mesoporous titanium dioxide.
[0058] Step 3, dispersing the powder obtained in step 2 and ammonium fluoride in 50 ml of ethanol at a molar ratio of 1:0.04, wherein the ammonium fluoride is 0.0008 mol, and continuing heating and stirring until the ethanol is completely volatilized to obtain a powder.
[0059] Step 4, placing the mixture obtained in step 3 into a muffle furnace, heating from room temperature to 450°C, controlling the rate to be 2°C / min, and then calcining at 450°C for 3h to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, which is a coated lithium-ion battery positive electrode material.
[0060] The titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide obtained in this example was scanned by electron microscope. Figure 1 As shown. Figure 1 It can be seen that the high nickel layered oxide positive electrode material NCM523 still maintains a good polygonal structure, Ti4 + Bulk doping and F-doped TiO2 coating have no effect on the crystal structure of NCM523.
[0061] The electrochemical performance test of the coated doped modified lithium ion battery positive electrode material obtained in this embodiment was carried out, wherein the lithium ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1 constituted the pole piece; the counter electrode was a lithium sheet, the diaphragm was a polypropylene microporous membrane Celgard2400, the electrolyte was a 1 mol / L LiPF6 aqueous solution, and EC, DEC and DMC were dissolved in a volume ratio of 1:1:1. A CR2032 button battery was prepared from the above-mentioned pole piece, counter electrode, diaphragm and electrolyte.
[0062] This embodiment uses the LAND battery test system to perform constant current charge and discharge tests on CR2032 button batteries. The results are as follows: Figure 2 and Figure 5 As shown, in the voltage window of 2.7 to 4.5 V and the current density of 0.1 C, Figure 2 As shown, the first cycle discharge capacity is 189 mAh / g, at a current density of 1C. Figure 5As shown, the capacity retention rate after 200 cycles increased from the original 46.4% of NCM523 to 93.16%.
[0063] Comparative Example 1
[0064] A titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide as a positive electrode material for lithium-ion batteries, comprising a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), average particle size is 1.5μm; coating layer is TiO2.
[0065] A method for preparing a titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide (i.e., a coated lithium-ion battery positive electrode material) specifically includes the following steps:
[0066] Step 1: Grind high nickel layered oxide positive electrode material powder NCM523 with tetrabutyl titanate, polyethyleneimine and acetic acid in a mass ratio of 1:0.005:0.001:0.2 using an agate mortar for 30 minutes to form a gel-like mixed system.
[0067] Step 2: Place the mixed system ground in step 1 into a muffle furnace, heat from room temperature to 450° C. at a rate of 2° C. / min, and then calcine at 450° C. for 3 h.
[0068] The titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide obtained in Comparative Example 1 was scanned by electron microscope. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that the high nickel layered oxide positive electrode material NCM523 still maintains a good polygonal structure, Ti4 + Bulk doping and TiO2 coating have no effect on the crystal structure of NCM523.
[0069] The electrochemical performance test of the coated lithium-ion battery positive electrode material obtained in Comparative Example 1 was carried out, wherein the lithium-ion battery positive electrode material, super-p and PVDF in a mass ratio of 8:1:1 constituted the pole piece; the counter electrode was a lithium sheet, the diaphragm was a polypropylene microporous membrane Celgard2400, the electrolyte was a 1 mol / L LiPF6 aqueous solution, and EC, DEC and DMC were dissolved in a volume ratio of 1:1:1. A CR2032 button battery was prepared from the above-mentioned pole piece, counter electrode, diaphragm and electrolyte.
[0070] Comparative Example 1: The LAND battery test system was used to perform constant current charge and discharge tests on CR2032 button batteries. The results were as follows: Figure 4 and Figure 5As shown, in the voltage window of 2.7 to 4.5 V and the current density of 0.1 C, Figure 4 As shown, the first cycle discharge capacity is 181mAh / g, at a current density of 1C. Figure 5 As shown, the capacity retention rate after 200 cycles is 80.69%.
[0071] By comparing the experimental results of Example 3 and Comparative Example 1, a conclusion can be drawn that: compared with the modified material coated with pure mesoporous TiO2, the modified material doped with F element introduced into the mesoporous TiO2 coating layer not only has a higher capacity, but also has a higher capacity retention rate after 200 cycles.
[0072] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide, characterized in that: It includes a core and a coating layer covering the core, wherein the core is Ti 4+ Bulk-doped high-nickel layered oxide, the high-nickel layered oxide is LiNi x Co y Mn 1-x-y O2, the coating layer is fluorine-doped mesoporous titanium dioxide.
2. The titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 1, characterized in that: The average particle size of the inner core is 1.5 to 5 μm, wherein 0.5≤x<1, 0≤y≤0.
2.
3. A method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1, grinding the high nickel layered oxide powder with tetrabutyl titanate, polyethyleneimine and acetic acid, wherein the mass ratio of the high nickel layered oxide powder to tetrabutyl titanate is 1:(0.002-0.02), to obtain a gel-like mixed system; Step 2, calcining the mixed system at 300-600° C. to obtain titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide powder; Step 3, mixing the powder and ammonium fluoride uniformly at a molar ratio of 1: (0.01-0.04) to obtain a mixture, and calcining the mixture at 300-600° C. to obtain a titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide.
4. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: In step 1, the mass ratio of high nickel layered oxide powder to polyethyleneimine and acetic acid is 1:(0.001-0.02):(0.1-0.4).
5. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 1: Grind the high-nickel layered oxide powder with tetrabutyl titanate, polyethyleneimine and acetic acid for 20 to 30 minutes to obtain a gel-like mixed system.
6. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 2: heating the mixed system from room temperature to 300-600° C. at a heating rate of 2-10° C. / min.
7. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 2: calcining the mixed system at 300-600° C. for 2-10 hours to obtain titanium-doped high-nickel layered oxide positive electrode material @ mesoporous titanium dioxide powder.
8. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 3: Disperse the powder and ammonium fluoride into ethanol or deionized water, and then stir them under heating until the ethanol or deionized water is completely volatilized to obtain a mixture.
9. The method for preparing the titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 3: heating the mixture from room temperature to 300-600° C. at a heating rate of 2-10° C. / min.
10. The method for preparing titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide according to claim 3, characterized in that: Step 3: calcining the mixture at 300-600° C. for 2-10 hours to obtain titanium-doped high-nickel layered oxide positive electrode material @ fluorine-doped mesoporous titanium dioxide.
Citation Information
Patent Citations
Surface doping and coating method for improving service life and high-temperature performance of lithium manganate-series lithium battery
CN106469810A
Mesoporous spherical titanium dioxide coated ternary material, preparation method thereof, lithium ion battery positive electrode and lithium ion battery
CN111342012A
Preparation method of titanium-doped high-nickel ternary lithium ion cathode material
CN111994967A
Mixed-phase titanium dioxide modified high-nickel ternary positive electrode material as well as preparation method and application thereof
CN112117451A
Hybrid membranes containing titanium dioxide doped with fluorine
US20130196251A1
Cited By
Titanium oxide and carbon composite coated positive electrode material and preparation method and application thereof
CN121172095A