Bulk silver powder, method for producing same, and conductive paste

By using specially made block silver powder and its manufacturing method, the problems of high line resistance and high line breakage rate in thin-wire printing are solved, and the electrical wiring effect with low line resistance and low line breakage rate is achieved.

CN118984746APending Publication Date: 2024-11-19DOWA ELECTRONICS MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380026799.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-02-27
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

There is a problem that the conductive paste using spherical silver powder and sheet silver powder is high when the wire resistance becomes larger during thin-line printing, and the wire breakage rate is high.

Method used

Special block silver powder is used, characterized by the BET specific surface area of ​​less than 0.5m2/g, the average aspect ratio is 1.2 or more and less than 2.0, the ratio of the circumference to the circumference of the outer rectangle is 0.84 or more, and the circularity coefficient is 0.65 to 0.88, the shape coefficient is 1.4 to 2.6, and the production method is used to prepare a conductive paste by collision of spherical silver powder with a medium.

Benefits of technology

Electrical wiring with small line resistance and low line breakage rate is realized, the density and contact points of silver particles are improved, and the stability and reliability of thin-wire printing are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984746A_ABST
    Figure CN118984746A_ABST
Patent Text Reader

Abstract

Provided is a bulk silver powder having a BET specific surface area of 0.5 m2 / g or less, an average aspect ratio of 1.2 or more and less than 2.0 when a cross-section of 100 or more silver particles is observed, and an average value of the ratio of the circumference of the silver particles to the circumference of a circumscribed rectangle represented by formula (1) is 0.84 or more (formula (1): L / (2 * major diameter + 2 * minor diameter). Wherein L is the perimeter ([mu] m) of the silver particle, and the long diameter and the short diameter are the long side ([mu] m) and the short side ([mu] m) of a rectangle with the smallest area among rectangles circumscribed with the profile of the cross section of the silver particle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to bulk silver powder, a method for producing the bulk silver powder, and a conductive paste. Background Art

[0002] In recent years, in devices such as solar cells and semiconductors that require electrical wiring, there is a demand for thinner electrical wiring. Therefore, there is a need for a conductive paste that has low resistance and no risk of disconnection even when the electrical wiring becomes thinner.

[0003] The silver powder used in the conductive paste is generally any one of spherical silver powder and flake silver powder. The average aspect ratio of the spherical silver powder is close to 1, and its shape is nearly spherical. The flake silver powder has a flat shape, and the average aspect ratio is 3 or more, and often 6 or more. Such flake silver powder is produced, for example, by mixing spherical silver powder and a medium in a rotary ball mill or a vibrating ball mill and causing them to collide (for example, see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-254845 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] However, when fine lines are printed using a conventional conductive paste using spherical silver powder or flake silver powder, there is a problem that line resistance increases and the rate of line breakage increases.

[0009] Therefore, an object of the present invention is to provide a cuboid silver powder for a conductive paste, a method for producing the same, and a conductive paste, the conductive paste being capable of realizing electrical wiring with a small line resistance and a low line breakage rate.

[0010] Solutions for solving problems

[0011] The means for solving the above-mentioned technical problem are as follows. That is,

[0012] <1> A bulk silver powder, characterized in that the BET specific surface area is 0.5 m 2 / g or less,

[0013] When observing cross sections of 100 or more silver particles, the average aspect ratio is 1.2 or more and less than 2.0, and the average ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more.

[0014] (Formula 1): L / (2×long diameter+2×short diameter)

[0015] Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

[0016] <2> According to the above <1> The bulk silver powder has an average value of a circularity coefficient shown in the following (Formula 2) of 0.65 to 0.88.

[0017] (Equation 2): 4πS / L 2

[0018] Where S is the area of ​​the silver particles (μm 2 ), L is the circumference of the silver particle (μm).

[0019] <3> According to the above <2> The bulk silver powder has a circularity coefficient of 0.65 to 0.88, which accounts for more than 40%.

[0020] <4> According to the above <1> to <3> The bulk silver powder described in any one of the above aspects has an average value of a shape factor represented by the following (Formula 3) of 1.4 to 2.6.

[0021] (Formula 3):π(L max ) 2 / 4S

[0022] Where S is the area of ​​the silver particles (μm 2 ), L max It represents the maximum length of silver particles (μm).

[0023] <5> According to the above <4> The bulk silver powder has a shape coefficient of 1.4 to 2.6 in a proportion of more than 40%.

[0024] <6> According to the above <1> to <5> The bulk silver powder according to any one of the preceding claims, wherein the cumulative 50% particle size (D 50 ) multiplied by the BET specific surface area gives a value of 6.5E-07m 3 / g or above and 1.0E-06m 3 / g or less.

[0025] <7> According to the above <1> to <5> The bulk silver powder described in any one of the above has a BET specific surface area of ​​0.35 m 2 / g or less.

[0026] <8> A method for manufacturing bulk silver powder, characterized in that it comprises: a bulking step, wherein spherical silver powder and a medium are placed in a container, and the spherical silver powder and the medium collide with each other through the movement of the container to obtain bulk silver powder,

[0027] In the bulk silver powder, when observing cross sections of more than 100 silver particles, the average aspect ratio is 1.2 or more and less than 2.0, and the average ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more.

[0028] (Formula 1): L / (2×long diameter+2×short diameter)

[0029] Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

[0030] <9> According to the above <8> The method for manufacturing bulk silver powder, wherein the bulking process is performed without using a lubricant.

[0031] <10> A conductive paste, characterized in that it contains the above <1> to <7> The bulk silver powder described in any one of the above.

[0032] Effects of the Invention

[0033] According to the present invention, it is possible to provide a bulk silver powder for conductive paste and a method for producing the same, as well as a conductive paste that can solve the various problems mentioned above in the past and achieve the above-mentioned purpose, wherein the conductive paste can realize electrical wiring with low line resistance and low disconnection rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This diagram explains the rectangle that is circumscribed to the outline of the cross section of the silver particle and has the smallest area.

[0035] Figure 2 This is a scanning electron microscope photograph of silver powder, which explains the silver particles that are the measurement objects of the ratio of the perimeter of the particle to the perimeter of the circumscribed rectangle, the circularity coefficient, the shape factor, and the aspect ratio.

[0036] Figure 3A is a scanning electron microscope photograph of the silver powder prepared in Example 1.

[0037] Figure 3B is a scanning electron microscope photograph of the cross section of the silver powder prepared in Example 1.

[0038] Figure 4A is a scanning electron microscope photograph of the silver powder prepared in Example 2.

[0039] Figure 4B is a scanning electron microscope photograph of the cross section of the silver powder prepared in Example 2.

[0040] Figure 5Ais a scanning electron microscope photograph of the silver powder prepared in Example 3.

[0041] Figure 5B is a scanning electron microscope photograph of the cross section of the silver powder prepared in Example 3.

[0042] Fig. 6A is a scanning electron microscope photograph of the silver powder prepared in Comparative Example 1.

[0043] Figure 6B is a scanning electron microscope photograph of the cross section of the silver powder prepared in Comparative Example 1.

[0044] Fig. 7A This is a scanning electron microscope photograph of the silver powder of Comparative Example 2.

[0045] Figure 7B This is a scanning electron microscope photograph of a cross section of the silver powder of Comparative Example 2. DETAILED DESCRIPTION

[0046] (Silver powder in bulk)

[0047] The BET specific surface area of ​​the bulk silver powder of the present invention is 0.5 m 2 / g or less, the average value of the aspect ratio when observing the cross sections of 100 or more silver particles is 1.2 or more and less than 2.0, and the average value of the ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more.

[0048] (Formula 1): L / (2×long diameter+2×short diameter)

[0049] Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

[0050] In the present invention, the bulk silver powder refers to an aggregate of silver particles having a bulk shape, wherein the average aspect ratio of more than 100 silver particle cross sections observed with a scanning electron microscope is 1.2 or more and less than 2, and the average ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle is 0.84 or more. It should be noted that there is no particular limitation on the number of silver particles observed in the cross section as long as it is 100 or more. With respect to the total number of silver particles measured, the ratio (number ratio) of particles whose perimeter of the silver particles to the perimeter of the circumscribed rectangle is preferably 40% or more, and more preferably 50% or more.

[0051] <Ratio of the particle's perimeter to the perimeter of the circumscribed rectangle>

[0052] In the bulk silver powder of the present invention, the average value of the ratio of the perimeter of the silver particles represented by (Formula 1) to the perimeter of the circumscribed rectangle is 0.84 or more, preferably 0.84 or more and 1.00 or less, and more preferably 0.85 or more and 1.00 or less.

[0053] When the average value of the ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the above (Formula 1) is 0.84 or more, electric wiring with low line resistance can be obtained when the conductive paste is prepared.

[0054] Here, Figure 1 This is a diagram illustrating the outline of the cross section of the silver particle, in which the area of ​​the silver particle is the smallest rectangle. Figure 1 As shown, a silver particle to be measured is selected, and all circumscribed rectangles are calculated while rotating the selected silver particle 360 ​​degrees. The rectangle with the smallest area is selected, and the long side of the rectangle is taken as the major diameter, and the short side is taken as the minor diameter.

[0055] It should be noted that the method for measuring L (circumference of the silver particles) and the major axis and minor axis in the above (Formula 1) will be described later.

[0056] Although the bulk silver powder of the present invention is not flat like the flake silver powder, a portion of its surface has a flat surface, and the cross section of the silver particle has a shape closer to a quadrilateral (rectangle) than a circle (ellipse). Therefore, the average value of the ratio of the perimeter of the silver particle to the perimeter of the rectangle circumscribed with the outline of the cross section of the silver particle shown in the above (Formula 1) is 0.84 or more. It should be noted that, as described later, the above flat surface is a mechanically formed surface, and therefore does not need to be a crystal plane generated by a crystal structure (face-centered cubic).

[0057] <Aspect Ratio>

[0058] The average value of the aspect ratio (longer diameter of silver particles / shorter diameter of silver particles) of the bulk silver powder of the present invention is 1.2 or more and less than 2.0, preferably 1.2 or more and 1.9 or less, and more preferably 1.3 or more and 1.8 or less.

[0059] The average value of the aspect ratio is smaller than the average value of the aspect ratio of flaky silver powder, being greater than 1.2 and less than 2.0. Therefore, when a conductive paste is made, there is less chance of silver particles clogging and poor discharge performance, which is advantageous in making the nozzle tip smaller for fine line printing.

[0060] Here, the major and minor axes of the silver particles are the long and short sides of the rectangle with the smallest area in the rectangle circumscribing the outline of the silver particle cross section. It should be noted that the method for measuring the major and minor axes of the silver particles will be described later.

[0061] When spherical silver powder and flake silver powder are mixed, silver powder with an aspect ratio of less than 2 may be classified as spherical silver powder, and silver powder with an aspect ratio of 2 or more may be classified as flake silver powder, but this is the case when only two types of spherical silver powder and flake silver powder exist. The average value of the aspect ratio of spherical silver powder is usually close to 1. The average value of the aspect ratio of flake silver powder in the above measurement method is usually 3 or more.

[0062] Unlike the aspect ratio measurement method of the present invention, when the aspect ratio (major diameter / thickness) is measured in a manner that allows the thickness of the flat shape to be uniformly measured by embedding the flaky silver particles in a resin in accordance with their orientation, the average aspect ratio is usually 6 or more.

[0063] <Circularity coefficient and shape coefficient>

[0064] In the bulk silver powder of the present invention, it is preferred that the average value of the circularity coefficient represented by the following (Formula 2) is 0.65 to 0.88, or the average value of the shape coefficient represented by the following (Formula 3) is 1.4 to 2.6.

[0065] (Equation 2): 4πS / L 2

[0066] Where S is the area of ​​the silver particles (μm 2 ), L is the circumference of the silver particle (μm).

[0067] (Formula 3):π(L max ) 2 / 4S

[0068] Where S is the area of ​​the silver particles (μm 2 )、L max It indicates the maximum length (μm) of a silver particle. The maximum length is the distance between two parallel lines when the outline of the silver particle is sandwiched between them and the distance between the parallel lines is the maximum.

[0069] It should be noted that S (area of ​​silver particles), L (circumference of silver particles), S (area of ​​silver particles), and L in the above (Formula 2) are max The method for measuring (the maximum length of the silver particles) will be described later.

[0070] The average circularity coefficient of the bulk silver powder of the present invention is preferably 0.65 to 0.88, more preferably 0.75 to 0.85. In addition, the proportion of the bulk silver powder having a circularity coefficient of 0.65 to 0.88 is preferably 40% or more, more preferably 50% or more.

[0071] The average value of the shape coefficient of the bulk silver powder of the present invention is preferably 1.4 to 2.6, more preferably 1.5 to 2.0. In addition, the proportion of the bulk silver powder having a shape coefficient of 1.4 to 2.6 is preferably 40% or more, more preferably 50% or more.

[0072] As described above, by satisfying the numerical ranges of the circularity coefficient and the shape coefficient, and by having a cross-section of the silver powder having a shape closer to a quadrilateral than a circle (block shape rather than a spherical shape), it is possible to obtain electrical wiring with low line resistance when a conductive paste is prepared. Although the reason is not clear, it is believed that this is because the block silver powder of the present invention can increase the density of silver particles in the wiring electrode, and the number of contact points between the silver particles also increases.

[0073] <Method for determining the ratio of the perimeter of a particle to the perimeter of a circumscribed rectangle, the circularity coefficient, the shape coefficient, and the aspect ratio>

[0074] Silver powder was placed in a resin (EPOFIX resin manufactured by Struers) and a curing agent (EPOFIX curing agent manufactured by Struers) to cure, and polished using an ion beam cross-section polisher (ArBlade5000 manufactured by Japan High-Tech Co., Ltd.) to expose the cross section of the silver particles. The cross section of the silver particles was observed using a scanning electron microscope (JEOL JSM-IT300LV, manufactured by JEOL Ltd.) at 5000 times magnification. It should be noted that the silver powder and resin were mixed manually and then poured into a mold for curing. The orientation of the silver particles exposed after polishing was random. Figure 2 As shown, the cross section of the silver particle whose entire outline can be captured in the field of view is measured.

[0075] Next, for cross sections of 100 or more silver particles selected at random, the outer periphery of the silver particles was traced using image analysis software (MacView, manufactured by MOUNTECH Co., Ltd., image analysis type particle size distribution measurement software), thereby measuring the major axis, minor axis, perimeter (L) of each silver particle, the area (S) of the silver particle, and the maximum length (L) of the silver particle. max ). The major diameter and minor diameter are automatically calculated as the values ​​when the area of ​​the circumscribed rectangle becomes the smallest. Based on these values, the ratio of the perimeter of the particle to the perimeter of the circumscribed rectangle is calculated based on the above (Formula 1). In addition, based on the above (Formula 2) and the above (Formula 3), the average values ​​of the circularity coefficient and the shape coefficient are calculated, and the proportion of the circularity coefficient is 0.65 to 0.88, and the proportion of the shape coefficient is 1.4 to 2.6. In addition, the average value of the aspect ratio (major diameter / minor diameter) is calculated.

[0076] The spherical silver powder is different from the massive silver powder of the present invention. The average value of the ratio of the perimeter of the silver particles shown in the above formula (Formula 1) to the perimeter of the circumscribed rectangle is closer to 0.79 in the case of a circle than that of the massive silver powder of the present invention.

[0077] The circularity coefficient and the shape coefficient of the spherical silver powder have values closer to 1 than those of the circularity coefficient and the shape coefficient of the massive silver powder of the present invention.

[0078] The massive silver powder of the present invention, only in terms of the average aspect ratio, is within the range of the spherical silver powder, but it can be distinguished from the spherical silver powder by the ratio of the perimeter of the silver particles shown in the above formula (Formula 1) to the perimeter of the circumscribed rectangle, the average value of the circularity coefficient, and the average value of the shape coefficient.

[0079] When observed with a scanning electron microscope, the massive silver powder of the present invention is neither spherical silver powder nor flaky silver powder with an average aspect ratio of 2 or more.

[0080] Therefore, the massive silver powder of the present invention is neither spherical silver powder nor flaky silver powder.

[0081] <BET specific surface area>

[0082] The BET specific surface area of the massive silver powder of the present invention is 0.5 m 2 / g or less, preferably 0.35 m 2 / g or less, more preferably 0.30 m 2 / g or less, further preferably 0.1 m 2 / g or more and 0.27 m 2 / g or less.

[0083] When the BET specific surface area is 0.5 m 2 / g or less, the silver particles can be smoothly discharged from the front end of the nozzle when making a conductive paste, which is beneficial to suppressing wire breakage in fine line printing.

[0084] The BET specific surface area can be measured by the BET single point method based on nitrogen adsorption using Macsorb HM-model 1210 (manufactured by MOUNTECH Co., Ltd.). It should be noted that in the measurement of the BET specific surface area, the degassing conditions before measurement are 60 °C and 10 minutes.

[0085] <Volume-based cumulative 50% particle size (D 50 ), ratio [(D 90 -D 10 ) / D 50 , and the value obtained by multiplying D 50 by the BET specific surface area>

[0086] The cumulative 50% particle size (D 50 ) is preferably from 0.5 μm to 5 μm, more preferably from 1 μm to 4 μm.

[0087] The volume-based cumulative 10% particle size (D 10 ) and cumulative 90% particle size (D 90 ) relative to the cumulative 50% particle size (D 50 ) ratio [(D 90 -D 10 ) / D 50 ] is preferably less than 2.0, more preferably less than 1.5, and further preferably less than 1.3.

[0088] The cumulative 50% particle size (D 50 The value obtained by multiplying the BET specific surface area is preferably 6.5E-07m 3 / g or above and 1.0E-06m 3 / g or less, more preferably 6.5E-07m 3 / g or above and 9.0E-07m 3 / g or less.

[0089] Here, the symbol "E" indicates that the value following it is a "power exponent" with a base of 10. The value represented by the exponential function with a base of 10 is multiplied by the value before "E". For example, "1.0E-07" means "1.0×10 -7 ”.

[0090] The cumulative 50% particle size (D 50 ) multiplied by the BET specific surface area, the flaky silver powder tends to be larger than the bulk silver powder.

[0091] <Tap density>

[0092] The tap density of the bulk silver powder is preferably 3.0 g / mL to 7.0 g / mL, and more preferably 4.0 g / mL to 7.0 g / mL.

[0093] As a method for measuring the tap density of the bulk silver powder, for example, a tap density measuring device (manufactured by Shibayama Science Co., Ltd., bulk density measuring device SS-DA-2) is used, 30 g of the silver powder sample is weighed and placed in a 20 mL test tube, and tapped 1000 times with a drop of 20 mm. The tap density can be calculated from tap density = sample weight (30 g) / sample volume after tapping (mL).

[0094] <Loss on ignition>

[0095] The ignition loss of the bulk silver powder is also called Ig-Loss, which indicates the weight change when heated from room temperature to 800° C. Specifically, it indicates the amount of the composition other than silver in the bulk silver powder, and is an indicator showing the amount of residual components such as the surface treatment agent in the spherical silver powder and the lubricant added to the silver paste when bulking, which are components remaining in the bulk silver powder.

[0096] The ignition loss of the bulk silver powder is not particularly limited and may be appropriately selected depending on the intended purpose, but is preferably 0.05% to 3.0%, more preferably 0.1% to 1.0%.

[0097] (Method for producing bulk silver powder)

[0098] The method for producing bulk silver powder of the present invention comprises: a bulking step, in which spherical silver powder and a medium are placed in a container, and the spherical silver powder and the medium collide with each other through the movement of the container to obtain bulk silver powder, and further comprises other steps as needed.

[0099] In the bulk silver powder, when observing cross sections of more than 100 silver particles, the average aspect ratio is 1.2 or more and less than 2.0, and the average ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more.

[0100] (Formula 1): L / (2×long diameter+2×short diameter)

[0101] Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

[0102] As the spherical silver powder (raw powder) used in the method for producing bulk silver powder of the present invention, silver powder having the following properties is preferred.

[0103] · Volume-based cumulative 50% particle size (D 50 ) is preferably from 0.5 μm to 5 μm, more preferably from 1 μm to 4 μm.

[0104] The BET specific surface area is preferably 0.5 m 2 / g or less, more preferably 0.3m 2 / g or less, more preferably 0.1m 2 / g or more and 0.27mm 2 / g or less.

[0105] The average value of the aspect ratio is preferably 1 to 1.5, and more preferably close to 1.

[0106] The average value of the shape factor is preferably less than 1.4, and more preferably close to 1.

[0107] The average value of the circularity coefficient is preferably greater than 0.88, and more preferably close to 1.

[0108] It should be noted that the volume-based cumulative 50% particle size (D 50 ), the method for determining the BET specific surface area, the average value of the aspect ratio, the average value of the shape coefficient, and the average value of the circularity coefficient is the same as that of the above-mentioned bulk silver powder.

[0109] The spherical silver powder may be a commercially available product or a spherical silver powder produced by a known production method (e.g., a wet reduction method). Examples of the commercially available product include AG-5-54F and AG-5-1F (both produced by Tonghe Electronic Technology Co., Ltd.). Details of the wet reduction method are described in, for example, Japanese Patent Application Laid-Open No. 7-76710.

[0110] The medium (sometimes also referred to as "balls" or "beads") is preferably a spherical medium with a diameter of 0.5 mm to 3 mm. If the diameter of the medium is less than 0.5 mm, the separation efficiency may be reduced due to clogging of the medium when the treated silver powder is separated from the medium. If the diameter of the medium is more than 3 mm, the silver particles are more bonded to each other, and the volume-based cumulative 50% particle size (D 50 ) may become too large, making it difficult to obtain bulk silver powder.

[0111] The material of the medium is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include metals such as titanium and stainless steel, and ceramics such as alumina and zirconia. Among them, stainless steel is preferred from the viewpoint of contamination of the silver powder.

[0112] The treatment time of the agglomeration step is preferably 10 minutes to 180 minutes. The treatment time can be appropriately adjusted according to the rotation speed of the device in order to match the purpose of stopping the process at a stage where each silver particle collides with the medium and forms a flat surface on a part of the surface, but flattening does not progress significantly. When the treatment time is prolonged and the work applied to the silver particles increases, the silver particles are bonded to each other, and the proportion of silver particles that form flaky silver powder with a large aspect ratio increases, and it may be impossible to obtain a silver powder in which the bulk silver particles are mainly bulk silver particles and the bulk silver particles account for more than 40% of the silver particles observed by an electron microscope. By adjusting "the time, the rotation speed, the medium and the filling rate of the silver powder with respect to the container volume" so that each silver particle collides with the medium to a degree where the aspect ratio is not as large as that of the flaky silver powder, the bulk silver powder of the present invention can be produced in which the average aspect ratio when observing the cross-section of more than 100 silver particles is 1.2 or more and less than 2.0, and the average ratio of the perimeter of the silver particles represented by the above formula (1) to the perimeter of the circumscribed rectangle is 0.84 or more.

[0113] The apparatus used in the agglomeration step is not particularly limited and may be appropriately selected depending on the intended purpose. Examples thereof include media stirring pulverizers such as a bead mill, a ball mill, and an attritor.

[0114] In the agglomeration process, a lubricant may be used or not, but it is preferred not to use a lubricant from the perspective of suppressing the increase of ignition loss (Ig-Loss) and further reducing the line resistance. The lubricant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include stearic acid, oleic acid, and the like.

[0115] <Other Processes>

[0116] As other steps, for example, there can be mentioned a spherical silver powder preparation step, a washing step, a drying step, and the like.

[0117] (Conductive paste)

[0118] The conductive paste of the present invention contains the aforementioned bulk silver powder of the present invention, preferably contains a resin and a solvent, and further contains other components as necessary.

[0119] In addition to the bulk silver powder of the present invention, the conductive paste may further contain silver powder in other shapes (spherical silver powder or flake silver powder, etc.).

[0120] The total amount of the silver powder including the bulk silver powder in the conductive paste is preferably 50% to 98% by mass, more preferably 80% to 95% by mass, based on the total amount of the conductive paste.

[0121] The resin is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include epoxy resins, acrylic resins, polyester resins, polyimide resins, polyurethane resins, phenoxy resins, silicone resins, ethyl cellulose, and mixtures thereof, etc. These can be used alone or in combination of two or more.

[0122] The solvent is not particularly limited and may be appropriately selected depending on the intended purpose, and examples thereof include terpineol, butyl carbitol, butyl carbitol acetate, terpineol-12, etc. These may be used alone or in combination of two or more.

[0123] Examples of other components include a curing agent, a glass frit, a dispersant, a surfactant, and a viscosity modifier.

[0124] The method for producing the conductive paste is not particularly limited and can be appropriately selected according to the purpose. For example, the conductive paste can be produced by mixing the block silver powder, the resin, the solvent, and the silver powder of other shapes as required and the other components of the present invention. For example, ultrasonic dispersion, a disperser, a three-roll mill, a ball mill, a bead mill, a biaxial kneader, a rotation-revolution type mixer, etc. can be used for the mixing.

[0125] The viscosity of the conductive paste is not particularly limited and may be appropriately selected depending on the intended purpose, but is preferably 150 Pa·s to 800 Pa·s, more preferably 200 Pa·s to 750 Pa·s, under the conditions of a paste temperature of 25° C. and a rotation speed of 1 rpm.

[0126] When the viscosity of the conductive paste is less than 150 Pa·s, “bleeding” may occur during printing, and when it is greater than 800 Pa·s, uneven printing may occur.

[0127] The viscosity of the conductive paste can be measured by, for example, using 5XHBDV-IIIUC manufactured by Brookfield as a rotational viscometer, using CPE-52 as the cone shaft, setting the measurement temperature at 25° C., setting the cone shaft rotation speed at 1 rpm, and adopting the viscosity value when the cone shaft is rotated for 5 minutes.

[0128] Since the conductive paste of the present invention contains the aforementioned bulk silver powder of the present invention, it has low line resistance and is suitable for thinning. Therefore, it is suitable for use in, for example, collecting electrodes of solar cell units, external electrodes of chip-type electronic components, electrodes or electrical wiring for RFID, electromagnetic wave shielding, membrane switches, electroluminescence, etc., or for use as a conductive adhesive for vibrator bonding, bonding between solar cell units such as single cells, etc.

[0129] Example

[0130] Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.

[0131] (Example 1)

[0132] 1.16 kg of spherical silver powder (AG-5-54F manufactured by DOWA HIGHTECH) was prepared and placed in a 5 L container of a vibration ball mill (B-1 manufactured by Chuo Kakoki Shoji Co., Ltd.) together with 12 kg of SUS balls (diameter 0.8 mm) as a medium, and the silver particles were collided with the medium at 800 rpm for 60 minutes. It should be noted that after the silver powder and the SUS balls were separated, they were crushed using a small pulverizer (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) and passed through a sieve with a mesh size of 25 μm.

[0133] The scanning electron microscope photograph of the bulk silver powder obtained in Example 1 is shown in Figure 3A The scanning electron microscope photograph of the cross section of the bulk silver powder is shown in Figure 3B .

[0134] (Example 2)

[0135] 1.16 kg of spherical silver powder (AG-5-54F manufactured by DOWA HIGHTECH) was prepared, 3.84 g of stearic acid was added as a lubricant and mixed thoroughly, and put into a 5 L container of a vibration ball mill (B-1 manufactured by Chuo Kakoki Shoji Co., Ltd.) together with 12 kg of SUS balls (diameter 0.8 mm) as a medium, and the silver particles were collided with the medium at 800 rpm for 60 minutes. It should be noted that after the silver powder was separated from the SUS balls, it was crushed using a small pulverizer (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) and passed through a sieve with a mesh size of 25 μm.

[0136] The scanning electron microscope photograph of the bulk silver powder obtained in Example 2 is shown in Figure 4A The scanning electron microscope photograph of the cross section of the bulk silver powder is shown in Figure 4B .

[0137] (Example 3)

[0138] 1.61 kg of spherical silver powder (AG-5-1F manufactured by DOWA HIGHTECH) was prepared and placed in a 6 L container of a rolling ball mill together with 16.62 kg of SUS balls (diameter 1.6 mm), and the silver particles were collided with the medium at 71 rpm for 180 minutes. It should be noted that after the silver powder was separated from the SUS balls, it was crushed using a small pulverizer (SK-M10 manufactured by Kyoritsu Riko Co., Ltd.) and passed through a sieve with a mesh size of 25 μm.

[0139] The scanning electron microscope photographs of the bulk silver powder obtained in Example 3 are shown in Figure 5A , and the scanning electron microscope photographs of the cross-section of the bulk silver powder are shown in Figure 5B .

[0140] (Comparative Example 1)

[0141] In Comparative Example 1, the step of colliding silver particles with the medium was carried out at 800 rpm for 240 minutes, and the silver powder of Comparative Example 1 was obtained in the same manner as in Example 1 except for this.

[0142] The scanning electron microscope photographs of the silver powder obtained in Comparative Example 1 are shown in Fig. 6A , and the scanning electron microscope photographs of the cross-section of the silver powder are shown in Figure 6B .

[0143] (Comparative Example 2)

[0144] The step of colliding silver particles with the medium was not carried out, and spherical silver powder (manufactured by DOWA HIGHTECH, AG-5-54F) was directly used. The scanning electron microscope photographs of the spherical silver powder of Comparative Example 2 are shown in Fig. 7A , and the scanning electron microscope photographs of the cross-section of the silver powder are shown in Figure 7B .

[0145] Next, the measurement results of the shape, BET specific surface area, particle size distribution, Ig-Loss, and tapped density of the spherical silver powder (AG-5-54F) used in Examples 1 and 2 and Comparative Examples 1 and 2, and the spherical silver powder (AG-5-1F) used in Example 3 are shown in Table 1. It should be noted that the measurement methods of the BET specific surface area, particle size distribution, Ig-Loss, and tapped density of the spherical silver powder (AG-5-54F) and the spherical silver powder (AG-5-1F) are the same as those of Examples 1 to 3 and Comparative Examples 1 to 2 described later.

[0146] [Table 1]

[0147]

[0148] Next, for the silver powders of Examples 1 to 3 and Comparative Examples 1 to 2 obtained, the average values of the shape, BET specific surface area, particle size distribution, Ig-Loss, tapped density, the ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle, the average value of the circularity coefficient, the ratio of the circularity coefficient of 0.65 to 0.88, the average value of the shape factor, the ratio of the shape factor of 1.4 to 2.6, and the average value of the aspect ratio were obtained as follows. The results are shown in Table 2.

[0149] [BET Specific Surface Area]

[0150] The BET specific surface area of ​​each prepared silver powder was measured by a BET specific surface area measuring device (Macsorb HM-model 1210, manufactured by MOUNTECH) using a BET one-point method based on nitrogen adsorption. It should be noted that in the measurement of the BET specific surface area, the degassing conditions before the measurement were 60° C. and 10 minutes.

[0151] <Measurement method of particle size distribution>

[0152] The volume-based cumulative 10% particle size (D 10 ), cumulative 50% particle size (D 50 ), cumulative 90% particle size (D 90 ), find the ratio [(D 90 -D 10 ) / D 50 ].

[0153] 0.1 g of silver powder was added to 40 mL of isopropyl alcohol (IPA), dispersed for 2 minutes using an ultrasonic homogenizer (device name: US-150T, manufactured by Nippon Seiki Co., Ltd.; 19.5 kHz, chip tip diameter 18 mm), and then measured using a laser diffraction / scattering particle size distribution measuring device (Microtrac BEL Corp., Microtrac MT-3300EXII).

[0154] <Method for determining the ratio of the perimeter of a particle to the perimeter of a circumscribed rectangle, the circularity coefficient, the shape coefficient, and the aspect ratio>

[0155] Each silver powder was put into a resin (EPOFIX resin manufactured by Struers) and a curing agent (EPOFIX curing agent manufactured by Struers) to be cured, and polished using an ion beam cross-section polisher (ArBlade 5000 manufactured by Japan High-Tech Co., Ltd.) to expose the cross section of the silver particles, and the cross section of each silver particle was observed using a scanning electron microscope (JEOL JSM-IT300LV, manufactured by JEOL Ltd.) at 5,000 times. Figure 2 As shown in FIG. 1 , for the cross sections of 100 silver particles randomly selected from the cross sections of the silver particles whose entire outlines can be captured in the field of view, the outer periphery of the silver particles was traced using image analysis software (MacView, manufactured by MOUNTECH Co., Ltd., image analysis type particle size distribution measurement software), thereby measuring the major axis, minor axis, perimeter (L) of each silver particle, the area (S) of the silver particle, and the maximum length (L) of the silver particle. max). The major diameter and minor diameter are automatically calculated as the values ​​when the area of ​​the circumscribed rectangle becomes the smallest. Based on these values, the ratio of the perimeter of the particle to the perimeter of the circumscribed rectangle is calculated based on the following (Formula 1). In addition, the average value of the circularity coefficient and the average value of the shape coefficient are calculated based on the following (Formula 2) and the following (Formula 3), and the proportion of the circularity coefficient is 0.65 to 0.88, and the proportion of the shape coefficient is 1.4 to 2.6. In addition, the average value of the aspect ratio (major diameter / minor diameter) is calculated.

[0156] (Formula 1): L / (2×long diameter+2×short diameter)

[0157] Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

[0158] (Equation 2): 4πS / L 2

[0159] Where S is the area of ​​the silver particles (μm 2 ), L is the circumference of the silver particle (μm).

[0160] (Formula 3):π(L max ) 2 / 4S

[0161] Where S is the area of ​​the silver particles (μm 2 ), L max It represents the maximum length of silver particles (μm).

[0162] <Determination method of ignition loss (Ig-Loss)>

[0163] For the ignition loss (Ig-Loss) of each prepared silver powder, 3 g of the silver powder sample (weighing value: w1) was accurately weighed and placed in a magnetic crucible and heated to 800°C. Then it was kept at 800°C for 30 minutes, which was enough time to reach a constant weight. Then it was cooled and weighed again (weighing value: w2). The w1 and w2 were substituted into the following (Formula 4) to obtain the ignition loss value.

[0164] Ig-Loss value (mass %) = (w1-w2) / w1×100 (Formula 4)

[0165] <Measurement method of tap density>

[0166] The tap density of each prepared silver powder was measured using a tap density measuring device (produced by Shibayama Science Co., Ltd., bulk density measuring device SS-DA-2). 30 g of silver powder was weighed and placed in a 20 mL test tube, and tapped 1000 times with a drop height of 20 mm. The tap density was calculated according to the following formula.

[0167] Tap density (g / mL) = sample weight (15g) / sample volume after tapping (mL)

[0168] [Table 2]

[0169]

[0170] (Manufacturing of Conductive Paste)

[0171] The silver powders of Examples 1 to 3 and Comparative Examples 1 to 2 and spherical silver powder (silver powder including spherical silver particles, manufactured by DOWA HIGHTECH, AG-2-1C Agent Added) were mixed at a weight ratio of 5:5 to prepare raw silver powder.

[0172] Next, epoxy resin (jER1009, manufactured by Mitsubishi Chemical Corporation) was added to a solvent (butyl carbitol acetate, hereinafter referred to as "BCA") and stirred while heating until completely dissolved to obtain an epoxy resin jER1009 carrier. The concentration of jER1009 in the epoxy resin carrier was 62.23% by mass.

[0173] 92.60 mass % of the above raw silver powder, 3.90 mass % of epoxy resin (EP-4901E, manufactured by ADEKA Co., Ltd.), 1.57 mass % of the above epoxy resin jER1009 carrier, 0.24 mass % of curing agent (boron trifluoride monoethylamine complex) and an appropriate amount of solvent (BCA) are mixed and kneaded.

[0174] For mixing and kneading, first, a paddleless self-rotation and revolution stirring and degassing device (manufactured by EME Co., Ltd., VMX-N360) was used to stir and mix at a revolution of 1200 rpm / rotation of 600 rpm for 30 seconds, and then the obtained mixture was kneaded using a three-roll mill (manufactured by Ott, Hermann, EXAKT80S). As described above, the conductive pastes before viscosity adjustment of Examples 1 to 3 and Comparative Examples 1 to 2 were obtained. For each conductive paste before viscosity adjustment, the viscosity was measured as follows. The results are shown in Table 3.

[0175] <Viscosity of Conductive Paste>

[0176] The viscosity of each conductive paste was measured using a 5XHBDV-IIIUC manufactured by Brookfield as a rotational viscometer under the following conditions. The cone shaft used was CPE-52. The measurement temperature was set to 25° C. and the cone shaft rotation speed was set to 1 rpm. The viscosity value was the value obtained when the cone shaft was rotated for 5 minutes.

[0177] [Table 3]

[0178] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Viscosity (1rpm) (Pa·s) 512 734 441 405 556

[0179] Furthermore, BCA was appropriately added to the conductive paste before viscosity adjustment in each of Examples and Comparative Examples to obtain conductive pastes after viscosity adjustment in Examples 1 to 3 and Comparative Examples 1 to 2 whose viscosities were adjusted to about 300 Pa·s.

[0180] The viscosity of each conductive paste after the viscosity adjustment was measured in the same manner as above.

[0181] <Formation of Conductive Film>

[0182] Each conductive paste after viscosity adjustment was printed on an alumina substrate using a screen printer (Microtech, MT-320T) at a speed of 150 mm / s with 9 line patterns of design width (line width) of 30 μm and 35 μm and length of 105 mm, respectively, to form a film of each conductive paste. The film was dried at 150° C. for 10 minutes using an atmospheric circulation dryer and then further heated at 200° C. for 30 minutes to cure and form a linear conductive film.

[0183] The wire resistance, wire breakage rate, and wiring cross-sectional area of ​​each of the obtained conductive films were evaluated in the following manner.

[0184] <Line resistance>

[0185] For each conductive film prepared from each conductive paste after viscosity adjustment, the resistance value was measured using a digital multimeter (R6551 manufactured by ADVANTEST), and the line resistance of the design width (line width) of 30 μm and 35 μm was calculated from the average value of 9 line patterns. It should be noted that a very high value of the line resistance of 100 kΩ or more was regarded as a broken line and was excluded from the calculation of the average value.

[0186] <Disconnection rate>

[0187] For each conductive film prepared from each conductive paste after viscosity adjustment, the line breakage rate with a design width (line width) of 30μm and 35μm was calculated. The line breakage rate is the ratio of the number of broken lines observed in all 9 line patterns when a very high value of the measured line resistance of 100kΩ or more is regarded as a broken line during the above-mentioned line resistance measurement.

[0188] <Wiring cross-sectional area>

[0189] For each conductive film prepared from each conductive paste after viscosity adjustment, any three of the nine line patterns were selected, and the film thickness (μm) and line width (μm) of the center portion in the longitudinal direction of each were measured using a laser microscope (manufactured by KEYENCE CORPORATION, VKX-1000). The wiring cross-sectional area (μm) of the wiring with a design width (line width) of 30 μm and 35 μm was calculated based on the film thickness × line width. 2 ).

[0190] [Table 4]

[0191] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Viscosity (1rpm) (Pa·s) 314 314 302 306 310 Silver powder (mass %) 91.8 91.2 92.0 92.0 91.7 Epoxy resin: EP-4901E (mass %) 3.9 3.8 3.9 3.9 3.9 Epoxy resin: jER1009 (mass %) 1.0 1.0 1.0 1.0 1.0 Curing agent: Boron trifluoride monoethylamine complex (mass %) 0.2 0.2 0.2 0.2 0.2 Solvent: BCA (mass %) 3.1 3.8 2.9 2.9 3.3 Line resistance of 30μm line width (Ω) 36 40 36 39 40 Line resistance of 35μm line width (Ω) 27 29 27 30 32 Wire breakage rate (%) for line width 30μm 0 0 0 22 11 Wire breakage rate at line width 35μm (%) 0 0 0 0 0 <![CDATA[The cross-sectional area of the wiring with a line width of 30 μm (μm 2 )]]> 261 240 235 210 207 <![CDATA[Cross-sectional area of wiring with a line width of 35 μm (μm 2 )]]> 310 334 338 255 271

[0192] From the results in Table 4, it can be seen that the conductive films prepared from the conductive paste using the bulk silver powder of Examples 1 to 3 have lower line resistance and lower wire breakage rate than the conductive films prepared from the conductive paste using the silver powder of Comparative Examples 1 and 2.

[0193] This international application claims the priority based on Japanese Patent Application No. 2022-040925 filed on March 16, 2022, and incorporates the entire contents of Japanese Patent Application No. 2022-040925 into this international application.

Claims

1. A bulk silver powder, characterized in that: BET specific surface area is 0.5m 2 / g or less, When observing cross sections of 100 or more silver particles, the average value of the aspect ratio is 1.2 or more and less than 2.0, and the average value of the ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more, (Formula 1): L / (2×long diameter+2×short diameter) Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

2. The bulk silver powder according to claim 1, wherein The average value of the circularity coefficient shown in the following (Formula 2) is 0.65 to 0.88, (Equation 2): 4πS / L 2 Where S is the area of ​​the silver particles (μm 2 ), L is the circumference of the silver particle (μm).

3. The bulk silver powder according to claim 2, wherein: The ratio of the circularity coefficient being 0.65 to 0.88 is 40% or more.

4. The bulk silver powder according to any one of claims 1 to 3, wherein The average value of the shape factor shown in the following (Formula 3) is 1.4 to 2.6, (Formula 3): π(L max ) 2 / 4S Where S is the area of ​​the silver particles (μm 2 ), L max It represents the maximum length of silver particles (μm).

5. The bulk silver powder according to claim 4, wherein: The proportion of the shape factor being 1.4 to 2.6 is 40% or more.

6. The bulk silver powder according to any one of claims 1 to 5, wherein The cumulative 50% particle size (D 50 ) multiplied by the BET specific surface area gives a value of 6.5E-07m 3 / g or above and 1.0E-06m 3 / g or less.

7. The bulk silver powder according to any one of claims 1 to 5, wherein the BET specific surface area is 0.35 m 2 / g or less.

8. A method for producing bulk silver powder, characterized in that: include: In the bulking process, spherical silver powder and a medium are placed in a container, and the spherical silver powder and the medium collide with each other through the movement of the container, thereby obtaining bulk silver powder. In the bulk silver powder, when observing cross sections of 100 or more silver particles, the average value of the aspect ratio is 1.2 or more and less than 2.0, and the average value of the ratio of the perimeter of the silver particles to the perimeter of the circumscribed rectangle represented by the following (Formula 1) is 0.84 or more, (Formula 1): L / (2×long diameter+2×short diameter) Here, L is the perimeter of the silver particle (μm), and the major axis and minor axis are the long side (μm) and short side (μm) of the rectangle with the smallest area in the rectangle circumscribing the outline of the cross section of the silver particle.

9. The method for producing bulk silver powder according to claim 8, wherein: The agglomeration process is performed without using a lubricant.

10. A conductive paste, characterized in that: Containing the bulk silver powder according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Making method for high-tap-density surface-modified silver powder

    CN104190946A

  • Silver powder mixture, method for producing same, and conductive paste

    CN111148586A

  • Silver powder, production method thereof, and conductive paste

    CN112752627A

  • Flake silver powder and its production method

    JP2007254845A

  • Conductive powder and forming method of conductive powder

    JP2007265801A