Method for preparing metal oxide catalyst for oxygen evolution reaction

By using nano-scale inorganic oxide cores to deposit a thin shell of platinum group metal oxides in water electrolytic catalysts, the problem of high cost of precious metal catalysts in PEM-WE and AEM-WE is solved, and high efficiency and stability are achieved The water electrolysis reaction reduces the overall cost of the battery stack.

CN118984733APending Publication Date: 2024-11-19UOP LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033201.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-10
Filing Date
2023-05-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing proton exchange membrane water electrolysis (PEM-WE) and anion exchange membrane water electrolysis (AEM-WE) technologies, the high capital cost of the battery stack, the expensiveness of precious metal catalysts and membrane materials are the main challenges, especially membrane hydroxyl groups. Ion conductivity and stability and catalyst integration problems are insufficient.

Method used

Using the method of depositing a substantially continuous thin shell of platinum group metal oxide on the nanoscale inorganic oxide core, a high-active and stable water electrolytic catalyst is formed by heat treatment to reduce the load of precious metals, and heat treatment is used to prepare high-quality Catalyst, reduces the size and cost of catalyst particles.

Benefits of technology

It realizes efficient and stable redox reaction performance in PEM-WE and AEM-WE, reduces the load of precious metals, improves the activity and stability of the catalyst, reduces production costs, and improves the efficiency of the water electrolysis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984733A_ABST
    Figure CN118984733A_ABST
Patent Text Reader

Abstract

Highly active and stable water electrolysis catalysts with reduced noble metal loading and methods of making the same are described. The method involves depositing a substantially continuous platinum group metal (PGM)-based precursor thin shell layer on a nanoscale inorganic oxide core to form a coated inorganic oxide core. The coated inorganic oxide core is heated in the presence of a template to convert the substantially continuous PGM-based precursor thin shell layer to a substantially continuous PGM oxide thin shell layer. The template is then removed, forming a water electrolysis catalyst comprising a nanoscale inorganic oxide core having a substantially continuous PGM oxide thin shell layer. The water electrolysis catalyst comprises less than 30% by weight of PGM oxide.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority declaration

[0002] This application claims priority to U.S. Application No. 17 / 662,677, filed on May 10, 2022, which is incorporated herein in its entirety.

[0003] Hydrogen plays an important role in the path towards an environmentally friendly, low-carbon energy structure as an energy carrier for grid balancing or power-to-gas and power-to-liquid processes. Water electrolysis produces high-quality hydrogen by electrochemically decomposing water into hydrogen and oxygen; the reaction is given by the following equation 1. The water electrolysis process is an endothermic process, and electricity is the energy source. When the method is operated by renewable energy such as wind, solar or geothermal energy, water electrolysis has a zero carbon footprint. The main water electrolysis technologies include alkaline electrolysis, proton exchange membrane (PEM) water electrolysis (such as Figure 1 PEM-WE as shown), anion exchange membrane (AEM) water electrolysis (such as Figure 2 AEM-WE) and solid oxide water electrolysis as shown.

[0004] like Figure 1 As shown, in the PEM-WE system 100, the anode 105 and the cathode 110 are separated by a solid PEM electrolyte 115, such as the one sold under the trademark A fluorinated copolymer based on sulfonated tetrafluoroethylene sold by the Chemours company. The anode and cathode catalysts typically comprise IrO2 and Pt, respectively. At the positively charged anode 105, pure water 120 is oxidized to produce oxygen 125, electrons (e - ) and protons; the reaction is given by Equation 2. Protons are transported from the anode 105 to the cathode 110 through the proton-conducting PEM 115. At the negatively charged cathode 110, a reduction reaction occurs in which electrons from the cathode 110 are given to protons to form hydrogen 130; the reaction is given by Equation 3. The PEM 115 not only conducts protons from the anode 105 to the cathode 110, but also separates the H2 gas 130 and O2 gas 125 produced in the water electrolysis reaction. PEM water electrolysis is one of the advantageous methods for converting renewable energy into high-purity hydrogen, with the advantages of compact system design at high pressure difference, high current density, high efficiency, fast response, small footprint, low temperature (20°C-90°C) operation, and high-purity oxygen byproduct. However, one of the main challenges of PEM water electrolysis is the high capital cost of the cell stack, including expensive acid-resistant stack hardware (such as Pt-coated Ti bipolar plates), expensive precious metal catalysts required for electrodes, and expensive PEMs.

[0005] Water electrolysis reaction: 2H2O→2H2+O2 (1)

[0006] Anodic oxidation reaction of PEM-WE: 2 H2O→O2+4 H + +4 e - (2)

[0007] Cathodic reduction reaction of PEM-WE: 2 H + +2 e - →H2 (3)

[0008] AEM-WE is a developing technology. Figure 2 As shown, in the AEM-WE system 200, the anode 205 and the cathode 210 are separated by a solid AEM electrolyte 215. Typically, a water feed 220 with an added electrolyte (such as diluted KOH or K2CO3 or deionized water) is fed to the cathode side. The anode and cathode catalysts typically include Ni-based or Ni alloy catalysts that do not contain platinum group metals. At the negatively charged cathode 210, water is reduced to form hydrogen 225 and hydroxyl ions by adding four electrons; the reaction is given by Equation 4. The hydroxyl ions diffuse from the cathode 210 to the anode 205 through the AEM 215 that conducts hydroxyl ions. At the positively charged anode 205, the hydroxyl ions recombine into water and oxygen 230; the reaction is given by Equation 5. The AEM 215 not only conducts hydroxyl ions from the cathode 210 to the anode 205, but also separates the H2 225 and O2 230 produced in the water electrolysis reaction. The AEM 215 allows the production of hydrogen 225 with a very high purity of at least 99.9% at high pressures of up to 35 bar.

[0009] Cathodic reduction reaction of AEM-WE: 4 H2O+4 e - →2 H2+4 OH (4)

[0010] Anodic oxidation reaction of AEM-WE: 4 OH - →2 H2O+O2+4 e - (5)

[0011] AEM-WE has advantages over PEM-WE because it allows the use of cheaper platinum group metal-free catalysts, such as Ni and Ni alloy catalysts. In addition, much cheaper stainless steel bipolar plates can be used in the gas diffusion layer (GDL) of AEM-WE instead of the expensive Pt-coated Ti bipolar plates currently used in PEM-WE. However, the biggest obstacle to the development of AEM systems is the membrane hydroxyl ion conductivity and stability, as well as the lack of understanding of how to integrate catalysts into AEM systems. Research on AEM-WE in the literature focuses on developing electrocatalysts, AEMs, and understanding the operating mechanism, with the general goal of obtaining efficient, low-cost and stable AEM-WE technology.

[0012] Fuel cells, which are the next generation of clean energy, convert the energy of chemical reactions such as oxidation / reduction redox reactions of hydrogen and oxygen into electrical energy. The three main types of fuel cells are alkaline electrolyte fuel cells, polymer electrolyte membrane fuel cells, and solid oxide fuel cells. Polymer electrolyte membrane fuel cells may include proton exchange membrane fuel cells (PEM-FC), anion exchange membrane fuel cells (AEM-FC), and direct methanol fuel cells. PEM-FC uses PEM to conduct protons from the anode to the cathode, and it also separates H2 gas and O2 gas to prevent gas crossover. AEM-FC uses AEM to conduct OH - It conducts from cathode to anode, and it also separates H2 gas and O2 gas to prevent gas crossover.

[0013] The anode in an electrochemical cell is an electrode whose main reaction is oxidation (e.g., a water oxidation / oxygen evolution reaction electrode for a water electrolyzer, or a hydrogen oxidation electrode for a fuel cell). The cathode in an electrochemical cell is an electrode whose main reaction is reduction (e.g., a proton reduction / hydrogen evolution reaction electrode for a water electrolyzer, or an oxygen reduction electrode for a fuel cell). The membrane is one of the key materials constituting an electrolyzer or a fuel cell, and is an important driving factor for safety and performance. Some important properties of membranes for fuel cells and membrane electrolysis include high conductivity, high ion permeability, high ion exchange capacity (for ion exchange membranes), high ion / H2 and O2 selectivity (low H2 and O2 permeability / crossover), low price, low area resistance to minimize efficiency loss caused by ohmic polarization, high tolerance to oxidation and reduction conditions, chemical inertness, high thermal stability, high proton conductivity, and high mechanical strength (thickness, low swelling) over a wide pH range.

[0014] For PEM water electrolysis and PEM-FC and AEM water electrolysis and AEM-FC to have widespread applications in renewable energy systems, significant advances are needed in cost-effective, high-performance, stable catalysts, membrane materials, and other cell stack components. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The patent or application file contains at least one color photograph. Copies of this patent or patent application publication with color photographs will be provided by the Office upon request and payment of the necessary fee.

[0016] Figure 1 is a diagram of one embodiment of a PEM-WE cell.

[0017] Figure 2 is a diagram of one embodiment of an AEM-WE battery.

[0018] Figure 3A and Figure 3Bis a scanning transmission electron microscopy (STEM) image of a substantially continuous IrOx / TiO2 core-shell catalyst.

[0019] Figure 4 Is discontinuous IrO x / TiO2 catalyst STEM image.

[0020] Figure 5 is a graph comparing the polarization curves of individual water electrolysis cells.

[0021] Figure 6 is a graph comparing the high frequency resistance (HFR) of a single water electrolysis cell versus current density. DETAILED DESCRIPTION

[0022] Novel methods have been developed to prepare catalysts for the oxygen evolution reaction (OER) that can be used in PEM or AEM water electrolyzers (WE). Using these methods, highly active and stable catalysts with reduced noble metal loadings can be produced. The new catalysts show improved OER performance compared to commercially available IrO2 catalysts.

[0023] One aspect is a method for preparing a water electrolysis catalyst. In one embodiment, the method includes depositing a substantially continuous platinum group metal (PGM)-based precursor thin shell layer on a nanoscale inorganic oxide core to form a coated inorganic oxide core; heating the coated inorganic oxide core in the presence of a template to convert the substantially continuous PGM-based precursor thin shell layer into a substantially continuous PGM oxide thin shell layer; and removing the template to form a water electrolysis catalyst comprising a nanoscale inorganic oxide core having a substantially continuous PGM oxide thin shell layer, wherein the water electrolysis catalyst comprises less than 30% by weight of PGM oxide. The PGM oxide includes PGM oxide nanoparticles, PGM oxide nanoparticle aggregates, or a combination thereof. "Substantially continuous" means that more than 90% of the surface of the nanoscale inorganic oxide core is covered by a PGM-based precursor thin shell layer or a PGM oxide thin shell layer, and the distance between a PGM oxide nanoparticle and the nearest PGM oxide nanoparticle within the shell layer is less than 5nm. The substantially continuous thin shell layer has a thickness of less than 10 nm, or less than 7 nm, or in the range of 0.1 nm to 10 nm, or 1 nm to 7 nm. The nanoscale inorganic oxide core particles have a size in the range of 10 nm to 500 nm, or 10 nm to 200 nm, or 10 nm to 50 nm.

[0024] A substantially continuous thin layer of a platinum group metal-based precursor is deposited on a nanoscale non-conductive inorganic oxide support such as TiO2, WO3, etc., thereby forming a coated inorganic oxide core. The solid coated inorganic oxide obtained from the first step is heat treated in the presence of a template to produce a conductive nanoscale material without particle aggregation.

[0025] The thermal treatment comprises heating the coated inorganic oxide core at a temperature in the range of 250° C. to 600° C., or 300° C. to 550° C., or 350° C. to 450° C., for a time in the range of 0.5 hour to 12 hours, or 0.5 hour to 6 hours, or 1 hour to 3 hours. The thermal treatment converts the substantially continuous PGM precursor thin shell layer into a substantially continuous PGM oxide thin shell layer.

[0026] The template is removed by a washing process to form a water electrolysis catalyst, which comprises a nanoscale inorganic oxide core having a substantially continuous thin shell of PGM oxide. In some embodiments, the washing process involves using deionized water to wash off the template. In some embodiments, the washing process involves using deionized water and then using an organic solvent. Suitable organic solvents for washing processes include but are not limited to alcohols such as methanol, ethanol, isopropanol, 1-propanol, acetone, ethers such as dimethyl ether, hydrocarbon solvents such as n-heptane, n-hexane or a combination thereof. The water electrolysis catalyst comprises less than 30% by weight of PGM oxide. In some embodiments, the water electrolysis catalyst comprises less than 25% by weight, or less than 20% of PGM oxide.

[0027] In some embodiments, the coated inorganic oxide core is dried in a vacuum oven at a temperature in the range of 15°C to 100°C, or 20°C to 60°C, or 20°C to 40°C, and the dried coated inorganic oxide core is mixed with the template before heating the coated inorganic oxide core.

[0028] The template can be an inorganic template or an organic template. Suitable inorganic templates include, but are not limited to, NaNO3, LiNO3, KNO3, Mg(NO3)2, Ca(NO3)2, NaCl, KCl, or a combination thereof. Suitable organic templates include, but are not limited to, citric acid, malic acid, ascorbic acid, glycerol, ethylene glycol, triethylene glycol, polyethylene oxide, polyethylene glycol, polyvinyl alcohol, poly(acrylic acid), poly(malic acid), poly(lactic acid), or a combination thereof.

[0029] Suitable PGMs include, but are not limited to, platinum, iridium, ruthenium, gold, rhodium, palladium, osmium, or combinations thereof.

[0030] Suitable nanoscale inorganic oxide cores include, but are not limited to, titanium dioxide, tungsten trioxide, molybdenum trioxide, aluminum oxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or combinations thereof.

[0031] Using this method, supported metal oxide catalysts with high conductivity, activity and stability for OER in PEM-WE cell tests were prepared. The synthesis of prior art water electrolysis catalysts does not use templates during thermal treatment. However, the use of templates (whether inorganic or organic) is highly beneficial for producing small catalyst particles, which allows the preparation of high-quality catalyst coated membranes (CCMs) for water electrolysis applications.

[0032] The use of supports in OER catalysts offers several benefits. The noble metal oxides loaded on CCMs to achieve the target water electrolysis performance are reduced due to the much smaller and more active catalytic sites. In addition, the performance is stable due to the strong support / active site interactions. For example, catalysts produced using this method show superior performance compared to commercial IrO2 catalysts with only half the IrO2 loading.

[0033] Another aspect is a water electrolysis catalyst. In one embodiment, the water electrolysis catalyst comprises: a nanoscale inorganic oxide core having a substantially continuous thin shell layer of a platinum group metal (PGM) oxide, wherein the water electrolysis catalyst comprises less than 30 wt% of the PGM oxide.

[0034] In some embodiments, the water electrolysis catalyst comprises less than 25 wt % PGM oxide, or less than 20 wt % PGM oxide.

[0035] In some embodiments, the PGM includes platinum, iridium, ruthenium, gold, rhodium, palladium, osmium, or a combination thereof.

[0036] In some embodiments, the PGM is iridium or a combination of iridium and ruthenium.

[0037] In some embodiments, the nanoscale inorganic oxide core includes titanium dioxide, tungsten trioxide, molybdenum trioxide, aluminum oxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or combinations thereof.

[0038] In some embodiments, the nanoscale inorganic oxide core comprises titanium dioxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or combinations thereof.

[0039] In some embodiments, the distance between one PGM oxide nanoparticle and the nearest neighboring PGM oxide nanoparticle within the shell layer is less than 5 nm and the thickness of the thin shell layer is less than 10 nm.

[0040] In some embodiments, the thickness of the thin shell layer is less than 7 nm.

[0041] Example

[0042] Example 1. Synthesis of continuous IrOx / TiO2 core-shell catalyst

[0043] A 200 mg sample of IrCl3·xH2O was mixed with 10 mL of water and ultrasonicated at room temperature for 30 minutes to ensure complete dissolution. A 253 mg amount of TiO2 (56 m 2 / g) was added to the Ir solution, and the mixture was ultrasonicated for another 30 minutes. The mixture was heated to 70°C in a water bath, and the pH was adjusted to 11.00 using an appropriate amount of 0.66M NaOH aqueous solution. The system was kept at 70°C for another 16 hours. The blue solid was recovered after centrifugation, washed three times with water and once with methanol. The recovered solid was dried and mixed with 4.95g NaNO3 and ground thoroughly. It was heated at 365°C for 1 hour, and then the temperature was reduced to 50°C. The recovered solid was then washed with a large amount of deionized water and dried to form a substantially continuous IrO x / TiO2 core-shell catalyst. The substantially continuous IrO x The Ir loading of the TiO2 core-shell catalyst was 22.0 wt%. A substantially continuous IrO2 layer with an average thickness of <7 nm was formed on the TiO2 core. x The thin shell can be seen from the scanning transmission electron microscopy (STEM) image in FIG3 .

[0044] Comparative Example 1. Discontinuous IrO x Synthesis of TiO2 catalyst

[0045] A 200 mg sample of IrCl3·xH2O was mixed with 10 mL of isopropanol and then with 253 mg of TiO2. After ultrasonic treatment at room temperature for 30 minutes, 4.95 g of NaNO3 was added to the mixture. After the mixture was dried at 70°C to remove all liquid, the solid was thoroughly ground at room temperature. The solid was then calcined at 365°C for 1 hour. The solid was washed with plenty of water and dried. It was determined that the coating was a discontinuous IrO2 coating on the TiO2 particles. x The discontinuous aggregation of IrO2 on TiO2 can be obtained from Figure 4 As can be seen in the STEM image.

[0046] Example 2. Continuous IrOx / TiO2 core-shell catalyst and discontinuous IrO x Water electrolysis performance of / TiO2 catalyst

[0047] Continuous IrOx / TiO2 core-shell catalyst and discontinuous IrO x The water electrolysis performance of the IrOx / TiO2 catalysts was evaluated at 80°C and atmospheric pressure using a single water electrolysis cell comprising a catalyst coated membrane (CCM) using a continuous IrOx / TiO2 core-shell catalyst (abbreviated as continuous IrOx / TiO2 core-shell catalyst CCM) and a catalyst coated membrane (CCM) using a discontinuous IrOx / TiO2 core-shell catalyst.x / TiO2 catalyst coated membrane (abbreviated as IrOx / TiO2 catalyst CCM).

[0048] The continuous IrOx / TiO2 core-shell catalyst CCM containing the continuous IrOx / TiO2 core-shell catalyst is prepared by using the continuous IrOx / TiO2 core-shell catalyst as an oxygen evolution reaction (OER) catalyst for the anode and coating the catalyst on a membrane. The continuous IrOx / TiO2 core-shell catalyst ink for spraying is prepared by mixing the catalyst and (perfluorinated sulfonic acid ionomer based on tetrafluoroethylene) ionomer (5 wt% alcohol solution). The mixture was finely dispersed using an ultrasonic bath. The ionomer content is controlled as the catalyst and The catalyst ink was sprayed onto the On one side of the FS-990-PK (polyetheretherketone reinforced perfluorinated cation exchange membrane) membrane. The continuous IrOx / TiO2 core-shell catalyst loading was 0.3 mg / cm 2 The continuous IrOx / TiO2 core-shell catalyst CCM was sandwiched between Pt-coated carbon paper (as the cathode porous transport layer coated with hydrogen evolution reaction (HER) catalyst) and Pt-coated Ti felt (as the anode porous transport layer) to form a continuous IrOx / TiO2 core-shell catalyst-based membrane electrode assembly. The test cell was installed using the continuous IrOx / TiO2 core-shell catalyst-based membrane electrode assembly.

[0049] Contains discontinuous IrO x Discontinuous IrO / TiO2 catalyst x / TiO2 catalyst CCM can be achieved by using discontinuous IrO x / TiO2 catalyst was used as an OER catalyst for the anode and was prepared by coating the catalyst on the membrane. The catalyst and Ionomer (5 wt % in alcohol) was used to prepare discontinuous IrO x / TiO2 catalyst ink. The mixture was finely dispersed using an ultrasonic bath. The ionomer content is controlled as the catalyst and The catalyst ink was sprayed onto the On one side of the FS-990-PK membrane. Discontinuous IrO x / TiO2 catalyst loading is 0.35mg / cm 2 . Will be based on discontinuous IrO xThe CCM of IrO2 / TiO2 catalyst was sandwiched between Pt-coated carbon paper (as the cathode porous transport layer coated with HER catalyst) and Pt-coated Ti felt (as the anode porous transport layer) to form a discontinuous IrO x / TiO2 catalyst-based membrane electrode assembly. Using discontinuous IrO x / TiO2 catalyst-based membrane electrode assembly installed in the test cell.

[0050] Proton exchange membrane (PEM) water electrolysis test station (Scribner 600 electrolyzer test system) is used to evaluate continuous IrO x / TiO2 core-shell catalysts CCM and discontinuous IrO x / TiO2 catalyst CCM has an active membrane area of ​​5cm 2 The water electrolysis performance in a single electrolyzer cell of 1000 mW was measured. The test station included an integrated power supply, potentiostat, impedance analyzer for electrochemical impedance spectroscopy (EIS) and high frequency resistance (HFR), and real-time sensors for product flow rate and permeation monitoring. The test was performed at 80 °C and at atmospheric pressure. Ultrapure water was supplied to the anode of the cell at a flow rate of 100 mL / min. The cell was heated to 80 °C and charged at 200 mA / cm 2 Keep at 1A / cm for 1 hour 2 These steps are counted together as one conditioning cycle. After conditioning, a polarization curve is plotted (each data point is held for 1 minute), as shown in Figure 5 shown. Figure 6 The continuous IrOx / TiO2 core-shell catalyst CCM and the discontinuous IrO x / TiO2 catalyst CCM without HFR voltage versus current density. Figure 5 It can be seen that the continuous IrOx / TiO2 core-shell catalyst CCM has a commercially feasible 1.5 A / cm 2 or higher current density, showing a higher performance than discontinuous IrO x The much lower cell voltage of the CCM with IrOx / TiO2 core-shell catalyst indicates that the continuous IrOx / TiO2 core-shell catalyst CCM has better performance than the discontinuous IrOx / TiO2 core-shell catalyst. x / TiO2 catalyst CCM higher cell efficiency. Figure 6 The results show that the continuous IrOx / TiO2 core-shell catalyst CCM at 1.5A / cm 2 or higher current density than discontinuous IrO x / TiO2 catalyst CCM has a lower HFR-free voltage, which contributes to the lower cell voltage of the continuous IrOx / TiO2 core-shell catalyst CCM.

[0051] As used herein, the term means within 10%, or within 5%, or within 1% of the value.

[0052] Although at least one exemplary embodiment has been presented in the aforementioned specific embodiments of the present invention, it should be understood that there are a large number of variations. It should also be understood that an exemplary embodiment or multiple exemplary embodiments are only examples and are not intended to limit the scope, applicability or construction of the present invention in any way. On the contrary, the aforementioned specific embodiments will provide a convenient roadmap for implementing the exemplary embodiments of the present invention for those skilled in the art. It should be understood that, without departing from the scope of the present invention as set forth in the appended claims, various changes can be made to the function and layout of the elements described in the exemplary embodiments.

[0053] Specific implementation plan

[0054] While the following is described in conjunction with specific embodiments, it should be understood that this description is intended to illustrate and not to limit the scope of the foregoing description and the appended claims.

[0055] The first embodiment of the present invention is a method for preparing a water electrolysis catalyst, comprising depositing a substantially continuous platinum group metal (PGM)-based precursor thin shell layer on a nanoscale inorganic oxide core to form a coated inorganic oxide core; heating the coated inorganic oxide core in the presence of a template to convert the substantially continuous PGM-based precursor thin shell layer into a substantially continuous PGM oxide thin shell layer; and removing the template to form a water electrolysis catalyst comprising a nanoscale inorganic oxide core having a substantially continuous PGM oxide thin shell layer, wherein the water electrolysis catalyst comprises less than 30 wt % of PGM oxide. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the template comprises an inorganic template or an organic template. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the inorganic template comprises NaNO3, LiNO3, KNO3, Mg(NO3)2, Ca(NO3)2, NaCl, KCl or a combination thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the organic template comprises citric acid, malic acid, ascorbic acid, glycerol, ethylene glycol, triethylene glycol, polyethylene oxide, polyethylene glycol, polyvinyl alcohol, poly(acrylic acid), poly(malic acid), poly(lactic acid), or a combination thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, further comprising drying the coated inorganic oxide core; mixing the dried coated inorganic oxide core with the template before heating the coated inorganic oxide core. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the PGM comprises platinum, iridium, ruthenium, gold, rhodium, palladium, osmium, or a combination thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the nanoscale inorganic oxide core comprises titanium dioxide, tungsten trioxide, molybdenum trioxide, aluminum oxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or a combination thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the water electrolysis catalyst comprises less than 25 wt % of PGM oxide. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the first embodiment in this paragraph, wherein the water electrolysis catalyst comprises less than 20 wt % of PGM oxide.

[0056] A second embodiment of the present invention is a water electrolysis catalyst comprising a nanoscale inorganic oxide core having a substantially continuous thin shell layer of platinum group metal (PGM) oxide, wherein the water electrolysis catalyst comprises less than 30 wt % of PGM oxide. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the PGM comprises platinum, iridium, ruthenium, gold, rhodium, palladium, osmium or a combination thereof. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the PGM is iridium or a combination of iridium and ruthenium. An embodiment of the present invention is one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the nanoscale inorganic oxide core comprises titanium dioxide, tungsten trioxide, molybdenum trioxide, aluminum oxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide or a combination thereof. Embodiments of the present invention are one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the nanoscale inorganic oxide core comprises titanium dioxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or a combination thereof. Embodiments of the present invention are one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the water electrolysis catalyst comprises less than 25% by weight of PGM oxide. Embodiments of the present invention are one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the water electrolysis catalyst comprises less than 20% by weight of PGM oxide. Embodiments of the present invention are one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the distance between a PGM oxide nanoparticle in the shell layer and the nearest adjacent PGM oxide nanoparticle is less than 5nm and the thickness of the thin shell layer is less than 10nm. Embodiments of the present invention are one, any or all of the previous embodiments in this paragraph up to the second embodiment in this paragraph, wherein the thickness of the thin shell layer is less than 7nm.

[0057] Although there is no further detailed description, it is believed that those skilled in the art can utilize the present invention to the greatest extent by using the foregoing description and can easily determine the essential characteristics of the present invention without departing from the spirit and scope of the present invention to make various changes and modifications of the present invention and adapt it to various usages and conditions. Therefore, the aforementioned preferred specific embodiments should be understood as merely illustrative and not to limit the rest of the present disclosure in any way, and are intended to cover various modifications and equivalent arrangements included within the scope of the appended claims.

[0058] In the foregoing, all temperatures are set forth in degrees Celsius and all parts and percentages are by weight unless otherwise indicated.

Claims

1. A method for preparing a water electrolysis catalyst, the method for preparing a water electrolysis catalyst comprising: depositing a substantially continuous thin shell layer of a platinum group metal (PGM) based precursor on the nanoscale inorganic oxide core to form a coated inorganic oxide core; heating the coated inorganic oxide core in the presence of a template to convert the substantially continuous thin PGM-based precursor shell layer into a substantially continuous thin PGM oxide shell layer; as well as The template is removed to form the water electrolysis catalyst comprising the nanoscale inorganic oxide core having the substantially continuous thin PGM oxide shell layer, wherein the water electrolysis catalyst comprises less than 30 wt % of the PGM oxide. 2 . The method according to claim 1 , wherein the template comprises an inorganic template or an organic template.

3. The method of claim 2, wherein the inorganic template comprises NaNO3, LiNO3, KNO3, Mg(NO3)2, Ca(NO3)2, NaCl, KCl, or a combination thereof.

4. The method of claim 2, wherein the organic template comprises citric acid, malic acid, ascorbic acid, glycerol, ethylene glycol, triethylene glycol, polyethylene oxide, polyethylene glycol, polyvinyl alcohol, poly(acrylic acid), poly(malic acid), poly(lactic acid), or a combination thereof.

5. The method according to any one of claims 1 to 4, further comprising: drying the coated inorganic oxide core; as well as Prior to heating the coated inorganic oxide core, the dried coated inorganic oxide core is mixed with the template.

6. The method of any one of claims 1 to 5, wherein the PGM comprises platinum, iridium, ruthenium, gold, rhodium, palladium, osmium, or a combination thereof.

7. The method according to any one of claims 1 to 6, wherein the nanoscale inorganic oxide core comprises titanium dioxide, tungsten trioxide, molybdenum trioxide, aluminum oxide, tungsten-doped titanium dioxide, niobium-doped titanium dioxide, or a combination thereof.

8. The method of any one of claims 1 to 7, wherein the water electrolysis catalyst comprises less than 25 wt% of the PGM oxide.

9. The method of any one of claims 1 to 8, wherein the water electrolysis catalyst comprises less than 20 wt% of the PGM oxide.

10. A water electrolysis catalyst, comprising: A nanoscale inorganic oxide core having a substantially continuous thin shell layer of a platinum group metal (PGM) oxide, wherein the water electrolysis catalyst comprises less than 30% by weight of the PGM oxide.