Magnetoresistive effect element
By using crystallized Coki Hasler alloy and boron absorbing layer in magnetoresistive effect elements and combining NiAl buffer layer, the problem of low MR ratio of magnetoresistive effect elements on high temperature or non-crystalline substrates in the prior art is solved. The effect of high spin polarization rate and large magnetoresistance ratio is achieved.
Patent Information
- Application Number
- CN202411068854.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-19
AI Technical Summary
When the existing magnetoresistive effect elements form films on high temperature or non-crystalline substrates, it is difficult to achieve sufficient large magnetoresistive ratio (MR ratio), resulting in a low output of the magnetic sensor.
Using a harsh magnetic layer and a non-magnetic layer containing crystallized Coki Hasler alloy, the crystal lattice matches through an annealing step, and boron and specific elements are added to the non-magnetic layer to promote crystallization, forming an L21 or B2 structure The Hasler alloy combines NiAl buffer layer and non-magnetic metal layer to ensure high crystallinity of the laminated structure.
The magnetoresistance ratio of the magnetoresistive effect element is significantly improved, the spin polarization rate is enhanced, and the output signal quality of the magnetic sensor is improved.
Smart Images

Figure CN118984643A_ABST
Abstract
Description
[0001] (This application is a divisional application of a patent application with a filing date of December 21, 2020, application number 202011519004.2, and invention name “Magnetoresistance Effect Element”.) Technical Field
[0002] The present invention relates to a magnetoresistance effect element. Background Art
[0003] A magnetoresistance element is an element whose resistance value in the stacking direction changes due to the magnetoresistance effect. A magnetoresistance element includes two ferromagnetic layers and a non-magnetic layer sandwiched between them. A magnetoresistance element that uses a conductor for the non-magnetic layer is called a giant magnetoresistance (GMR) element, and a magnetoresistance element that uses an insulating layer (tunnel barrier layer, blocking layer) for the non-magnetic layer is called a tunnel magnetoresistance (TMR) element. Magnetoresistance elements can be used in a variety of applications such as magnetic sensors, high-frequency components, magnetic heads, and non-volatile random access memory (MRAM).
[0004] Patent document 1 describes a magnetic sensor having a magnetoresistive effect element, in which a Heusler alloy is used for a ferromagnetic layer. The Heusler alloy has a spin polarization rate, and it can be expected that the output signal of the magnetic sensor will be enhanced. On the other hand, Patent document 1 describes that if the film is not formed on a thick base substrate having a high temperature or a predetermined crystallinity, the Heusler alloy is difficult to crystallize. According to the description of Patent document 1, film formation at a high temperature and a thick base substrate can be said to be the cause of the low output of the magnetic sensor. Patent document 1 describes that the output of the magnetic sensor can be increased by setting the ferromagnetic layer to a stacked structure of a non-crystalline layer and a crystalline layer.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: U.S. Patent No. 9412399 Summary of the invention
[0008] The magnitude of the output signal of the magnetic sensor depends on the magnetoresistance change rate (MR ratio) of the magnetoresistance effect element. Generally speaking, the crystallinity of the ferromagnetic layer sandwiched between the non-magnetic layer is high, but there is a tendency for the MR ratio to become larger. In the magnetoresistance effect element described in Patent Document 1, the ferromagnetic layer in contact with the non-magnetic layer is amorphous, making it difficult to obtain a sufficiently large MR ratio.
[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a magnetoresistive effect element that can achieve a large MR ratio.
[0010] In order to solve the above problems, the present invention provides the following technical solutions.
[0011] (1) A magnetoresistance effect element according to a first embodiment comprises: a first ferromagnetic layer, a second ferromagnetic layer and a non-magnetic layer located between the first ferromagnetic layer and the second ferromagnetic layer, wherein at least one of the first ferromagnetic layer and the second ferromagnetic layer has a first layer and a second layer in sequence from a side close to the non-magnetic layer, wherein the first layer comprises a crystallized Co-based Heusler alloy, and at least a portion of the second layer is crystallized and contains a ferromagnetic element, a boron element and an additive element, wherein the additive element is any element selected from the group consisting of Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt and Au.
[0012] (2) According to the magnetoresistive effect element of the above aspect, the first ferromagnetic layer and the second ferromagnetic layer may both include the first layer and the second layer.
[0013] (3) According to the magnetoresistive effect element of the above aspect, the Co-based Heusler alloy may have a stoichiometric composition and be expressed as CoYZ or Co2YZ, and the Co composition ratio of the Co-based Heusler alloy may be smaller than the stoichiometric composition ratio.
[0014] (4) According to the magnetoresistive effect element of the above aspect, the second layer may be made of crystallized CoFeB-A, and a content of Fe in the second layer may be higher than a content of Co.
[0015] (5) According to the magnetoresistive effect element of the above aspect, in the second layer, the content of the additional element may be higher than the content of boron.
[0016] (6) According to the magnetoresistive effect element of the above aspect, the first layer and the second layer can be lattice matched.
[0017] (7) According to the magnetoresistance effect element of the above method, it can be made to have a boron absorption layer that is in contact with the surface of the second layer away from the non-magnetic layer, and the boron absorption layer contains any element selected from the group consisting of Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt, and Au.
[0018] (8) According to the magnetoresistance effect element of the above aspect, the Co-based Heusler alloy may have an L21 structure or a B2 structure.
[0019] (9) According to the magnetoresistive element of the above embodiment, the Co-based Heusler alloy can be represented as Co2Y α Z β, wherein Y is one or more elements selected from the group consisting of Fe, Mn, and Cr, and Z is one or more elements selected from the group consisting of Si, Al, Ga, and Ge, satisfying α+β>2.
[0020] (10) According to the magnetoresistive effect element of the above aspect, a buffer layer containing NiAl alloy or Ni may be provided between at least one of the first ferromagnetic layer and the nonmagnetic layer and between the second ferromagnetic layer and the nonmagnetic layer.
[0021] (11) According to the magnetoresistive effect element of the above aspect, the buffer layer may have a thickness of 0.63 nm or less.
[0022] (12) According to the magnetoresistive effect element of the above aspect, the nonmagnetic layer may contain a metal or an alloy of any element selected from the group consisting of Cu, Au, Ag, Al, and Cr.
[0023] (13) The magnetoresistive effect element according to the above aspect may further include a substrate which is a base on which the first ferromagnetic layer, the second ferromagnetic layer, and the nonmagnetic layer are stacked, and the substrate is amorphous.
[0024] According to the magnetoresistive effect element of the present invention, a large MR ratio is exhibited. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a cross-sectional view of a magnetoresistance effect element according to the first embodiment;
[0026] Figure 2 is a diagram showing the crystal structure of a Heusler alloy;
[0027] Figure 3 is a cross-sectional view for explaining a method for manufacturing a magnetoresistance effect element according to the first embodiment;
[0028] Figure 4 is a cross-sectional view of a magnetoresistance effect element according to a first modification of the first embodiment;
[0029] Figure 5 is a cross-sectional view of a magnetoresistance effect element according to a second modification of the first embodiment;
[0030] Figure 6 is a cross-sectional view of a magnetoresistance effect element according to a third modified example of the first embodiment;
[0031] Figure 7 is a cross-sectional view of a magnetic recording element according to Application Example 1;
[0032] Figure 8is a cross-sectional view of a magnetic recording element according to Application Example 2;
[0033] Fig. 9 is a cross-sectional view of a magnetic recording element according to Application Example 3;
[0034] Fig.10 is a cross-sectional view of a magnetic wall moving element according to Application Example 4;
[0035] Fig.11 is a cross-sectional view of a high-frequency device according to Application Example 5. DETAILED DESCRIPTION
[0036] The present embodiment will be described in detail below with reference to the accompanying drawings as appropriate. In order to facilitate understanding of the features of the present embodiment, the accompanying drawings used in the following description may sometimes enlarge the features for convenience, and the dimensional ratios of the components may sometimes be different from the actual ones. The materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited thereto, and may be implemented with appropriate changes within the scope of the subject matter.
[0037] [First embodiment]
[0038] Figure 1 2 is a cross-sectional view of a magnetoresistive element according to the first embodiment. First, directions are defined. The direction in which each layer is stacked can be referred to as the stacking direction. Also, the direction in which each layer extends that intersects the stacking direction can be referred to as the in-plane direction.
[0039] Figure 1 The magnetoresistance effect element 10 shown includes a first ferromagnetic (ferromagnetic) layer 1, a second ferromagnetic layer 2, and a non-magnetic layer 3. The non-magnetic layer 3 is located between the first ferromagnetic layer 1 and the second ferromagnetic layer 2.
[0040] The magnetoresistance effect element 10 outputs the change in the relative angle between the magnetization of the first ferromagnetic layer 1 and the magnetization of the second ferromagnetic layer 2 as a change in resistance. The magnetization of the second ferromagnetic layer 2 is easier to change than the magnetization of the first ferromagnetic layer 1, for example. When a predetermined external force is applied, the direction (orientation) of the magnetization of the first ferromagnetic layer 1 does not change (is fixed), while the direction of the magnetization of the second ferromagnetic layer 2 changes. The resistance value of the magnetoresistance effect element 10 changes due to the change in the direction of the magnetization of the second ferromagnetic layer 2 relative to the direction of the magnetization of the first ferromagnetic layer 1. In this case, the first ferromagnetic layer 1 can be called a fixed magnetization layer, and the second ferromagnetic layer 2 can be called a free magnetization layer. In the following, the first ferromagnetic layer 1 is described as a fixed magnetization layer, and the second ferromagnetic layer 2 is described as a free magnetization layer, but the relationship between the two can also be reversed.
[0041] When a predetermined external force is applied, the difference in the ease of change of the magnetization of the first ferromagnetic layer 1 and the magnetization of the second ferromagnetic layer 2 is caused by the difference in the coercive force of the first ferromagnetic layer 1 and the second ferromagnetic layer 2. For example, if the thickness of the second ferromagnetic layer 2 is made thinner than the thickness of the first ferromagnetic layer 1, the coercive force of the second ferromagnetic layer 2 is smaller than the coercive force of the first ferromagnetic layer 1. Moreover, for example, an antiferromagnetic layer may be provided on the surface of the first ferromagnetic layer 1 opposite to the non-magnetic layer 3 via a spacer layer. Thus, the first ferromagnetic layer 1, the spacer layer, and the antiferromagnetic layer form a synthetic antiferromagnetic structure (SAF structure). The synthetic antiferromagnetic structure is composed of two magnetic layers sandwiching a spacer layer. Due to the antiferromagnetic coupling between the first ferromagnetic layer 1 and the antiferromagnetic layer, the coercive force of the first ferromagnetic layer 1 becomes larger than that of the case where there is no antiferromagnetic layer. The antiferromagnetic layer is, for example, IrMn, PtMn, etc. The spacer layer contains, for example, at least one selected from the group consisting of Ru, Ir, and Rh.
[0042] The first ferromagnetic layer 1 and the second ferromagnetic layer 2 contain a ferromagnetic substance. Figure 1 The first ferromagnetic layer 1 and the second ferromagnetic layer 2 of the magnetoresistance effect element 10 shown in the figure respectively include the first layer 1A, 2A and the second layer 1B, 2B. The first ferromagnetic layer 1 includes the first layer 1A and the second layer 1B in order from the side close to the non-magnetic layer 3. The second ferromagnetic layer 2 includes the first layer 2A and the second layer 2B in order from the side close to the non-magnetic layer 3.
[0043] For example, the first layer 1A and the second layer 1B are lattice matched, and the first layer 2A and the second layer 2B are lattice matched. Lattice matching means that atoms are arranged continuously in the stacking direction at the interface between the first layer 1A and the second layer 1B, and the interface between the first layer 2A and the second layer 2B. The lattice matching degree between the first layer 1A and the second layer 1B, or the first layer 2A and the second layer 2B is, for example, within 5%. The lattice matching degree is the degree of deviation of the lattice constant of the second layer 1B and 2B when the lattice constant of the first layer 1A and 2A is used as a reference. When the first layer 1A and the second layer 1B, and the first layer 2A and the second layer 2B are lattice matched, the MR ratio of the magnetoresistive effect element 10 becomes larger.
[0044] The first layers 1A and 2A both contain a crystallized Co-based Heusler alloy. The first layers 1A and 2A are each composed of, for example, a Co-based Heusler alloy, and at least a portion of the Co-based Heusler alloy is crystallized. The first layers 1A and 2A may also be composed of, for example, a completely crystallized Co-based Heusler alloy.
[0045] Heusler alloys are intermetallic compounds with a chemical composition of XYZ or X2YZ. A ferromagnetic Heusler alloy written as X2YZ is called a full Heusler alloy, while a ferromagnetic Heusler alloy written as XYZ is called a half Heusler alloy. A half Heusler alloy is obtained when part of the atoms in the X crystal position of a full Heusler alloy become lattice vacancies. Both are typical intermetallic compounds based on bcc structure.
[0046] Figure 2 This is an example showing the crystal structure of a Heusler alloy. Figure 2 (a) to (c) are examples of the crystal structures of full Heusler alloys. Figure 2 (d) to (f) are examples of crystal structures of semi-Heusler alloys.
[0047] Figure 2 (a) is called L21 structure. In L21 structure, elements in X crystal position, elements in Y crystal position, and elements in Z crystal position are fixed. Figure 2 (b) is called the B2 structure derived from the L21 structure. In the B2 structure, the elements entering the Y crystal position and the elements entering the Z crystal position are mixed, while the elements entering the X crystal position are fixed. Figure 2 (c) is called the A2 structure derived from the L21 structure. In the A2 structure, elements that enter the X crystal position, elements that enter the Y crystal position, and elements that enter the Z crystal position are mixed together.
[0048] Figure 2 (d) is called C1 b Construction. C1 b In the structure, the elements entering the X crystal position, the elements entering the Y crystal position, and the elements entering the Z crystal position are fixed. Figure 2 (e) is called obtained from C1 b In the B2 structure, the elements entering the Y crystal position and the elements entering the Z crystal position are mixed together, while the elements entering the X crystal position are fixed. Figure 2 (f) is called obtained from C1 b In the A2 structure, the elements that enter the X crystal position, the elements that enter the Y crystal position, and the elements that enter the Z crystal position are mixed together.
[0049] In full Heusler alloys, the crystallinity increases in the order of L21 structure > B2 structure > A2 structure, while in half Heusler alloys, the crystallinity increases in the order of C1 bThe crystallinity increases in the order of structure>B2 structure>A2 structure. The crystallinity of these crystal structures varies, but they are all crystals. Therefore, the first layers 1A and 2A each have, for example, any of the above-mentioned crystal structures. The crystal structures of the first layers 1A and 2A are, for example, L21 structure or B2 structure.
[0050] Whether the Heusler alloy is crystallized can be determined by a transmission electron microscope (TEM) image (e.g., a high-angle scattering annular dark field scanning transmission electron microscope: HAADF-STEM image) or an electron beam diffraction image using a transmission electron beam. If the Heusler alloy has been crystallized, the regular arrangement of atoms can be confirmed using, for example, a HAADF-STEM image taken by a TEM. More specifically, in the Fourier transform image of the HAADF-STEM image, spots of the crystal structure of the Heusler alloy are present. In addition, if the Heusler alloy has been crystallized, diffraction spots from at least one of the (001) plane, (002) plane, (110) plane, and (111) plane can be confirmed in the electron beam diffraction image. When crystallization can be confirmed by at least one means, it can be said that at least a portion of the Heusler alloy has been crystallized.
[0051] The composition analysis of each layer constituting the magnetoresistive element can be performed by energy dispersive X-ray analysis (EDS). By performing EDS X-ray analysis, for example, the composition analysis of each material in the film thickness direction can be confirmed.
[0052] Co-based Heusler alloy is a Heusler alloy in which the X crystal position is Co. Y is a transition metal of the Mn, V, Cr, Ti family, or a transition metal or noble metal element of the Co, Fe, Ni, Cu family. Z is a typical element from group III to group V. The Y element is preferably one or more elements selected from the group consisting of Fe, Mn, and Cr. The Z element is preferably one or more elements selected from the group consisting of Si, Al, Ga, and Ge.
[0053] Full Heusler alloys such as Co2FeSi, Co2FeGe, Co2FeGa, Co2FeAl, Co2FeGe x Ga 1-x , Co2MnSi, Co2MnGe, Co2MnGa, Co2MnSn, Co2MnAl, Co2CrAl, Co2VAl, Co2Mn 1-a Fe a Al b Si 1-b Etc. Semi-Heusler alloys include, for example, CoFeSb, NiMnSe, NiMnTe, NiMnSb, PtMnSb, PdMnSb, CoFeSb, RhMnSb, CoMnSb, IrMnSb, and NiCrSb.
[0054] The Co-based Heusler alloy constituting the first layers 1A and 2A is represented by, for example, Co2Y α Z β . The Co-based full Heusler alloy of the stoichiometric composition is recorded as Co2YZ. The Co composition ratio of the Co-based Heusler alloy constituting the first layer 1A, 2A is preferably smaller than the stoichiometric composition ratio. That is, when the Co-based Heusler alloy is a full Heusler alloy, it is preferred to satisfy α+β>2. When the Co-based Heusler alloy is a half-Heusler alloy, the Co-based Heusler alloy constituting the first layer 1A, 2A is recorded as Co2Y α Z β , preferably satisfying α+β>1.
[0055] If the Co composition ratio is smaller than the elements in the Y crystal position, it is possible to avoid the elements in the Y crystal position being replaced by the anti-position of the elements in the X crystal position (the crystal position where Co enters). The anti-position causes the Fermi level of the Heusler alloy to change. If the Fermi level changes, the semi-metallic properties of the Heusler alloy decrease, and the spin polarization rate decreases. The low spin polarization rate is the reason why the MR ratio of the magnetoresistive effect element 10 is low.
[0056] The second layers 1B and 2B each include a crystallized portion. Furthermore, the second layers 1B and 2B each include an alloy containing a ferromagnetic element, boron, and an additive element. The second layer may also contain other elements besides the ferromagnetic element, boron, and the additive element. For example, the second layers 1B and 2B each may be composed of an alloy of a ferromagnetic element, boron, and an additive element, or at least a portion of the ferromagnetic element, boron, and the additive element may be crystallized. For example, the second layers 1B and 2B each may be fully crystallized, or may be composed of an alloy of a ferromagnetic element, boron, and an additive element.
[0057] The ferromagnetic element is, for example, at least one magnetic element selected from the group consisting of Cr, Mn, Co, Fe and Ni. The additive A element is any element selected from the group consisting of Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt and Au.
[0058] Alloys containing ferromagnetic elements, boron and additive elements are, for example, CoFeB-A and CoFeGaGeB-A. CoFeB-A is obtained by adding additive elements as A elements to CoFeB alloy. In addition, CoFeGaGeB-A is obtained by adding additive elements as A elements to CoFeGaGeB alloy. That is, A element is an example of an additive element. Even if A element invades the crystal structure of CoFeB, it can be replaced by any element of CoFeB crystal. A element is preferably any element selected from the group consisting of Ti, Ru and Ta, and is particularly preferably Ta.
[0059] The A element has a property of attracting boron. Among the A elements, Ti, Ru, and Ta have particularly strong properties. As will be described in detail later, since the second layer 1B, 2B contains the A element, boron moves in the second layer 1B, 2B during heating, thereby promoting crystallization of the second layer 1B, 2B.
[0060] The content of the A element in the second layer 1B, 2B is higher than, for example, the content of boron. The content of the A element is, for example, 0.1 or more in the composition ratio of CoFeB-A. When there is a sufficient amount of the A element, the A element does not adsorb too much or too little boron in the second layer 1B, 2B. As a result, the diffusion of boron from the second layer 1B, 2B to the first layer 1A, 2A can be suppressed. If boron is included in the first layer 1A, 2A, the crystallinity of the first layer 1A, 2A decreases, which may cause a decrease in the MR ratio.
[0061] In the case of CoFeB-A in which the second layers 1B and 2B are crystallized, the Fe content in the second layers 1B and 2B is, for example, greater than the Co content. When the Fe content in the second layers 1B and 2B increases, diffusion of the Co element in the first layers 1A and 2A into the second layers 1B and 2B can be suppressed during annealing. By preventing the Co element in the first layers 1A and 2A from diffusing from the X crystal position, the crystal structure of the first layers 1A and 2A becomes an L21 structure, a C1 b Structure and B2 structure. L21 structure, C1 b The B2 structure and the B2 structure are highly crystalline, and the magnetoresistance effect element 10 having the first layers 1A, 2A having the crystalline structures exhibits a large MR ratio.
[0062] The non-magnetic layer 3 is made of, for example, a non-magnetic metal. The non-magnetic layer 3 is, for example, a metal or alloy containing any element selected from the group consisting of Cu, Au, Ag, Al, and Cr. The non-magnetic layer 3 contains, for example, any element selected from the group consisting of Cu, Au, Ag, Al, and Cr as main constituent elements. The main constituent elements refer to the proportion of Cu, Au, Ag, Al, and Cr accounting for more than 50% in the composition formula. The non-magnetic layer 3 preferably contains Ag, and preferably contains Ag as the main constituent element. Since the spin diffusion length of Ag is long, the MR ratio of the magnetoresistance effect element 10 using Ag is large.
[0063] The thickness of the non-magnetic layer 3 is, for example, in the range of 1 nm to 10 nm. The non-magnetic layer 3 suppresses magnetic coupling between the first ferromagnetic layer 1 and the second ferromagnetic layer 2 .
[0064] The non-magnetic layer 3 can be an insulator or a semiconductor. Non-magnetic insulators are, for example, Al2O3, SiO2, MgO, MgAl2O4, and materials in which a portion of Al, Si, and Mg are replaced by Zn, Be, etc. These materials have a large band gap and excellent insulating properties. When the non-magnetic layer 3 is made of a non-magnetic insulator, the non-magnetic layer 3 is a tunnel barrier layer. Non-magnetic semiconductors are, for example, Si, Ge, CuInSe2, CuGaSe2, Cu(In, Ga)Se2, etc.
[0065] Next, a method of manufacturing the magnetoresistance effect element 10 will be described. The method of manufacturing the magnetoresistance effect element 10 includes a film forming step of each layer and an annealing step after the film forming. In the annealing step, the ferromagnetic element, boron, and the A element are crystallized.
[0066] Figure 3 1 is a schematic diagram for explaining a method for manufacturing a magnetoresistive effect element 10 according to a first embodiment. First, a substrate Sub is prepared as a base for film formation. The substrate Sub can be crystalline or amorphous. Examples of crystalline substrates include metal oxide single crystals, silicon single crystals, and sapphire single crystals. Examples of amorphous substrates include silicon single crystals with thermal oxidation films, ceramics, and quartz glass.
[0067] Next, the second layer 11B, the first layer 11A, the nonmagnetic layer 13, the first layer 12A, and the second layer 12B are sequentially stacked on the substrate Sub. These layers are formed into films by, for example, a sputtering method.
[0068] The second layers 11B and 12B are both made of an alloy containing the above-mentioned ferromagnetic element, boron and A element. After film formation, the second layers 11B and 12B are both amorphous. The first layers 11A and 12A are both the above-mentioned Co-based Heusler alloys. Since the first layers 11A and 12A grow on an amorphous substrate, they grow in the (110) direction that they are easily generated. Therefore, the first layers 11A and 12A are crystals with low crystallinity. The non-magnetic layer 13 is made of the same material as the above-mentioned non-magnetic layer 3.
[0069] Next, the stacked body stacked on the substrate Sub is annealed at a temperature of, for example, 300° C. or less, for example, 250° C. or more and 300° C. or less.
[0070] When the stacked body is annealed, in the second layers 11B and 12B, boron included in the ferromagnetic element, boron, and element A is attracted to element A. Boron is attracted to element A and diffuses in the second layers 11B and 12B. When boron diffuses in the second layers 11B and 12B, atoms in the second layers 11B and 12B are mixed. The mixed atoms are rearranged, and the second layers 11B and 12B are crystallized.
[0071] The second layers 11B and 12B both have a bcc type crystal structure. In the process of forming the second layers 11B and 12B into bcc type crystal structures, the atoms contained in the first layers 11A and 12A are also rearranged. The atoms contained in the first layers 11A and 12A are rearranged under the influence of the crystal structure of the adjacent second layer 11B or the second layer 12B, so that the first layers 11A and 12A are crystallized. That is, each layer in the first layer 11A and 12A is dragged by the crystallization of each layer in the second layer 11B and 12B, and is further regularized to become a crystal with high crystallinity.
[0072] As described above, by annealing the laminate, the second layers 11B and 12B are crystallized to become the second layers 1B and 2B, and the first layers 11A and 12A are crystallized to become the first layers 1A and 2A. The nonmagnetic layer 13 becomes the nonmagnetic layer 3. As a result, Figure 1 The magnetoresistance effect element 10 is shown.
[0073] As described above, by using the manufacturing method of the magnetoresistive effect element 10 according to the present embodiment, the Heusler alloy can be crystallized regardless of the crystal structure of the substrate. Here, one of the processes of the manufacturing method of the magnetoresistive effect element 10 is introduced, but the above method can also be applied to the crystallization method of a single ferromagnetic layer. For example, by stacking a layer of an alloy containing a ferromagnetic element, boron and an A element and a ferromagnetic layer containing a Heusler alloy and heating them, a crystalline Heusler alloy can be obtained.
[0074] In the manufacturing method of the magnetoresistive effect element 10 according to the present embodiment, the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are crystallized at a low temperature of 300°C or less. If the temperature is 300°C or less, even if annealing is performed after manufacturing other constituent elements of the magnetic head, for example, the adverse effects on other constituent elements (for example, magnetic shielding) can be reduced. Therefore, the timing of annealing is not limited, and the manufacturing of elements such as magnetic heads becomes easy.
[0075] In the magnetoresistance effect element 10 according to the present embodiment, the first ferromagnetic layer 1 and the second ferromagnetic layer 2 sandwiching the nonmagnetic layer 3 are crystallized. Therefore, the first ferromagnetic layer 1 and the second ferromagnetic layer 2 show high spin polarization. As a result, the magnetoresistance effect element 10 according to the present embodiment shows a high MR ratio.
[0076] Although the embodiments of the present invention have been described in detail with reference to the drawings, the configuration and combination of each embodiment are examples, and additions, omissions, substitutions and other changes may be made to the configuration without departing from the gist of the present invention.
[0077] For example, Figure 4FIG. 1 is a cross-sectional view of a magnetoresistance effect element 10A according to a first modification. Figure 4 In the magnetoresistance effect element 10A shown, only the first ferromagnetic layer 1 has a first layer 1A and a second layer 1B. Figure 4 In the example in which only the first ferromagnetic layer 1 has the first layer and the second layer, only the second ferromagnetic layer 2 may have the first layer and the second layer. In this case, the remaining one ferromagnetic layer may be, for example, a metal selected from the group consisting of Cr, Mn, Co, Fe, and Ni, an alloy containing one or more of these metals, an alloy containing these metals and at least one element of B, C, and N, or a Heusler alloy. For example, the composition of the remaining one ferromagnetic layer is Co-Fe, Co-Fe-B.
[0078] For example, the magnetoresistance effect element may have layers other than the first ferromagnetic layer 1 , the second ferromagnetic layer 2 , and the nonmagnetic layer 3 .
[0079] Figure 5 2 is a cross-sectional view of a magnetoresistance effect element 10B according to a second modification. Figure 5 The magnetoresistance effect element 10B shown in FIG. Figure 1 The magnetoresistance effect element 10 shown is different in that it has boron absorption layers 4 , 5 .
[0080] The boron absorption layers 4 and 5 are non-magnetic layers. The boron absorption layers 4 and 5 each contain boron and any element selected from the group consisting of Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt, and Au. In the following, Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt, and Au are the same as the above-mentioned A element, but the A element contained in the boron absorption layers 4 and 5 is not necessarily the same as the A element contained in the second layers 1B and 2B.
[0081] The boron absorption layers 4 and 5 are obtained, for example, by adding boron to a metal or alloy consisting of element A. The boron absorption layers 4 and 5 preferably contain any element A selected from the group consisting of Ti, Ru and Ta. The boron absorption layers 4 and 5 are obtained, for example, by adding boron or carbon to a metal or alloy containing any element selected from the group consisting of Ti, Ru and Ta.
[0082] The boron absorbing layers 4 and 5 do not contain boron in the film forming step, for example. That is, the boron absorbing layers 4 and 5 before the annealing step are, for example, metal or alloy of element A. As described above, element A has the property of attracting boron. In the boron absorbing layers 4 and 5, boron is contained because element A attracts boron during annealing.
[0083] The boron absorption layers 4 and 5 suppress the diffusion of boron into the first layers 1A and 2A and the non-magnetic layer 3 during annealing. When the first layers 1A and 2A contain boron, the crystallinity of the first layers 1A and 2A decreases, and the MR ratio of the magnetoresistive effect element 10 decreases. When the non-magnetic layer 3 contains boron, the crystallinity of the non-magnetic layer 3 decreases, and the MR ratio of the magnetoresistive effect element 10B decreases. That is, the boron absorption layers 4 and 5 prevent the boron contained in the second layers 1B and 2B from diffusing into the first layers 1A and 2A and the non-magnetic layer 3, and suppress the decrease in the MR ratio of the magnetoresistive effect element 10B.
[0084] Figure 6 is a cross-sectional view of the magnetoresistive effect element 10C according to the third modification. Figure 6 The shown magnetoresistive effect element 10C is different from Figure 1 the shown magnetoresistive effect element 10 in that it has buffer layers 6 and 7.
[0085] The buffer layers 6 and 7 are layers containing NiAl alloy or Ni, respectively. The buffer layer 6 is a buffer layer that alleviates the lattice mismatch between the first ferromagnetic layer 1 and the non-magnetic layer 3. The buffer layer 7 is a buffer layer that alleviates the lattice mismatch between the non-magnetic layer 3 and the second ferromagnetic layer 2.
[0086] The thickness t of the buffer layers 6 and 7 is, for example, 0 < t ≤ 0.63 nm, respectively. If the thickness t becomes too thick, spin scattering may occur in the electrons moving from the first ferromagnetic layer 1 (or the second ferromagnetic layer 2) to the second ferromagnetic layer 2 (or the first ferromagnetic layer 1). When the thickness t is within this range, spin scattering in the moving electrons is suppressed, the lattice mismatch between the first ferromagnetic layer 1 and the non-magnetic layer 3 is reduced, and the lattice mismatch between the non-magnetic layer 3 and the second ferromagnetic layer 2 is reduced. As the lattice mismatch of each layer becomes smaller, the MR ratio of the magnetoresistive effect element 10C increases. In Figure 6 it, an example in which the magnetoresistive effect element 10C has both buffer layers 6 and 7 is shown, but the magnetoresistive effect element may have at least one of the buffer layers 6 and 7.
[0087] Although the first modification to the third modification are shown above, they are also examples of the magnetoresistive effect element according to the present embodiment. For example, the characteristic structures of the first modification to the third modification can be combined.
[0088] The above magnetoresistive effect elements 10, 10A, 10B, and 10C can be used for various purposes. The magnetoresistive effect elements 10, 10A, 10B, and 10C can be applied to, for example, magnetic heads, magnetic sensors, magnetic memories, high-frequency filters, etc.
[0089] Next, application examples of the magnetoresistive effect element according to the present embodiment will be described. In the following application examples, the magnetoresistive effect element 10 is used as the magnetoresistive effect element, but the magnetoresistive effect element is not limited thereto.
[0090] Figure 7 is a cross-sectional view of a magnetic recording element 100 according to Application Example 1. Figure 7 It is a cross-sectional view of the magnetoresistive effect element 10 cut along the stacking direction.
[0091] like Figure 7 As shown, the magnetic recording element 100 has a magnetic head MH and a magnetic recording medium W. Figure 7 In the figure, one direction in which the magnetic recording medium W extends is set as the X direction, and the direction perpendicular to the X direction is the Y direction. The XY plane is parallel to the main surface of the magnetic recording medium W. The direction connecting the magnetic recording medium W and the magnetic head MH and perpendicular to the XY plane is the Z direction.
[0092] In the magnetic head MH, an air bearing surface (Air Bearing Surface: a surface facing the medium) S faces the surface of the magnetic recording medium W. The magnetic head MH moves along the surface of the magnetic recording medium W in the directions of arrows +X and -X at a certain distance from the magnetic recording medium W. The magnetic head MH has a magnetoresistive effect element 10 used as a magnetic sensor and a magnetic recording portion (not shown). The resistance measuring device 21 measures the resistance value of the magnetoresistive effect element 10 in the stacking direction.
[0093] The magnetic recording section applies a magnetic field to the recording layer W1 of the magnetic recording medium W to determine the magnetization direction of the recording layer W1. That is, the magnetic recording section performs magnetic recording of the magnetic recording medium W. The magnetoresistive effect element 10 reads information on the magnetization of the recording layer W1 written by the magnetic recording section.
[0094] The magnetic recording medium W has a recording layer W1 and a backing layer W2. The recording layer W1 is a portion for magnetic recording, and the backing layer W2 is a magnetic path (a path of magnetic flux) for returning magnetic flux used for writing to the magnetic head MH again. The recording layer W1 records magnetic information as a magnetization direction.
[0095] The second ferromagnetic layer 2 of the magnetoresistive element 10 is, for example, a free magnetization layer. Therefore, the second ferromagnetic layer 2 exposed on the air bearing surface S is affected by the magnetization recorded on the recording layer W1 of the opposing magnetic recording medium W. For example, Figure 7 In the embodiment, the magnetization direction of the second ferromagnetic layer 2 is oriented in the +z direction due to the influence of the magnetization in the +z direction of the recording layer W1. In this case, the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 as fixed magnetization layers are parallel.
[0096] Here, the resistance when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are parallel is different from the resistance when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are antiparallel. The greater the difference between the resistance value in the parallel case and the resistance value in the antiparallel case, the greater the MR ratio of the magnetoresistance effect element 10. The magnetoresistance effect element 10 according to the present embodiment includes a crystallized Heusler alloy and has a large MR ratio. Therefore, information related to the magnetization of the recording layer W1 can be accurately read by the resistance measuring device 21 as a change in the resistance value.
[0097] For example, the first ferromagnetic layer 1 may be disposed away from the magnetic recording medium W to prevent the leakage magnetic field of the magnetic recording medium W from affecting the first ferromagnetic layer 1 of the magnetoresistive element 10 .
[0098] Figure 8 is a cross-sectional view of a magnetic recording element 101 according to Application Example 2. Figure 8 It is a cross-sectional view of the magnetic recording element 101 cut along the stacking direction.
[0099] like Figure 8 As shown, magnetic recording element 101 includes magnetoresistance element 10, power supply 22 and measuring unit 23. Power supply 22 generates a potential difference in the stacking direction of magnetoresistance element 10. Power supply 22 is, for example, a DC power supply. Measuring unit 23 measures the resistance value of magnetoresistance element 10 in the stacking direction.
[0100] When a potential difference is generated between the first ferromagnetic layer 1 and the second ferromagnetic layer 2 by the power supply 22, an electric current flows along the stacking direction of the magnetoresistance effect element 10. When the electric current passes through the first ferromagnetic layer 1, it is spin-polarized and becomes a spin-polarized current. The spin-polarized current reaches the second ferromagnetic layer 2 via the non-magnetic layer 3. By receiving the spin transfer torque (STT) generated by the spin-polarized current, the magnetization of the second ferromagnetic layer 2 is reversed. By changing the relative angle between the magnetization direction of the first ferromagnetic layer 1 and the magnetization direction of the second ferromagnetic layer 2, the resistance value of the magnetoresistance effect element 10 in the stacking direction is changed. The resistance value of the magnetoresistance effect element 10 in the stacking direction is read out by the measuring unit 23. That is, Figure 8 The illustrated magnetic recording element 101 is a spin transfer torque (STT) type magnetic recording element.
[0101] Figure 8 The magnetic recording element 101 shown can accurately record data because it includes the magnetoresistive effect element 10 including a crystalline Heusler alloy and having a large MR ratio.
[0102] Fig. 9 is a cross-sectional view of a magnetic recording element 102 according to Application Example 3. Fig. 9It is a cross-sectional view of the magnetic recording element 102 cut along the stacking direction.
[0103] like Fig. 9 As shown, the magnetic recording element 102 has a magnetoresistance effect element 10, a spin-orbit torque wiring 8, a power supply 22 and a measuring unit 23. The spin-orbit torque wiring 8 is in contact with the second layer 1B of the first ferromagnetic layer 1, for example. The spin-orbit torque wiring 8 extends in one direction in the in-plane direction. The power supply 22 is connected to the first end and the second end of the spin-orbit torque wiring 8. In a plan view, the magnetoresistance effect element 10 is sandwiched between the first end and the second end. The power supply 22 causes a write current to flow along the spin-orbit torque wiring 8. The measuring unit 23 measures the resistance value of the magnetoresistance effect element 10 in the stacking direction.
[0104] When a potential difference is generated between the first end and the second end of the spin-orbit torque wiring 8 by the power supply 22, current flows in the in-plane direction of the spin-orbit torque wiring 8. The spin-orbit torque wiring 8 has a function of generating a spin current by a spin hole effect when a current flows. The spin-orbit torque wiring 8 is, for example, any one of a metal, an alloy, an intermetallic compound, a metal boride, a metal carbide, a metal silicate, and a metal phosphide having a function of generating a spin current by a spin hole effect when a current flows. For example, the wiring includes a non-magnetic metal having a d electron or a f electron in the outermost shell and an atomic number of 39 or more.
[0105] When current flows in the in-plane direction of the spin-orbit torque wiring 8, a spin hole effect is generated by the spin-orbit interaction. The spin hole effect is a phenomenon in which the moving spins are bent in a direction orthogonal to the current flow direction. The spin hole effect generates an uneven distribution of spins in the spin-orbit torque wiring 8 and induces a spin flow in the thickness direction of the spin-orbit torque wiring 8. The spins are injected from the spin-orbit torque wiring 8 into the first ferromagnetic layer 1 through the spin flow.
[0106] The spin injected into the first ferromagnetic layer 1 imparts a spin-orbit torque (SOT) to the magnetization of the first ferromagnetic layer 1. The first ferromagnetic layer 1 receives the spin-orbit torque (SOT) and reverses its magnetization. In this case, the first ferromagnetic layer 1 becomes a free magnetization layer, and the second ferromagnetic layer 2 becomes a fixed magnetization layer. By changing the magnetization direction of the first ferromagnetic layer 1 and the magnetization direction of the second ferromagnetic layer 2, the resistance value of the magnetoresistive effect element 10 in the stacking direction is changed. The resistance value of the magnetoresistive effect element 10 in the stacking direction is read by the measuring unit 23. That is, Fig. 9 The illustrated magnetic recording element 102 is a spin-orbit torque (SOT) type magnetic recording element.
[0107] Fig. 9The magnetic recording element 102 shown in FIG. 1 can accurately record data because it includes the magnetoresistive effect element 10 including a crystalline Heusler alloy and having a large MR ratio.
[0108] Fig.10 1 is a cross-sectional view of a magnetic wall displacement element (magnetic wall displacement type magnetic recording element) according to Application Example 4. The magnetic wall displacement element 103 has a magnetoresistance effect element 10, a first fixed magnetization layer 24 and a second fixed magnetization layer 25. The magnetoresistance effect element 10 is composed of a first ferromagnetic layer 1, a second ferromagnetic layer 2 and a non-magnetic layer 3. Fig.10 In the figure, the direction in which the first ferromagnetic layer 1 extends is set as the X direction, the direction perpendicular to the X direction is the Y direction, and the direction perpendicular to the XY plane is the Z direction.
[0109] The first fixed magnetization layer 24 and the second fixed magnetization layer 25 are connected to the first end and the second end of the first ferromagnetic layer 1. The first end and the second end sandwich the second ferromagnetic layer 2 and the non-magnetic layer 3 in the X direction.
[0110] The first ferromagnetic layer 1 is a layer capable of magnetically recording information by changing the internal magnetic state. The first ferromagnetic layer 1 has a first magnetic region MD1 and a second magnetic region MD2 inside. The magnetization of the first ferromagnetic layer 1 at a position overlapping with the first fixed magnetization layer 24 or the second fixed magnetization layer 25 in the Z direction is fixed in one direction. For example, the magnetization at a position overlapping with the first fixed magnetization layer 24 in the Z direction is fixed in the +Z direction, and for example, the magnetization at a position overlapping with the second fixed magnetization layer 25 in the Z direction is fixed in the -Z direction. As a result, a magnetic wall DW is formed at the boundary between the first magnetic region MD1 and the second magnetic region MD2. The first ferromagnetic layer 1 may have a magnetic wall DW inside. Fig.10 In the first ferromagnetic layer 1 shown in FIG. 1 , the magnetization M of the first magnetic region MD1 is MD1 The magnetization M of the second magnetic region MD2 is oriented in the +Z direction. MD2 Oriented along the -Z direction.
[0111] The magnetic wall displacement element 103 can record data in multiple values or continuously according to the position of the magnetic wall DW of the first ferromagnetic layer 1. When a read current is applied, the data recorded in the first ferromagnetic layer 1 is read as a change in the resistance value of the magnetic wall displacement element 103.
[0112] The ratio of the first magnetic region MD1 to the second magnetic region MD2 in the first ferromagnetic layer 1 changes with the movement of the magnetic wall DW. MD1 In the same direction (parallel) and in the same direction as the magnetization M of the second magnetic region MD2 MD2In the opposite direction (antiparallel). When the magnetic wall DW moves in the +X direction and the area of the first magnetic region MD1 in the portion overlapping with the second ferromagnetic layer 2 when viewed from the Z direction becomes larger, the resistance value of the magnetic wall moving element 103 will become lower. On the contrary, when the magnetic wall DW moves in the -X direction and the area of the second magnetic region MD2 in the portion overlapping with the second ferromagnetic layer 2 when viewed from the Z direction becomes larger, the resistance value of the magnetic wall moving element 103 will become higher.
[0113] The magnetic wall DW causes the write current to flow in the X direction of the first ferromagnetic layer 1 or to move by applying an external magnetic field. For example, when a write current (e.g., a current pulse) is applied in the +X direction of the first ferromagnetic layer 1, electrons flow in the -X direction opposite to the current, so that the magnetic wall DW moves in the -X direction. When the current flows from the first magnetic region MD1 to the second magnetic region MD2, the spin-polarized electrons in the second magnetic region MD2 cause the magnetization M of the first magnetic region MD1 to move. MD1 Magnetization reversal. Due to the magnetization M of the first magnetic region MD1 MD1 The magnetization is reversed and the magnetic wall DW moves in the -X direction.
[0114] because Fig.10 The magnetic wall displacement element 103 shown in FIG. 1 includes the magnetoresistive effect element 10 including a crystallized Heusler alloy and having a large MR ratio, and thus data can be accurately recorded.
[0115] Fig.11 is a schematic diagram of a high frequency device 104 according to Application Example 5. Fig.11 As shown, the high-frequency device 104 includes a magnetoresistance effect element 10 , a DC power supply 26 , an inductor 27 , a capacitor 28 , an output port 29 , and wirings 30 , 31 .
[0116] Wiring 30 connects magnetoresistance effect element 10 and output port 29. Wiring 31 branches out from wiring 30 and reaches ground G through inductor 27 and DC power supply 26. DC power supply 26, inductor 27 and capacitor 28 can use known ones. Inductor 27 cuts off the high frequency component of the current and allows the constant component of the current to pass. Capacitor 28 allows the high frequency component of the current to pass and cuts off the constant component of the current. Inductor 27 is arranged at the part where the flow of high frequency current is to be suppressed, and capacitor 28 is arranged at the part where the flow of DC current is to be suppressed.
[0117] When an alternating current or an alternating magnetic field is applied to the ferromagnetic layer included in the magnetoresistive effect element 10, the magnetization of the second ferromagnetic layer 2 performs a precession motion. When the frequency of the high-frequency current or high-frequency magnetic field applied to the second ferromagnetic layer 2 is close to the ferromagnetic resonance frequency of the second ferromagnetic layer 2, the magnetization of the second ferromagnetic layer 2 vibrates strongly, and does not vibrate much at a frequency far from the ferromagnetic resonance frequency of the second ferromagnetic layer 2. This phenomenon is called a ferromagnetic resonance phenomenon.
[0118] The resistance value of the magnetoresistance effect element 10 changes due to the vibration of the magnetization of the second ferromagnetic layer 2. The DC power supply 26 applies a DC current to the magnetoresistance effect element 10. The DC current flows in the stacking direction of the magnetoresistance effect element 10. The DC current flows to the ground G through the wiring 30, 31 and the magnetoresistance effect element 10. The potential of the magnetoresistance effect element 10 changes according to Ohm's law. In response to the change in the potential (change in the resistance value) of the magnetoresistance effect element 10, a high-frequency signal is output from the output port 29.
[0119] Fig.11 The high-frequency device 104 shown includes the magnetoresistive effect element 10 which includes a crystalline Heusler alloy and has a wide range of variation in resistance value, and can transmit a high-frequency signal with a large output.
[0120] [Example]
[0121] (Example 1)
[0122] As Example 1, a Figure 1 The magnetoresistance effect element 10 shown in the figure. The first ferromagnetic layer 1 and the second ferromagnetic layer 2 are respectively composed of the first layer 1A, 2A and the second layer 1B, 2B. The first layer 1A, 2A is a crystallized Co-based Heusler alloy with a composition ratio of Co2FeGa 0.5 Ge 0.5 The second layers 1B and 2B are crystallized CoFeB-A, and the composition ratio is (Co 0.4 Fe 0.4 B 0.2 ) 0.9 Ta 0.1 The non-magnetic layer 3 is Ag.
[0123] The magnetoresistance effect element 10 according to Example 1 is manufactured by the following steps. First, on an amorphous substrate, the second layer 1B, the first layer 1A, the non-magnetic layer 3, the first layer 2A, and the second layer 2B having the above-mentioned composition are sequentially sputtered and formed by the sputtering method. After the film formation, the first layers 1A and 2A become crystals with low crystallinity, and the second layers 1B and 2B are amorphous.
[0124] Then, the stacked layered body is annealed at 300° C. for 10 hours. The second layers 1B and 2B are crystallized by the annealing, and the crystallinity of the first layers 1A and 2A is also improved by the crystallization of the second layers 1B and 2B.
[0125] The MR ratio and RA (surface resistance) of the manufactured magnetoresistance effect element 10 were measured. The MR ratio is a measurement of the change in the resistance value of the magnetoresistance effect element 10 by monitoring the voltage applied to the magnetoresistance effect element 10 with a voltmeter while a constant current is passed along the stacking direction of the magnetoresistance effect element 10 and a magnetic field is scanned from the outside to the magnetoresistance effect element 10. The value is calculated by the following formula based on the resistance values obtained by measuring the resistance value when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are parallel and the resistance value when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are antiparallel. The measurement of the MR ratio was performed at 300K (room temperature).
[0126] MR ratio (%) = (R AP -R P ) / R P ×100
[0127] R P is the resistance value when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are parallel, R AP It is the resistance value when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are antiparallel.
[0128] RA is the resistance R when the magnetization directions of the first ferromagnetic layer 1 and the second ferromagnetic layer 2 are parallel. p The product is obtained by multiplying the area A of the magnetoresistive element 10 in the in-plane direction.
[0129] The MR ratio of the magnetoresistive element 10 according to Example 1 is 11%, and the RA is 0.8 Ω·μm. 2 .
[0130] (Example 2)
[0131] The difference between Example 2 and Example 1 is that the first layer 1A, 2A is composed of Co2FeGa 0.6 Ge 0.8 The Co composition ratio of the Co-based Heusler alloy constituting the first layers 1A, 2A according to Example 2 is smaller than the stoichiometric composition ratio.
[0132] The MR ratio of the magnetoresistive element 10 according to Example 2 is 14%, and the RA is 0.09 Ω·μm. 2 .
[0133] (Example 3)
[0134] The difference between Example 3 and Example 1 is that the composition of the second layer 1B, 2B is (Co 0.2 Fe 0.6 B 0.2 ) 0.9 Ta 0.1 In the second layers 1B and 2B of Example 3, the Fe content is higher than the Co content.
[0135] The MR ratio of the magnetoresistive element 10 according to Example 3 is 13%, and the RA is 0.07 Ω·μm. 2 .
[0136] (Example 4)
[0137] The difference between Example 4 and Example 1 is that the first layers 1A and 2A are composed of Co2FeGa 0.6 Ge 0.8 The composition of the second layer 1B and 2B is (Co 0.2 Fe 0.6 B 0.2 ) 0.9 Ta 0.1 The Co composition ratio of the Co-based Heusler alloy constituting the first layers 1A and 2A according to Example 4 is lower than the stoichiometric composition ratio. The Fe content of the second layers 1B and 2B is higher than the Co content.
[0138] The MR ratio of the magnetoresistive element 10 according to Example 4 is 16%, and the RA is 0.08 Ω·μm. 2 .
[0139] (Example 5)
[0140] The difference between Example 5 and Example 1 is that the first layers 1A and 2A are composed of Co2FeGa 0.6 Ge 0.8 The composition of the second layer 1B and 2B is (Co 0.2 Fe 0.65 B 0.15 ) 0.85 Ta 0.15 The Co composition ratio of the Co-based Heusler alloy constituting the first layers 1A and 2A according to Example 5 is lower than the stoichiometric composition ratio. The Fe content of the second layers 1B and 2B is higher than the Co content. In Example 5, the Ta content is higher than that of Examples 1 to 4.
[0141] The MR ratio of the magnetoresistive element 10 according to Example 5 is 18%, and the RA is 0.11 Ω·μm. 2 .
[0142] (Example 6)
[0143] The difference between Example 6 and Example 1 is that the first layers 1A and 2A are composed of Co2FeGa 0.6 Ge 0.8 The composition of the second layer 1B and 2B is (Co 0.39 Fe 0.19 Ga 0.12 Ge 0.15 B 0.15 ) 0.85 Ta 0.15 The Co-based Heusler alloy constituting the first layer 1A, 2A and the (Co 0.39 Fe 0.19 Ga 0.12 Ge 0.15 B 0.15 ) 0.85 Ta 0.15 The Co composition ratio is less than the stoichiometric composition ratio.
[0144] The MR ratio of the magnetoresistive element 10 according to Example 6 is 21%, and the RA is 0.13 Ω·μm. 2 .
[0145] (Comparative Example 1)
[0146] The difference between Comparative Example 1 and Example 1 is that the composition of the second layers 1B and 2B is (Co 0.4 Fe 0.4 B 0.2 ) 0.93 Ta 0.07 Since the Ta content of the second layers 1B and 2B is low, the atoms in the second layers 1B and 2B are not mixed sufficiently, and the second layers 1B and 2B remain amorphous. The first layers 1A and 2A of Comparative Example 1 are crystallized, but the crystallinity is lower than that of Example 1.
[0147] The magnetoresistance effect element 10 according to Comparative Example 1 has an MR ratio of 5% and an RA of 0.08 Ω·μm. 2 .
[0148] (Comparative Example 2)
[0149] The difference between Comparative Example 2 and Example 2 is that the composition of the second layer 1B, 2B is (Co 0.4 Fe 0.4 B 0.2 ) 0.93 Ta 0.07 Since the Ta content of the second layers 1B and 2B is low, the atoms in the second layers 1B and 2B are not mixed sufficiently, and the second layers 1B and 2B remain amorphous. The first layers 1A and 2A of Comparative Example 2 are crystallized, but the crystallinity is lower than that of Example 2.
[0150] The MR ratio of the magnetoresistive element 10 according to Comparative Example 2 was 7%, and the RA was 0.08 Ω·μm. 2 .
[0151] The results of Examples 1 to 6 and Comparative Examples 1 to 2 are summarized in Table 1 below.
[0152]
Table 1
[0153]
[0154] Description of Reference Numerals
[0155] 1…first ferromagnetic layer; 1A, 2A, 11A, 12A…first layer; 1B, 2B, 11B, 12B…second layer; 2…second ferromagnetic layer; 3, 13…non-magnetic layer; 4, 5…boron absorption layer; 6, 7…buffer layer; 8…spin-orbit torque wiring; 10, 10A, 10B, 10C…magnetoresistance effect element; 21…resistance measuring device; 22…power supply; 23…measuring unit; 24…first fixed magnetization layer; 25…second fixed magnetization layer; 26…DC power supply; 27…inductor; 28…capacitor; 29…output port; 30, 31…wiring; 100, 101, 102…magnetic recording element; 103…magnetic wall moving element; 104…high-frequency device; DW…magnetic wall; MD1…first magnetic region; MD2…second magnetic region; Sub…substrate.
Claims
1. A magnetoresistance effect element, characterized in that: include: a first ferromagnetic layer, a second ferromagnetic layer, and a non-magnetic layer located between the first ferromagnetic layer and the second ferromagnetic layer, At least one of the first ferromagnetic layer and the second ferromagnetic layer has a first layer and a second layer in order from a side close to the non-magnetic layer, The first layer includes a crystallized Co-based Heusler alloy. At least a portion of the second layer is crystallized and contains a ferromagnetic element and a boron element. The Co-based Heusler alloy is recorded as CoYZ or Co2YZ according to the stoichiometric composition. The Co composition ratio of the Co-based Heusler alloy is lower than the stoichiometric composition ratio.
2. A magnetoresistance effect element, characterized in that: include: a first ferromagnetic layer, a second ferromagnetic layer, and a non-magnetic layer located between the first ferromagnetic layer and the second ferromagnetic layer, At least one of the first ferromagnetic layer and the second ferromagnetic layer has a first layer and a second layer in order from a side close to the non-magnetic layer, The first layer includes a crystallized Co-based Heusler alloy. At least a portion of the second layer is crystallized and contains a ferromagnetic element and a boron element. The second layer is crystallized CoFeB-A. In the second layer, the content of Fe is greater than the content of Co.
3. The magnetoresistance effect element according to claim 1 or 2, characterized in that: The Co-based Heusler alloy is denoted as Co2Y α Z β , The Y is one or more elements selected from the group consisting of Fe, Mn, and Cr, The Z is one or more elements selected from the group consisting of Si, Al, Ga, and Ge, Satisfies α+β>2.
4. A magnetoresistance effect element, characterized in that: include: a first ferromagnetic layer, a second ferromagnetic layer, and a non-magnetic layer located between the first ferromagnetic layer and the second ferromagnetic layer, At least one of the first ferromagnetic layer and the second ferromagnetic layer has a first layer and a second layer in order from a side close to the non-magnetic layer, The first layer includes a crystallized Co-based Heusler alloy. At least a portion of the second layer is crystallized and contains a ferromagnetic element and a boron element. The Co-based Heusler alloy is denoted as Co2Y α Z β , The Y is one or more elements selected from the group consisting of Fe, Mn, and Cr, The Z is one or more elements selected from the group consisting of Si, Al, Ga, and Ge, Satisfies α+β>2.
5. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: The first ferromagnetic layer and the second ferromagnetic layer both have the first layer and the second layer.
6. The magnetoresistance effect element according to claim 2 or 4, characterized in that: The Co-based Heusler alloy is recorded as CoYZ or Co2YZ according to the stoichiometric composition. The Co composition ratio of the Co-based Heusler alloy is lower than the stoichiometric composition ratio.
7. The magnetoresistance effect element according to claim 1 or 4, characterized in that: The second layer is crystallized CoFeB-A. In the second layer, the content of Fe is greater than the content of Co.
8. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: The first layer and the second layer are lattice matched.
9. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: A boron absorption layer is provided which is in contact with a surface of the second layer which is away from the non-magnetic layer. The boron absorption layer includes any element selected from the group consisting of Ti, V, Cr, Cu, Zn, Zr, Mo, Ru, Pd, Ta, W, Ir, Pt, and Au.
10. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: The Co-based Heusler alloy has an L21 structure or a B2 structure.
11. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: A buffer layer is provided at least one of between the first ferromagnetic layer and the non-magnetic layer and between the second ferromagnetic layer and the non-magnetic layer. The buffer layer contains NiAl alloy or Ni.
12. The magnetoresistance effect element according to claim 11, wherein The thickness of the buffer layer is less than 0.63 nm.
13. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: The nonmagnetic layer includes a metal or an alloy of any element selected from the group consisting of Cu, Au, Ag, Al, and Cr.
14. The magnetoresistance effect element according to any one of claims 1, 2 and 4, characterized in that: Also having a substrate, The substrate is a base on which the first ferromagnetic layer, the second ferromagnetic layer and the non-magnetic layer are stacked. The substrate is in an amorphous state.