Silk protein-metal ion complex transparent nanogel as well as preparation and application thereof

By preparing silk protein-metal ion complex transparent nanogel, the problem of metal ion concentration and stability control is solved, and multifunctional biological activity and stability is achieved. It is suitable for skin care and regenerative medicine, which is better than the existing technology. Blue copper peptide.

CN118986767APending Publication Date: 2024-11-22SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410950352.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the concentration and stability of metal ions, resulting in limited biological activity performance, and polypeptide-metal ion complexes have poor compatibility in the field of effective skin care and limited application space.

Method used

By preparing silk protein-metal ion complex transparent nanogels, ultrasonic treatment is used to regulate the size of silk protein nanofibers, combined with the appropriate metal ion concentration and stirring rate, stable silk protein-metal ion complex nanoparticles are formed to avoid Opacity gel is formed and fiber network formation is induced through the maturation process to achieve long-term stable dispersion.

Benefits of technology

It realizes the long-term stability and multifunctional biological activity of silk protein-metal ion complex, can be combined with different active ingredients, is better than the stability and compatibility of blue copper peptide, and is suitable for tissue regeneration and repair and effective skin care.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118986767A_ABST
    Figure CN118986767A_ABST
Patent Text Reader

Abstract

The invention discloses silk protein-metal ion complex transparent nanogel as well as preparation and application thereof, and a preparation method comprises the following steps: treating silk protein nanofibers, and regulating and controlling the nano size of the silk protein nanofibers; adding a metal salt aqueous solution with a proper concentration into the silk protein nanofiber or particle solution under a stirring or ultrasonic condition, and uniformly mixing; carrying out high-speed centrifugation on the mixture to remove large-size aggregates so as to obtain a transparent silk protein-ion complex nano-particle solution; and curing the complex nanoparticle solution at a proper temperature to obtain the silk protein-metal ion complex transparent nanogel, and the transparent nanogel can maintain good biocompatibility while having good antibacterial property, vascularization promoting capability and inflammation inhibiting property, and can be combined with different active ingredients to achieve the effects of inhibiting inflammation and promoting blood circulation, so that the silk protein-metal ion complex transparent nanogel can be used for preparing the silk protein-metal ion complex transparent nanogel. Unification of biological activity, stability and compatibility is achieved, the preparation process is simple, conditions are mild, and large-scale production and future transformation are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to a silk protein-metal ion complex transparent nanogel and a preparation and application thereof. Background Art

[0002] Metal ions are key regulatory factors in living organisms, playing an important role in maintaining life homeostasis, promoting the repair of different tissues, and treating different diseases. The biological activity of most metal ions is concentration-dependent, and excessive concentrations can lead to cytotoxicity. Therefore, how to effectively control the concentration of metal ions and correctly exert the biological activity of metal ions is a key issue in the application of metal ions in the field of regenerative medicine.

[0003] In order to avoid the sudden release or too fast disappearance of ions, researchers have developed a variety of methods for fixing and slow-release metal ions, such as complexation with polymers / macromolecular complexes, biomineralization, and bioglass. The ion release of the above methods is mainly achieved through the degradation of complexes or composite systems, but the degradation behavior of minerals and bioglass is difficult to effectively regulate, resulting in the activity of metal ions being greatly restricted. Inside the living body, the formation of stable complexes by complexation of peptides and metal ions is a reliable method for metal ions to exert biological activity. Blue copper peptide is a complex formed by peptides and copper ions. It is considered to be an efficient growth factor. It has multiple functions in the body, such as promoting angiogenesis / regulating inflammation, and is widely used in the field of functional skin care. However, it is easy to inactivate and reacts with a variety of active molecules to cause inactivation. Therefore, blue copper peptide has poor compatibility in the field of functional skin care and limited application space. While avoiding the side effects of metal ions, it is urgent to solve the stability and compatibility problems of blue copper peptides and develop a new type of active material with stable structure and efficient biological activity of metal ions. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a silk protein-metal ion complex transparent nanogel and its preparation and application.

[0005] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0006] The first aspect of the present invention provides a method for preparing a silk protein-metal ion complex transparent nanogel, comprising the following steps:

[0007] (1) treating a silk protein fiber gel containing 0.2 to 6 wt% of silk protein by ultrasonic treatment to obtain a silk protein nanofiber or particle solution having a diameter of 10 to 1200 nm;

[0008] (2) mixing the metal salt aqueous solution with the silk protein nanofiber or particle solution obtained in step (1) at a stirring rate of 200 to 700 rpm to obtain a silk protein-metal ion complex nanoparticle solution, wherein the concentration of metal ions in the silk protein-metal ion complex nanoparticle solution is 10 to 1000 μM;

[0009] (3) The silk protein-metal ion complex nanoparticle solution obtained in step (2) is centrifuged, and the supernatant is subjected to a aging treatment to convert uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-metal ion complex transparent nanogel.

[0010] The present invention firstly processes high-crystalline silk protein nanofibers to adjust their nanometer size; adds a metal salt aqueous solution of appropriate concentration to the silk protein nanofiber or particle solution under stirring or ultrasonic conditions and mixes them evenly; centrifuges the mixture at high speed to remove large-sized aggregates to obtain a transparent silk protein-ion complex nanoparticle solution; and matures the complex nanoparticle solution at a suitable temperature to obtain a silk protein-metal ion complex transparent nanogel. The preparation process is simple and the conditions are mild, which is conducive to large-scale production and future transformation.

[0011] The present invention is based on the technology of complex formation by the action of silk protein nanofibers or particles and metal ions. By controlling parameters such as the size of silk protein nanoaggregates and the metal ion concentration, the formation rate and size of the silk protein-metal ion complex are controlled. At the same time, the ratio / rate of the complexation between silk protein aggregates and metal ions and the further aggregation behavior of silk protein aggregates are regulated to avoid gelation caused by too rapid complexation and re-aggregation of silk protein aggregates, which leads to excessive size of nanoparticles and disordered aggregation to form opaque gel.

[0012] There are three forces in the process of silk protein nanofiber or particle solution complexing with metal ions: first, the non-covalent interaction between silk protein nanofibers or particles and metal ions to form aggregates; second, the reaggregation of silk protein nanofibers or particles and metal ion aggregates; third, the addition of metal ions leads to a decrease in the repulsive force between silk protein nanofibers or particles, and uncontrollable aggregation between silk protein nanofibers or particles. Therefore, the concentration of metal ions, the ratio and rate of silk protein aggregates and metal ion complexation are crucial, and the three together micro-regulate the aggregation process. In addition, the regulation of the complexation rate between silk protein and metal ions and the formation of silk protein nanofiber network induced by late maturation are the key to achieving complex size regulation and long-term stable dispersion.

[0013] The size of silk protein nanofibers can be reduced by ultrasound. While improving its fluidity, the reduction in size can effectively avoid the uncontrollable reaggregation of silk protein aggregates, which is the premise for regulating the size of the complex with ions. Subsequently, the concentration of copper ions added is coordinated with the stirring rate and the addition rate to adjust the size of the complex to avoid the excessive growth of the complex size, resulting in excessive size and the formation of opaque aggregates. In the process of adding ion solution, the excess of silk protein is maintained, which not only relatively reduces the degree of decrease in negative charge density when ions are added, so as to maintain sufficient negative charge repulsion to avoid uncontrollable aggregation between silk proteins, but also can inhibit the aggregation of complexes through the presence of silk protein network in the solution, so as to achieve size control and balance. After the complex is fully formed, the system still retains excess unacted silk protein, which can grow again through the synergy of charge repulsion and hydrophobic effect, and transform from particles after ultrasound into fibers. At the same time, the system is changed from solution state to gel state, so as to achieve long-term stability of the system.

[0014] Therefore, the present invention first optimizes the complexation of high-crystalline silk protein aggregates with metal ions through nano-regulation, and then uses metal ions of appropriate concentration to regulate the complexation rate of nano-aggregates and metal ions and the rate of re-aggregation of silk protein aggregates triggered by complex formation, so as to control the size of silk protein-metal ion complex below 200nm, avoid re-aggregation of complexes and silk protein aggregates, and form a solution with small complex size and transparent morphology. In order to avoid further aggregation of complex nanoparticles formed in the solution state, the controllable re-aggregation of silk protein aggregates in the solution is actively induced through a maturation process, a nanofiber network is formed to transform the solution into a transparent gel, and the complex nanoparticles are stably dispersed in the silk protein nanofiber network to achieve long-term stable storage of the complex.

[0015] Furthermore, the volume ratio of the silk protein nanofiber or particle solution in step (1) to the metal salt aqueous solution in step (2) is (1-50):1, preferably (2-10):1.

[0016] The amount of silk protein nanofibers or particles added should be greater than that of metal ions, so that the uncomplexed silk protein nanofibers or particles can form a fiber network, and the silk protein-metal ion complex nanoparticles can be controlled within the network to achieve a stable state without aggregation for a long time.

[0017] Furthermore, in step (2), the metal ions are one or more of copper ions, zinc ions, iron ions, magnesium ions, manganese ions and calcium ions.

[0018] The silk protein-ion complex nanoparticles with good water dispersibility and excellent activity obtained by the present invention can meet multi-level needs such as tissue regeneration and repair, functional skin care, etc., and exert antibacterial, anti-inflammatory, angiogenic, and stem cell differentiation-inducing functions according to the types of metal ions.

[0019] Furthermore, the silk protein-metal ion complex nanoparticles obtained in step (2) are uniformly and stably dispersed in the solution without aggregation, have a size below 200 nm, a stable structure, remain transparent for a long time, and have excellent biological activity.

[0020] The activities and functions of silk protein-metal ion complex nanoparticles of different sizes are completely different. The existing technology is concentration-dependent, while the silk protein-metal ion complex nanoparticles prepared by the present invention can be stably dispersed and exist in the aqueous phase, can achieve multifunctionality within this size, and maintain good biocompatibility while having good antibacterial, pro-angiogenic and anti-inflammatory properties. It can be compatible with different active ingredients to achieve the unity of biological activity, stability and compatibility, and its comprehensive performance is better than that of blue copper peptide.

[0021] Furthermore, in step (3), the centrifugal treatment is carried out at a centrifugal rate of 1000 to 9000 rpm.

[0022] Furthermore, in step (3), the temperature of the centrifugal treatment is 0 to 90°C.

[0023] Furthermore, in step (3), the centrifugal treatment time is 2 to 200 minutes.

[0024] Furthermore, in step (3), the aging treatment temperature is 0 to 100° C., and the time is 30 min to 240 h.

[0025] Silk protein-metal ion complex nanoparticle solutions will deposit or aggregate if left for a long time. Therefore, the present invention actively induces the uncomplexed silk protein nanofibers or particles in the solution to reassemble through a simple aging process to form a stable fiber network, thereby fixing the silk protein-metal ion complex nanoparticles and solving the problem of long-term stable existence of nanoparticles in an aqueous environment.

[0026] The second aspect of the present invention provides a silk protein-metal ion complex transparent nanogel prepared by the method described in the first aspect, which can fully exert the biological activity of metal ions, avoid the toxicity of metal ions, and solve the weaknesses of poor compatibility / poor stability of polypeptide-metal ion complexes such as blue copper peptide.

[0027] Furthermore, the silk protein-metal ion complex nanoparticles are dispersed in the silk protein-metal ion complex transparent nanogel and fixed by the silk protein nanofiber network.

[0028] Due to the presence of excess silk protein nanofibers, the aggregation of silk protein-metal ion complex nanoparticles is avoided, and the negative charge of the nanofibers simultaneously inhibits the aggregation of the silk protein itself. Similar to the silk protein nanofiber gel, the silk protein-metal ion complex transparent nanogel provided by the present invention can be added to water and shaken to obtain a silk protein-metal ion complex nanoparticle solution.

[0029] The third aspect of the present invention provides a use of the silk protein-metal ion complex transparent nanogel described in the second aspect in the preparation of functional skin care products.

[0030] The transparent silk protein-metal ion complex transparent nanogel prepared by the present invention has a complex nanoparticle size of less than 200 nm. It can have multiple biological activities such as anti-inflammatory / antibacterial / angiogenic while maintaining good biocompatibility. At the same time, its excellent stability enables it to be directly compatible with different active ingredients such as vitamin C and retinol, providing new raw material options for the flexible design of functional skin care products.

[0031] Beneficial effects of the present invention:

[0032] (1) The present invention first optimizes the complexation of high-crystalline silk protein aggregates with metal ions through nano-regulation, and then uses metal ions of appropriate concentration to regulate the complexation rate of nano-aggregates and metal ions and the rate of re-aggregation of silk protein aggregates triggered by complex formation, so as to control the size of silk protein-metal ion complex below 200nm, avoid re-aggregation of complexes and silk protein aggregates, and form a solution with small complex size and transparent morphology. In order to avoid further aggregation of complex nanoparticles formed in the solution state, the controllable re-aggregation of silk protein aggregates in the solution is actively induced through the maturation process, a nanofiber network is formed to transform the solution into a transparent gel, and the complex nanoparticles are stably dispersed in the silk protein nanofiber network to achieve long-term stable storage of the complex. The preparation process is simple and the conditions are mild, which is conducive to large-scale production and future transformation.

[0033] (2) The transparent silk protein-metal ion complex transparent nanogel prepared by the present invention has a complex nanoparticle size of less than 200 nm. It can have multiple biological activities such as anti-inflammatory / antibacterial / angiogenic while maintaining good biocompatibility. At the same time, its excellent stability enables it to be directly compatible with different active ingredients such as vitamin C and retinol, providing new raw material options for the flexible design of functional skin care products. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 These are the scanning electron microscope images and infrared spectra of the high-crystalline silk protein nanofibers after ultrasonic treatment in Example 1; wherein a is the scanning electron microscope image, and b is the infrared spectra.

[0035] Figure 2 These are macroscopic images and electron microscope images of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex gel prepared in Comparative Example 1.

[0036] Figure 3 The macroscopic images and particle size images of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex gel prepared in Comparative Examples 1-2 are shown.

[0037] Figure 4 This is a macroscopic picture of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex transparent solution prepared in Comparative Example 3.

[0038] Figure 5 The figure shows the cell compatibility test results of silk protein-copper ion complex nanoparticle solutions with different copper ion concentrations and free copper ion copper chloride aqueous solution; among them, a is human umbilical vein endothelial cells, and b is bone marrow mesenchymal stem cells.

[0039] Figure 6 This is a test result diagram of the co-culture of silk protein-copper ion complex nanoparticle solution and copper chloride aqueous solution with Staphylococcus aureus and Escherichia coli; wherein a is Staphylococcus aureus and b is Escherichia coli.

[0040] Figure 7 The figure shows the results of the detection of the content of various factors after co-culture of silk protein-copper ion complex nanoparticle solutions with different copper ion concentrations, copper chloride aqueous solution and blue copper peptide solution with human umbilical vein endothelial cells and macrophages; among them, a is vascular endothelial growth factor VEGF, b is the pro-inflammatory factor TNF-α, c is the anti-inflammatory factor IL-10, and d is the pro-inflammatory factor IL-6.

[0041] Figure 8 This is a graph showing the compatibility test results of silk protein-copper ion complex nanoparticle solution and blue copper peptide solution. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0043] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0044] Example 1

[0045] A method for preparing a silk protein-copper ion complex transparent nanogel comprises the following steps:

[0046] (1) A high-crystalline silk protein fiber gel containing 2 wt% silk protein was subjected to ultrasonic treatment at a power of 650 W for 30 min to obtain a silk protein nanoparticle solution with a size of about 100 nm.

[0047] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 200 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 3:1, and a transparent silk protein-copper ion complex nanoparticle solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 500 μM.

[0048] (3) The silk protein-copper ion complex nanoparticle solution was centrifuged for 30 minutes at a centrifugal rate of 1000 rpm and a centrifugal temperature of 40°C. The supernatant was sealed and placed at 60°C for 24 hours to transform the uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-copper ion complex transparent nanogel.

[0049] Figure 1 The scanning electron microscope image and infrared spectrum image of the high-crystalline silk protein nanofiber after ultrasonic treatment in Example 1 are shown in FIG. Figure 1 It can be seen that the processed silk protein is nanoparticles or nanofibers, and the content of high-crystalline β-sheet is rich.

[0050] Example 2

[0051] A method for preparing a silk protein-copper ion complex transparent nanogel comprises the following steps:

[0052] (1) A high-crystalline silk fiber gel with a silk protein content of 2 wt% was subjected to ultrasonic treatment at a power of 400 W for 60 min to obtain a silk protein nanoparticle solution with a size of about 200 nm.

[0053] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 400 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 10:1, and a transparent silk protein-copper ion complex nanoparticle solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 200 μM.

[0054] (3) The silk protein-copper ion complex nanoparticle solution was centrifuged for 40 minutes at a centrifugal rate of 4000 rpm and a centrifugal temperature of 25°C. The supernatant was sealed and placed at 4°C for 120 hours to transform the uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-copper ion complex transparent nanogel.

[0055] Example 3

[0056] A method for preparing a silk protein-copper ion complex transparent nanogel comprises the following steps:

[0057] (1) A high-crystalline silk protein fiber gel containing 1 wt% silk protein was subjected to ultrasonic treatment at a power of 600 W for 60 min to obtain a silk protein nanoparticle solution with a size of about 150 nm.

[0058] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 600 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 5:1, and a transparent silk protein-copper ion complex nanoparticle solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 1000 μM.

[0059] (3) The silk protein-copper ion complex nanoparticle solution was centrifuged for 20 minutes at a centrifugal speed of 3000 rpm and a centrifugal temperature of 4°C. The supernatant was sealed and placed at 25°C for 60 hours to transform the uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-copper ion complex transparent nanogel.

[0060] Example 4

[0061] A method for preparing a silk protein-copper ion complex transparent nanogel comprises the following steps:

[0062] (1) A high-crystalline silk protein fiber gel containing 2 wt% silk protein was subjected to ultrasonic treatment at a power of 360 W for 60 min to obtain a silk protein nanoparticle solution with a size of about 300 nm.

[0063] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 700 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 2:1, and a transparent silk protein-copper ion complex nanoparticle solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 300 μM.

[0064] (3) The silk protein-copper ion complex nanoparticle solution is centrifuged for 40 minutes at a centrifugal rate of 2000 rpm and a centrifugal temperature of 25°C. The supernatant is sealed and placed at 40°C for 48 hours to transform the uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-copper ion complex transparent nanogel.

[0065] Example 5

[0066] A method for preparing a silk protein-copper ion complex transparent nanogel comprises the following steps:

[0067] (1) A high-crystalline silk protein fiber gel with a silk protein content of 1.5 wt% was subjected to ultrasonic treatment at a power of 600 W for 30 min to obtain a silk protein nanoparticle solution with a size of about 100 nm.

[0068] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 200 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 3:1, and a transparent silk protein-copper ion complex nanoparticle solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 150 μM.

[0069] (3) The silk protein-copper ion complex nanoparticle solution is centrifuged for 60 minutes at a centrifugal rate of 1500 rpm and a centrifugal temperature of 40°C. The supernatant is sealed and placed at 60°C for 48 hours to transform the uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-copper ion complex transparent nanogel.

[0070] Comparative Example 1

[0071] A method for preparing a silk protein-copper ion complex gel comprises the following steps:

[0072] (1) A high-crystalline silk fiber gel containing 2 wt% silk protein was subjected to ultrasonic treatment at a power of 650 W for 30 min to obtain a silk protein nanoparticle solution with a size of about 2 μm.

[0073] (2) The copper chloride aqueous solution was added dropwise to the silk protein nanoparticle solution at a stirring rate of 200 rpm, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution was 1:1, and a silk protein-copper ion complex solution was obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution was 1500 μM.

[0074] (3) The silk protein-copper ion complex solution was centrifuged for 30 minutes at a centrifugal speed of 1000 rpm and a centrifugal temperature of 40° C. The supernatant was sealed and placed at 60° C. for 24 hours to obtain a silk protein-copper ion complex gel.

[0075] Figure 2 The macroscopic and electron microscopic images of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex gel prepared in Comparative Example 1 are shown. Figure 2 It can be observed that Example 1 prepares a transparent gel, in which the size of the silk protein-copper ion complex is about 100 nm, and is dispersed and fixed by the nanofiber network; Comparative Example 1 prepares an opaque gel, in which the silk protein-copper ion complex forms aggregates of micron size, whose specific morphology cannot be seen, and after the silk protein-copper ion complex forms aggregates, it is impossible to disperse them thoroughly.

[0076] Comparative Example 2

[0077] A method for preparing a silk protein-copper ion complex gel comprises the following steps:

[0078] (1) A high-crystalline silk protein fiber gel containing 2 wt% silk protein was subjected to ultrasonic treatment at a power of 650 W for 30 min to obtain a silk protein nanoparticle solution with a size of about 100 nm.

[0079] (2) The copper chloride aqueous solution is directly added dropwise to the silk protein nanoparticle solution without stirring, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution is 3:1, and a silk protein-copper ion complex solution is obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution is 500 μM.

[0080] (3) The silk protein-copper ion complex solution was centrifuged for 30 minutes at a centrifugal speed of 1000 rpm and a centrifugal temperature of 40° C. The supernatant was sealed and placed at 60° C. for 24 hours to obtain a silk protein-copper ion complex gel.

[0081] Figure 3 The macroscopic image and particle size image of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex gel prepared in Comparative Examples 1 and 2. Figure 3 It can be observed that the particle size of Example 1 is 78.8nm, and the macroscopic image is a transparent gel. The aggregate size of Comparative Example 1 is 2300nm, and the macroscopic image is an opaque gel. The aggregate size of Comparative Example 2 is about 342nm, and the macroscopic image is a solution with irregular block gel.

[0082] Comparative Example 3

[0083] A method for preparing a silk protein-metal ion complex transparent solution comprises the following steps:

[0084] (1) A high-crystalline silk protein fiber gel containing 2 wt% silk protein was subjected to ultrasonic treatment at a power of 650 W for 30 min to obtain a silk protein nanoparticle solution with a size of about 100 nm.

[0085] (2) The copper chloride aqueous solution is directly added dropwise to the silk protein nanoparticle solution without stirring, the volume ratio of the silk protein nanoparticle solution to the copper chloride aqueous solution is 3:1, and a silk protein-copper ion complex solution is obtained. The concentration of copper ions in the silk protein-copper ion complex nanoparticle solution is 500 μM.

[0086] (3) The silk protein-copper ion complex solution was centrifuged for 30 minutes at a centrifugal speed of 1000 rpm and a centrifugal temperature of 40° C. The supernatant was temporarily stored at 4° C. to obtain a transparent silk protein-metal ion complex solution.

[0087] Figure 4 The macroscopic images are of the silk protein-metal ion complex transparent nanogel prepared in Example 1 and the silk protein-metal ion complex transparent solution prepared in Comparative Example 3. Figure 4 It can be observed that the comparative example 3 is still in a transparent solution state without active induction of the aging process, while the example 1 forms a transparent gel after the aging process.

[0088] The silk protein-copper ion complex transparent nanogel prepared in Example 1 was added into water and shaken, and the obtained silk protein-copper ion complex nanoparticle solution was subjected to the following tests.

[0089] Cytocompatibility testing

[0090] The cell compatibility tests were carried out on silk protein-copper ion complex nanoparticle solutions with different copper ion concentrations and copper chloride aqueous solutions.

[0091] The test method is: physiological saline, silk protein solution, silk protein-copper ion complex nanoparticle solution with copper ion concentration of 150μM, 300μM, 600μM, and copper chloride aqueous solution were diluted three times with cell culture medium to obtain mixed culture medium with copper ion concentration of 0, 50μM, 100μM, and 200μM (normal saline group (Control), silk protein group (SNF), silk protein-copper ion complex group (SCu-50, SCu-100, SCu-200), copper chloride group (Cu-50, Cu-100, Cu-200) as the control group). The mixed culture medium was used to co-culture with human umbilical vein endothelial cells and bone marrow mesenchymal stem cells, respectively, and the cell seeding density was 5×10 4 CCK-8Kit was used to detect cell activity at different time points.

[0092] The test results are as follows Figure 5As shown, a is human umbilical vein endothelial cells, b is bone marrow mesenchymal stem cells, when the copper ion concentration is 50 μM and 100 μM, free copper ions have obvious cytotoxicity, while silk protein-copper ion complex nanoparticles still maintain excellent cell compatibility.

[0093] Antimicrobial testing

[0094] The antibacterial properties of silk protein-copper ion complex nanoparticle solutions and copper chloride aqueous solutions with different copper ion concentrations were tested.

[0095] The test method is as follows: the silk protein solution, the free copper ion solution with a copper ion concentration of 150 μM, 300 μM, and 600 μM, and the silk protein-copper ion complex nanoparticle solution are diluted three times with normal saline to obtain mixed culture solutions with copper ion concentrations of 0, 50 μM, 100 μM, and 200 μM (normal saline group (Control), silk protein group (SNF), silk protein-copper ion complex group (SCu-50, SCu-100, SCu-200), and copper chloride group (Cu-50, Cu-100, Cu-200)). The mixed culture solution is diluted with 2×10 6 CFU / mL of Escherichia coli and Staphylococcus aureus were co-cultured for 24 hours. After the culture was completed, the bacterial solution was diluted 100 times and spread on solid agar medium, and photographed and counted after 24 hours of culture.

[0096] The test results are as follows Figure 6 As shown, Figure 6 This is the test result of co-culturing silk protein-copper ion complex nanoparticle solution and copper chloride aqueous solution with Staphylococcus aureus and Escherichia coli, where a is Staphylococcus aureus and b is Escherichia coli. It can be seen from the figure that both silk protein-copper ion complex nanoparticles and free copper ions show good antibacterial properties.

[0097] Tests of angiogenesis-promoting and inflammation-suppressing abilities

[0098] The angiogenesis-promoting and inflammation-inhibiting abilities of silk protein-copper ion complex nanoparticle solutions, copper chloride aqueous solutions and blue copper peptide solutions with different copper ion concentrations were tested.

[0099] The test method is: physiological saline, silk protein solution, silk protein-copper ion complex nanoparticle solution with copper ion concentration of 150μM and 300μM, and blue copper peptide solution with copper ion concentration of 300μM were diluted three times with cell culture medium to obtain mixed culture medium with copper ion concentration of 0, 50μM, 100μM and 200μM (physiological saline group (Control), silk protein group (SNF), silk protein-copper ion complex group (SCu-50, SCu-100), blue copper peptide group (GHK-Cu-100)). The mixed culture medium was used to co-culture with human umbilical vein endothelial cells and macrophages, respectively, and the cell seeding density was 2×10 5 / mL, macrophages were induced to react with inflammatory response for 12h using cell culture medium containing 100ng / mL LPS before co-culture. After three days of co-culture with human umbilical vein endothelial cells, the cell culture supernatant was collected, and the factor content in the cell culture supernatant was detected using ELISA Kit for detecting VEGF; after 24h of co-culture with macrophages, the cell culture supernatant was collected, and the factor content in the cell culture supernatant was detected using ELISA Kit for detecting TNF-α, IL-6 and IL-10 respectively.

[0100] The test results are as follows Figure 7 As shown, a is vascular endothelial growth factor VEGF, b is pro-inflammatory factor TNF-α, c is anti-inflammatory factor IL-10, and d is pro-inflammatory factor IL-6. When the copper ion concentration is 100 μM, compared with free copper ions, silk protein and copper ion complex nanoparticles show better pro-angiogenesis ability and inflammation inhibition ability.

[0101] Activity test

[0102] The activity of silk protein-copper ion complex nanoparticle solutions with different copper ion concentrations, copper chloride aqueous solutions and blue copper peptide solutions were tested.

[0103] The test method is as follows: After placing the silk protein-copper ion complex nanoparticle solution and the blue copper peptide solution with a copper ion concentration of 300μM at 90℃ for 9h, they were diluted three times with cell culture medium to obtain mixed culture medium with different copper ion concentrations (silk protein-copper ion complex group (SCu-100-90℃), blue copper peptide group (GHK-Cu-100-90℃)). The mixed culture medium was co-cultured with human umbilical vein endothelial cells and macrophages respectively, and the cell seeding density was 2×10 5 / mL, macrophages were induced to react with inflammatory response for 12h using cell culture medium containing 100ng / mL LPS before co-culture. After three days of co-culture with human umbilical vein endothelial cells, the cell culture supernatant was collected, and the factor content in the cell culture supernatant was detected using ELISA Kit for detecting VEGF; after 24h of co-culture with macrophages, the cell culture supernatant was collected, and the factor content in the cell culture supernatant was detected using ELISA Kit for detecting TNF-α, IL-6 and IL-10 respectively.

[0104] The test results are as follows Figure 7 As shown, after 9 hours of treatment, the ability of blue copper peptide to promote cell angiogenesis and regulate inflammation decreased significantly, while the biological activity of silk protein-copper ion complex nanoparticles remained unchanged, maintaining good angiogenesis and regulating inflammation properties.

[0105] Compared with the test results of blue copper peptide, it can be seen that after temperature treatment, the activity of blue copper peptide decreased, while the silk protein and copper ion complex nanoparticles still maintained their activity.

[0106] Compatibility test

[0107] The compatibility of silk protein-copper ion complex nanoparticle solution and blue copper peptide solution was tested.

[0108] The test method is: add vitamin C powder and carbomer to the blue copper peptide solution with the same copper ion concentration and the silk protein-copper ion complex nanoparticle solution prepared in Example 1, respectively, shake evenly and then take photos for observation.

[0109] The test results are as follows Figure 8 As shown, the color of the blue copper peptide solution changed from blue to light yellow after vitamin C was added, and blue substance precipitated after carbomer was added, while the silk protein-copper ion complex nanoparticle solution had no precipitation and color change.

[0110] The present invention discloses a silk protein-metal ion complex nanoparticle transparent gel with high stability and good biological activity and a preparation method thereof. The complexation rate of the silk protein-metal ion complex is controlled by adjusting the nanometer size of the silk protein aggregate and the ion concentration of the metal ion solution to avoid the direct formation of an opaque gel; and then, through a aging process, the uncomplexed silk protein nanoparticles in the system are further induced to transform into a nanofiber network to achieve long-term stable dispersion of the complex nanoparticles. The silk protein-metal ion complex nanoparticle transparent gel prepared by the present invention has no significant free metal ion precipitation, achieves the unity of biological activity, water dispersibility and stability, has multiple biological activities, and can be compatible with different active ingredients, which is conducive to direct addition in functional skin care products and flexible compatibility with other active ingredients.

[0111] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a silk protein-metal ion complex transparent nanogel, characterized in that: The following steps are involved: (1) treating a silk protein fiber gel containing 0.2 to 6 wt% of silk protein by ultrasonic treatment to obtain a silk protein nanofiber or particle solution having a diameter of 10 to 1200 nm; (2) mixing the metal salt aqueous solution with the silk protein nanofiber or particle solution obtained in step (1) at a stirring rate of 200 to 700 rpm to obtain a silk protein-metal ion complex nanoparticle solution, wherein the concentration of metal ions in the silk protein-metal ion complex nanoparticle solution is 10 to 1000 μM; (3) The silk protein-metal ion complex nanoparticle solution obtained in step (2) is centrifuged, and the supernatant is subjected to a aging treatment to convert uncomplexed silk protein nanofibers or particles into a silk protein nanofiber network to obtain a silk protein-metal ion complex transparent nanogel.

2. The preparation method according to claim 1, characterized in that: The volume ratio of the silk protein nanofiber or particle solution in step (1) to the metal salt aqueous solution in step (2) is (1-50):

1.

3. The preparation method according to claim 1, characterized in that: In step (2), the metal ions are one or more of copper ions, zinc ions, iron ions, magnesium ions, manganese ions and calcium ions.

4. The preparation method according to claim 1, characterized in that: In step (2), the particle size of the silk protein-metal ion complex nanoparticles is below 200 nm.

5. The preparation method according to claim 1, characterized in that: In step (3), the centrifugal treatment is carried out at a centrifugal rate of 1000 to 9000 rpm.

6. The preparation method according to claim 1, characterized in that: In step (3), the temperature of the centrifugal treatment is 0 to 90°C.

7. The preparation method according to claim 1, characterized in that: In step (3), the temperature of the aging treatment is 0 to 100°C.

8. A silk protein-metal ion complex transparent nanogel prepared according to the method according to any one of claims 1 to 7.

9. The silk protein-metal ion complex transparent nanogel according to claim 8, characterized in that: The silk protein-metal ion complex nanoparticles are dispersed in the silk protein-metal ion complex transparent nanogel and fixed by the silk protein nanofiber network.

10. Use of the silk protein-metal ion complex transparent nanogel according to claim 8 or 9 in preparing functional skin care products.