Nickel-aluminum positive electrode material and preparation method and application thereof
By doping high-valent metal elements such as molybdenum and niobium into nickel-aluminum positive electrode materials, the problem of material structure and performance decay after cobalt is eliminated is solved, the mechanical stability and cyclic performance of nickel-aluminum positive electrode materials are improved, and the production cost is reduced. It realizes efficient application of lithium-ion batteries.
Patent Information
- Application Number
- CN202411167778.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the structure and performance of nickel-based layered oxide cathode material will be affected by elimination of cobalt, and nickel-rich cathode material has problems such as lithium-nickel mixed displacement, resulting in material performance deterioration and high production costs.
High-valent metal elements such as molybdenum and niobium doped nickel-aluminum positive electrode materials are prepared by mixing and sintering of nickel-aluminum precursor in the preparation method and lithium source and additives to prepare a dense nickel-aluminum positive electrode material to inhibit H2-H3 phase change Release oxygen to slow down structural degradation and avoid mixed discharge of lithium and nickel.
Improve the mechanical stability and cyclic performance of nickel-aluminum positive electrode material, enhance specific capacity, slow down the cracks and surface structure degradation of the positive electrode material, reduce production costs, avoid lithium-nickel mixed discharge, maintain the order of the material and Lithium ion migration efficiency.
Smart Images

Figure CN119050344A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of positive electrode material preparation, and specifically relates to a nickel-aluminum positive electrode material and a preparation method and application thereof. Background Art
[0002] Nickel-based layered oxides are considered to be one of the most promising cathode materials for lithium-ion batteries due to their high energy density. x Co y Mn 1-x-y O2(NCM) and LiNi x Co y Al 1-x-y O2 (NCA) cathode materials have been successfully used in electric vehicles. Studies have shown that the energy density of nickel-based hierarchical oxide cathodes is positively correlated with their nickel content. Adding cobalt to nickel-rich cathodes can maintain the order of the material structure and promote lithium ion migration. Eliminating cobalt from the material may further aggravate the decline of the material structure and performance; however, the production cost of nickel-based hierarchical oxide cathodes is limited by the supply of cobalt raw materials.
[0003] At present, the common strategy to increase energy density and reduce manufacturing costs at the same time is to increase the nickel content x in the material and reduce or even eliminate the use of cobalt. However, as the nickel content increases, the nickel-rich cathode will face similar problems as pure lithium nickel oxide, namely, severe lithium-nickel mixing, high difficulty in synthesizing pure phase materials, and poor structural and chemical stability. Therefore, it is necessary to develop a nickel-aluminum cathode material that eliminates cobalt while ensuring that the material structure and performance will not decline. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the problems in the prior art that the structure and performance of the material will be affected after the elimination of cobalt, and that the nickel-rich material has a mixed arrangement of lithium and nickel, thereby providing a nickel-aluminum positive electrode material and its preparation method and application.
[0005] To this end, the present invention provides the following technical solutions.
[0006] The present invention provides a nickel-aluminum positive electrode material, wherein the nickel-aluminum positive electrode material is a nickel-aluminum material doped with a high-valent metal element; the high-valent metal element includes at least one of molybdenum and niobium.
[0007] In an optional embodiment, based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material, the concentration of molybdenum in the nickel-aluminum positive electrode material is 0.1-1.0 mol%;
[0008] In an optional embodiment, based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material, the concentration of niobium in the nickel-aluminum positive electrode material is 0.1-1.0 mol%.
[0009] In an optional embodiment, the high-valent metal element includes niobium.
[0010] The present invention provides a method for preparing a nickel-aluminum positive electrode material, comprising the following steps:
[0011] (1) preparing a nickel aluminum precursor;
[0012] (2) mixing a nickel-aluminum precursor, a lithium source, and an additive, sintering after mixing evenly, to obtain a nickel-aluminum positive electrode material;
[0013] The additive is a compound containing a high-valent metal element; the high-valent metal element includes at least one of molybdenum and niobium.
[0014] In an optional embodiment, the ratio of the total molar amount of aluminum element and nickel element in the nickel-aluminum precursor to the molar amount of the high-valent metal element in the additive is 1:(0.0029-0.0093).
[0015] In an optional embodiment, the additive is a niobide;
[0016] In an optional embodiment, the ratio of the total molar amount of aluminum element and nickel element in the nickel-aluminum precursor to the molar amount of lithium element in the lithium source is 1:(1.0-1.4);
[0017] In an optional embodiment, the lithium source includes at least one of lithium carbonate, lithium oxalate, and lithium hydroxide;
[0018] In an optional embodiment, the niobide includes at least one of niobium pentoxide, niobium dioxide, and niobium trioxide;
[0019] In an optional embodiment, the molybdenum compound includes at least one of molybdenum dioxide and molybdenum disulfide;
[0020] In an optional embodiment, the particle size of the nickel aluminum precursor is 2.5-5 μm.
[0021] In an optional embodiment, the step (1) of preparing the nickel-aluminum precursor comprises: mixing a nickel source, an aluminum source and a portion of an alkaline solution to obtain a reaction solution, and continuously adding an alkaline solution to the reaction solution, reacting and drying to obtain a nickel-aluminum precursor;
[0022] The alkaline solution is added to the reaction solution in two parts. The amount of each part added is not specifically limited. The first added amount can dissolve the nickel source and the aluminum source, and the second added amount can ensure that the reaction system meets the ammonia value and pH value.
[0023] Preferably, the molar ratio of the nickel element in the nickel source to the aluminum element in the aluminum source is (19-24):1;
[0024] Preferably, the alkaline substance in the alkaline solution includes at least one of sodium hydroxide and ammonia;
[0025] Preferably, when carrying out the reaction, the pH value of the reaction system is 10-11, and the ammonia value is 4.0-6.0 g / L;
[0026] The amount of sodium hydroxide solution and ammonia water added in the present invention is not specifically limited, and the conventional amount in the art is used to ensure that the reaction system meets the ammonia value and pH value;
[0027] Preferably, the reaction temperature is 60-70°C, and the reaction time is 4-12h;
[0028] Preferably, the reaction is carried out under a protective gas atmosphere;
[0029] The protective gas includes inert gas and nitrogen;
[0030] Preferably, the drying temperature is 100-120°C;
[0031] Preferably, the nickel source includes at least one of nickel sulfate, nickel chloride, and nickel trioxide;
[0032] Preferably, the aluminum source includes at least one of aluminum oxide, aluminum hydroxide, sodium aluminate, aluminum chloride and aluminum sulfate.
[0033] In an optional embodiment, in the step (2), the sintering is carried out in an oxygen atmosphere with a volume concentration of 93-99%;
[0034] Preferably, the flow rate of the oxygen is 0.2-0.6 L / min;
[0035] Preferably, the sintering temperature is 680-720° C., and the sintering time is 8-12 hours.
[0036] The present invention provides a nickel-aluminum positive electrode material prepared by the above preparation method.
[0037] The present invention provides an application of the nickel-aluminum positive electrode material prepared by the above preparation method in a lithium ion battery.
[0038] The technical solution of the present invention has the following advantages:
[0039] 1. The nickel-aluminum positive electrode material provided by the present invention is a nickel-aluminum material doped with a high-valent metal element; the high-valent metal element includes at least one of molybdenum and niobium. The valence state of the high-valent metal element is higher than +4, which can make the microstructure of the nickel-aluminum positive electrode material dense and increase the mechanical stability; inhibit the H2-H3 phase transition, slow down the formation and expansion of the positive electrode material cracks; stabilize the lattice oxygen on the surface of the positive electrode material, slow down the oxygen release and the degradation of the surface structure of the positive electrode material, and help reduce the phenomenon of lithium-nickel mixing in nickel-rich materials. The battery made of the nickel-aluminum positive electrode material has good cycle performance and high specific capacity.
[0040] 2. The preparation method of the nickel-aluminum positive electrode material provided by the present invention comprises: (1) preparing a nickel-aluminum precursor; (2) mixing the nickel-aluminum precursor, a lithium source, and an additive, sintering after uniform mixing to obtain a nickel-aluminum positive electrode material; the additive is a compound containing a high-valent metal element; the high-valent metal element includes at least one of molybdenum and niobium. The nickel-aluminum positive electrode material prepared by the preparation method refines the size of the primary grains of the positive electrode material by doping with high-valent elements, making the microstructure of the nickel-aluminum positive electrode material more compact and increasing the mechanical stability of the nickel-aluminum positive electrode material; secondly, doping with high-valent elements can effectively inhibit the H2-H3 phase transition and slow down the formation and expansion of cracks in the positive electrode material; in addition, doping with high-valent elements can stabilize the lattice oxygen on the surface of the positive electrode material, slowing down the release of oxygen and the degradation of the surface structure of the positive electrode material. The present invention uses an aluminum source instead of a cobalt source, which has good cost-effectiveness. The battery made of the nickel-aluminum positive electrode material prepared in the present invention has higher cycle stability and rate performance, can maintain the orderliness of the material structure, promote lithium ion migration, and avoid the serious problems of lithium-nickel mixing and difficulty in synthesizing pure phase materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 This is an electron microscope image (50,000 times) of the nickel-aluminum positive electrode material prepared in Example 2 of the present invention;
[0043] Figure 2 This is an electron microscope image (10,000 times) of the nickel-aluminum positive electrode material prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0044] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0045] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0046] Example 1
[0047] This embodiment provides a method for preparing a nickel-aluminum positive electrode material, comprising the following steps:
[0048] (1) Nickel sulfate and aluminum chloride are mixed and dissolved with ammonia water and sodium hydroxide solution in a molar ratio of nickel element to aluminum element of 19:1 to obtain a reaction solution, wherein the total molar concentration of all metal ions in the reaction solution is 2 mol / L, the concentration of ammonia water is 5 mol / L, and the concentration of sodium hydroxide solution is 6 mol / L. The reaction solution flows into a 2.5L intermittent reaction container, and 5 mol / L ammonia water, 6 mol / L sodium hydroxide solution and deionized water are introduced into the reaction container at the same time, wherein the stirring speed of the system is controlled to be 600 rpm, the ammonia water is controlled to adjust the ammonia value of the reaction system to 6.0 g / L, and the sodium hydroxide solution is controlled to adjust the pH value of the reaction system to 10-11; the temperature is raised to 70°C under a nitrogen atmosphere for reaction for 6 hours, and the precursor powder is obtained after being rinsed with sodium hydroxide solution and deionized water, and the nickel-aluminum precursor is obtained after drying and sieving for demagnetization; wherein the drying temperature is 120°C. The particle size D50 of the nickel-aluminum precursor is 3-3.5 μm.
[0049] (2) Mixing a nickel-aluminum precursor, lithium carbonate, and molybdenum dioxide, wherein the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of lithium in the lithium source is 1:1.015, and the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of molybdenum in the molybdenum source is 1:0.009, mixing evenly with a high-speed mixer, sintering at 720° C. for 12 hours (atmosphere flow rate of 0.6 L / min) under an oxygen volume concentration of 99%, to obtain a nickel-aluminum positive electrode material. It was determined that the concentration of molybdenum in the nickel-aluminum positive electrode material was 0.7 mol%, based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material.
[0050] Example 2
[0051] This embodiment provides a method for preparing a nickel-aluminum positive electrode material, comprising the following steps:
[0052] (1) Nickel chloride and aluminum sulfate are mixed and dissolved with ammonia water and sodium hydroxide solution in a molar ratio of nickel element to aluminum element of 24:1 to obtain a reaction solution, wherein the total molar concentration of all metal ions in the reaction solution is 2 mol / L, the concentration of ammonia water is 6 mol / L, and the concentration of sodium hydroxide solution is 6 mol / L. The reaction solution is flowed into a 2.5L intermittent reaction container, and 6 mol / L ammonia water, 6 mol / L sodium hydroxide solution and deionized water are introduced into the reaction container at the same time, wherein the stirring speed of the system is controlled to be 500 rpm, the ammonia value of the reaction system is controlled to be 5.0 g / L by ammonia water, and the pH value of the reaction system is controlled to be 10-11 by sodium hydroxide solution; the temperature is raised to 65°C under a nitrogen atmosphere for reaction for 8 hours, and the precursor powder is obtained after being rinsed with sodium hydroxide solution and deionized water, and the nickel-aluminum precursor is obtained after being dried and sieved for demagnetization; wherein the drying temperature is 110°C. The particle size D50 of the nickel-aluminum precursor is 3.5-4 μm.
[0053] (2) Mixing a nickel-aluminum precursor, lithium oxalate, and niobium pentoxide, wherein the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of lithium in the lithium source is 1:1.2, and the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of niobium in the niobium source is 1:0.008, mixing them evenly with a high-speed mixer, sintering at 700° C. for 10 hours (atmosphere flow rate of 0.5 L / min) under an oxygen volume concentration of 93%, to obtain a nickel-aluminum positive electrode material. It was determined that the concentration of niobium in the nickel-aluminum positive electrode material was 0.6 mol%, based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material.
[0054] Figure 1 and Figure 2 This is an electron microscope image of the nickel-aluminum positive electrode material of this embodiment. It can be seen from the image that the positive electrode material has a uniform morphology.
[0055] Example 3
[0056] This embodiment provides a method for preparing a nickel-aluminum positive electrode material, comprising the following steps:
[0057] (1) Nickel trioxide and sodium aluminate are mixed and dissolved with ammonia water and sodium hydroxide solution according to the molar ratio of nickel element to aluminum element of 22:1 to obtain a reaction solution, wherein the total molar concentration of all metal ions in the reaction solution is 2 mol / L, the concentration of ammonia water is 8 mol / L, and the concentration of sodium hydroxide solution is 4 mol / L. The reaction solution flows into a 2.5L intermittent reaction container, and 10 mol / L ammonia water, 6 mol / L sodium hydroxide solution and deionized water are introduced into the reaction container at the same time, wherein the stirring speed of the system is controlled to be 400 rpm, the ammonia water is controlled to adjust the ammonia value of the reaction system to 4.0 g / L, and the sodium hydroxide solution is controlled to adjust the pH value of the reaction system to 10-11; the temperature is raised to 60°C under a nitrogen atmosphere for reaction for 6 hours, and the precursor powder is obtained after being rinsed with sodium hydroxide solution and deionized water, and the nickel-aluminum precursor is obtained after drying and sieving for demagnetization; wherein the drying temperature is 100°C. The particle size D50 of the nickel-aluminum precursor is 3-3.5 μm.
[0058] (2) Mixing a nickel-aluminum precursor, lithium hydroxide, and niobium trioxide, wherein the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of lithium in the lithium source is 1:1.35, and the ratio of the total molar amount of nickel and aluminum in the nickel-aluminum precursor to the molar amount of niobium in the niobium source is 1:0.004, mixing evenly with a high-speed mixer, sintering at 680° C. for 8 hours under an oxygen volume concentration of 96% (atmosphere flow rate of 0.2 L / min), to obtain a nickel-aluminum positive electrode material. It was determined that the concentration of niobium in the nickel-aluminum positive electrode material was 0.3 mol%, based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material.
[0059] Comparative Example 1
[0060] This comparative example provides a method for preparing a nickel-aluminum positive electrode material, which differs from Example 1 in that tungsten oxide replaces the molybdenum dioxide in step (2) in equal moles.
[0061] Comparative Example 2
[0062] This comparative example provides a method for preparing a nickel-aluminum positive electrode material, which differs from Example 1 in that zirconium oxide and magnesium oxide replace the molybdenum dioxide in step (2), wherein the molar ratio of the zirconium element in the zirconium oxide, the magnesium element in the magnesium oxide to the total molar amount of the nickel element and the aluminum element in the nickel-aluminum precursor is 0.0045:0.0045:1.
[0063] Comparative Example 3
[0064] This comparative example provides a method for preparing a nickel-aluminum positive electrode material, which differs from Example 1 in that the molybdenum dioxide in step (2) is not added.
[0065] Test Example 1
[0066] This test example provides the performance test of the nickel-aluminum positive electrode materials of each embodiment and comparative example, as follows:
[0067] (1) Particle size test method of nickel-aluminum precursor: Malvern laser particle sizer (Master sizer 2000E) was used for testing. The results are shown in the specific examples.
[0068] (2) Electrochemical properties of nickel-aluminum cathode materials:
[0069] Assemble button batteries: Weigh nickel-aluminum cathode materials, acetylene black, and PVDF (polyvinylidene fluoride) in a mass ratio of 95:2.5:2.5, mix, add appropriate amount of deionized water, grind thoroughly, and then apply on aluminum foil. The compaction density is 3.5g / cm 3 After vacuum drying at 120℃ for 12h and natural cooling, the electrode was sliced using a slicer to obtain a circular electrode with a diameter of 14mm. The battery model is CR2025 button half-cell, the electrolyte is LiPF6 solution, and the solvent in the electrolyte includes ethylene carbonate: dimethyl carbonate: methyl ethyl carbonate in a volume ratio of 1:1:1.
[0070] Test method:
[0071] (1) 0.2C discharge specific capacity measurement: The battery was charged at room temperature at 0.2C constant current to 4.25 V, then at constant voltage (voltage 4.5 V) to a current of 20 mA, and allowed to stand for 10 min; then charged at 0.2C constant current to 2.7 V, allowed to stand for 10 min, and cycled three times. The results are shown in Table 1.
[0072] (2) 1C discharge specific capacity measurement: The above battery (the battery obtained after operating according to test method (1)) was charged at room temperature with 1C constant current to 3.75V, and then charged with constant voltage (voltage is 3.75V) to a current of 20mA, and allowed to stand for 10 minutes; then charged with 1C constant current to 2.7V, allowed to stand for 10 minutes, and cycled 100 times. The results are shown in Table 1.
[0073] Cycle performance = (100th discharge specific capacity / 1st discharge specific capacity) × 100%.
[0074] Table 1 Electrochemical properties of the nickel-aluminum positive electrode materials obtained in Examples 1-3 and Comparative Examples 1-3 when used as positive electrodes for lithium-ion batteries.
[0075]
[0076] As can be seen from Table 1, after the batteries are made of the nickel-aluminum positive electrode materials prepared by the preparation method of the present invention in the test examples, their 0.2C discharge specific capacity is greater than 227.0 mAh / g, and their 1C discharge specific capacity is greater than 181.1 mAh / g. The cycle performance after 100 cycles is maintained at more than 86.9% of the initial discharge capacity.
[0077] Comparison of Example 2 with Examples 1 and 3 shows that niobium is better than molybdenum as a high-valent metal element. Compared with the examples, Comparative Example 1 uses tungsten oxide as a high-valent metal element doping, and its 0.2C discharge capacity and 1C discharge capacity are both reduced, and the cycle performance after 100 cycles is significantly reduced, indicating that the effect of tungsten as a high-valent metal element doping is not as good as the molybdenum and niobium of the present invention; in Comparative Example 2, zirconium and magnesium elements are doped, and the 0.2C discharge capacity is also reduced, and the 1C discharge capacity and the cycle performance after 100 cycles are significantly reduced, indicating that the effect of using composite metal elements for doping is not as good as the molybdenum and niobium selected in the present invention; in Comparative Example 3, no high-valent metal element molybdenum is added for doping, and the 1C discharge capacity and the cycle performance after 100 cycles are greatly reduced; from Comparative Examples 1-3, it can be seen that the high-valent metal elements molybdenum and niobium selected in the present invention can effectively improve the 1C discharge capacity and the cycle performance after 100 cycles of the prepared nickel-aluminum positive electrode material.
[0078] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A nickel-aluminum positive electrode material, characterized in that: The nickel-aluminum positive electrode material is a nickel-aluminum material doped with a high-valent metal element; The high-valent metal element includes at least one of molybdenum and niobium.
2. The nickel-aluminum positive electrode material according to claim 1, characterized in that Based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material, the concentration of molybdenum in the nickel-aluminum positive electrode material is 0.1-1.0 mol%; and / or, Based on the total molar amount of nickel and aluminum in the nickel-aluminum positive electrode material, the concentration of niobium in the nickel-aluminum positive electrode material is 0.1-1.0 mol%.
3. The nickel-aluminum positive electrode material according to claim 2, characterized in that: The high-valent metal element includes niobium.
4. A method for preparing a nickel-aluminum positive electrode material, characterized in that: The following steps are involved: (1) preparing a nickel aluminum precursor; (2) mixing a nickel-aluminum precursor, a lithium source, and an additive, sintering after mixing evenly, to obtain a nickel-aluminum positive electrode material; The additive is a compound containing a high-valent metal element; the high-valent metal element includes at least one of molybdenum and niobium.
5. The preparation method according to claim 4, characterized in that: The ratio of the total molar amount of aluminum element and nickel element in the nickel-aluminum precursor to the molar amount of the high-valent metal element in the additive is 1:(0.0029-0.0093).
6. The preparation method according to claim 4 or 5, characterized in that: The additive is a niobium compound; and / or, The ratio of the total molar amount of aluminum and nickel in the nickel-aluminum precursor to the molar amount of lithium in the lithium source is 1:(1.0-1.4); and / or, The lithium source includes at least one of lithium carbonate, lithium oxalate and lithium hydroxide; and / or, The niobium compound comprises at least one of niobium pentoxide, niobium dioxide and niobium trioxide; and / or, The molybdenum compound includes at least one of molybdenum dioxide and molybdenum disulfide; and / or, The particle size of the nickel-aluminum precursor is 2.5-5 μm.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The step (1) of preparing the nickel-aluminum precursor comprises: mixing a nickel source, an aluminum source and a portion of an alkaline solution to obtain a reaction solution, and continuously adding an alkaline solution to the reaction solution, reacting and drying to obtain a nickel-aluminum precursor; Preferably, the molar ratio of the nickel element in the nickel source to the aluminum element in the aluminum source is (19-24):1; Preferably, the alkaline substance in the alkaline solution includes at least one of sodium hydroxide and ammonia; Preferably, when carrying out the reaction, the pH value of the reaction system is 10-11, and the ammonia value is 4.0-6.0 g / L; Preferably, the reaction temperature is 60-70°C, and the reaction time is 4-12h; Preferably, the reaction is carried out under a protective gas atmosphere; Preferably, the drying temperature is 100-120°C; Preferably, the nickel source includes at least one of nickel sulfate, nickel chloride, and nickel trioxide; Preferably, the aluminum source includes at least one of aluminum oxide, aluminum hydroxide, sodium aluminate, aluminum chloride and aluminum sulfate.
8. The preparation method according to any one of claims 4 to 7, characterized in that: In the step (2), the sintering is carried out in an oxygen atmosphere with a volume concentration of 93-99%; Preferably, the flow rate of the oxygen is 0.2-0.6 L / min; Preferably, the sintering temperature is 680-720° C., and the sintering time is 8-12 hours.
9. The nickel-aluminum positive electrode material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the nickel-aluminum positive electrode material prepared by the preparation method according to any one of claims 1 to 8 in lithium-ion batteries.