Gel-state polybenzimidazole ionic solvent membrane with double-crosslinking cation network structure, preparation method of gel-state polybenzimidazole ionic solvent membrane and application of gel-state polybenzimidazole ionic solvent membrane in hydrogen production by alkaline electrolysis of water
Through PPA solution-gel phase conversion and nucleophilic substitution reaction, a gel PBI ion solvent film with a double crosslinked cationic network structure was prepared, which solved the problem of poor ion conduction ability of traditional membranes under low concentration alkaline liquid, and achieved the High conductivity and excellent electrolytic properties, suitable for alkaline electrolytic water production.
Patent Information
- Application Number
- CN202411106921.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The traditional casting method prepares ion solvent films with poor ion conduction capacity and limited alkali absorption capacity under low concentration alkali liquid, which limits the performance of hydrogen production by electrolyzing water.
The gel PBI membrane was prepared by the PPA solution-gel phase conversion process. Through nucleophilic substitution and in-situ radical polymerization, cationic groups were introduced to form a PBI ion solvent membrane with a double crosslinked cationic network structure, and the alkaline was Doping in liquid to improve conductivity and stability.
The ion conductivity and electrolytic performance are significantly improved under low concentration alkali liquid, the electrolytic performance is improved, and it has shown excellent application prospects in the field of alkaline electrolytic hydrogen production.
Smart Images

Figure CN118988016A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ion solvent membrane that can be used in the field of hydrogen production by water electrolysis, and in particular to a gel-state polybenzimidazole (PBI) ion solvent membrane with a double cross-linked cationic network structure, a preparation method thereof, and an application in hydrogen production by alkaline water electrolysis. Background Art
[0002] Hydrogen production by water electrolysis has the advantage of zero carbon emissions and can be combined with renewable energy sources such as wind and solar energy. It is considered to be a promising technology for industrial applications. Ion exchange membrane is one of the core components for hydrogen production by water electrolysis. Excellent ion exchange membranes can ensure efficient and stable operation of water electrolysis. Ion exchange membrane is a polymer electrolyte material in which ionic functional groups are covalently bonded to the polymer backbone. These ion exchange membranes are mainly divided into two types, namely cation exchange membrane (CEM) and anion exchange membrane (AEM). Cation exchange membranes connect anionic functional groups (such as sulfonate and carboxylate) to polymers and can freely conduct cations (such as hydrogen ions, lithium, sodium, potassium, etc.). Anion exchange membranes connect cationic functional groups (such as quaternary ammonium salts, imidazolinium salts, etc.) to polymers and can freely conduct anions (such as hydroxide, chloride, carbonate ions, etc.). In addition, there are ion exchange membrane systems such as amphoteric ion exchange membranes (AIEM), bipolar membranes (BPM), and ion solvation membranes (ISM).
[0003] As a type of ion solvent membrane, polybenzimidazole (PBI) membrane has the advantages of excellent chemical stability, high mechanical strength and excellent thermal stability. It has become a promising ion conductor due to its amphoteric imidazole properties. Under acid / base doping, PBI ion solvent membrane can be used as a cation or anion conductive solid electrolyte because the imidazole structure on the polymer backbone can act as a Lewis acid or Lewis base in different media.
[0004] At present, many researchers have used PBI ion solvent membranes in the fields of liquid flow batteries and water electrolysis to produce hydrogen. In order to improve the electrolytic performance of PBI membranes in low-concentration alkaline solutions, many researchers have introduced cationic groups into the membranes, which can effectively improve the ion conductivity, thereby improving its electrolytic performance and stability. It still has excellent performance in low-concentration alkaline electrolytes. Henkensmeier et al. prepared a membrane with cationic groups by combining FAA anion membrane with m-PBI. After absorbing 25wt% (5.5MKOH), the room temperature reached 166mS cm -1 The higher ionic conductivity is 80% higher than that of m-PBI (Journal of Membrane Science 564 (2018) 653-662), indicating that the introduction of cationic groups is beneficial to improving the hydroxide conductivity of ISMs while improving the electrolytic performance.
[0005] In view of the problems of limited alkali absorption and poor ion conductivity of the traditional casting method for preparing ion solvent membranes, the present invention proposes to prepare gel-state PBI by using the phase inversion process of PPA solution-gel, subjecting it to nucleophilic substitution and in-situ free radical polymerization, and then soaking it in alkaline solution to prepare a PBI ion solvent membrane with a double cross-linked cationic network structure. The present invention combines the advantages of the porous morphology of the gel membrane with the functional structure design, introduces cationic groups, and aims to increase multiple OH - The transfer site can obtain high conductivity and high performance, and has excellent water electrolysis performance under low concentration alkali solution. It can be applied to the field of water electrolysis to produce hydrogen and has good application prospects. Summary of the invention
[0006] In order to overcome the deficiencies of the prior art, the present invention provides a gel-state polybenzimidazole (PBI) ion solvent membrane with a double cross-linked cationic network structure and a preparation method thereof, as well as an application of the membrane in hydrogen production by alkaline water electrolysis.
[0007] The technical solution of the present invention is as follows:
[0008] A gel-state polybenzimidazole ion solvent membrane with a double cross-linked cationic network structure, comprising polybenzimidazole, hydroxide ions (OH - , so that the charge is balanced), ionic solvents;
[0009] in,
[0010] The structural formula of the double cross-linked cationic network polybenzimidazole is as follows:
[0011]
[0012] Wherein, x=1-3, y=0-3, z=1-4, n=350-400;
[0013] The ionic solvent is an alkaline solution, for example, one or more of a potassium hydroxide solution and a sodium hydroxide solution.
[0014] The gel-state polybenzimidazole ion solvent membrane with a double cross-linked cationic network structure of the present invention has a network porous structure in cross section and a wrinkled shape in the plane.
[0015] The preparation process of the gel-state polybenzimidazole ion solvent membrane with a double cross-linked cationic network structure of the present invention comprises: using polyphosphoric acid (PPA) as a solvent, directly carrying out a PBI polycondensation reaction of tetraamine and carboxylic acid monomers under a nitrogen atmosphere, obtaining a phosphoric acid-doped gel-state PBI membrane through a solution-gel phase inversion process, then removing the phosphoric acid in the membrane, carrying out a nucleophilic substitution reaction with a halogenated olefin, and then carrying out a free radical polymerization reaction with an imidazole salt containing a diene group, and finally soaking in an alkali solution to obtain the ion solvent membrane.
[0016] Specifically, a method for preparing a gel-state polybenzimidazole ion solvent membrane having a double cross-linked cationic network structure comprises the following steps:
[0017] Step 1: Under an inert atmosphere, tetraamine, carboxylic acid monomer and polyphosphoric acid are mixed, stirred and heated to 120-200° C. for condensation reaction for 18-24 hours to obtain a polybenzimidazole solution;
[0018] The tetraamine is an aromatic tetraamine and its derivatives, selected from one or more of 3,3-diaminobenzidine, 1,2,4,5-tetraaminobenzene, and 3,3',4,4'-tetraaminodiphenyl ether;
[0019] The carboxylic acid monomer is selected from one or more of 2-hydroxyterephthalic acid, 2,5-dihydroxyterephthalic acid, 5-hydroxyisophthalic acid, 4,6-dihydroxyisophthalic acid, terephthalic acid, isophthalic acid, and trimesic acid;
[0020] Polyphosphoric acid is used as a reaction solvent, preferably, after tetraamine, carboxylic acid monomer and polyphosphoric acid are mixed, the total mass fraction of monomers (tetraamine and carboxylic acid monomer) is 1 to 15 wt%;
[0021] Step 2: Scrape the polybenzimidazole solution obtained in step 1 onto a glass substrate to complete the phase transformation from the solution to the gel state, thereby obtaining a phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane;
[0022] Preferably, the thickness of the polybenzimidazole solution applied on the glass substrate is 20 to 500 μm;
[0023] The temperature of the phase conversion process is 0-80°C and the relative humidity is 40-100%;
[0024] Step 3: Soak the phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane obtained in step 2 in deionized water until it becomes neutral, so as to remove the phosphoric acid doped in the membrane;
[0025] Soaking in deionized water was carried out at room temperature for ≥ 2 days, and the water was changed every 24 hours;
[0026] Step 4: Mix the polybenzimidazole gel ion solvent membrane treated in step 3 with a solution containing halogenated olefins, perform nucleophilic substitution reaction at 60-90° C. for 12-24 hours, and prepare a polybenzimidazole gel ion solvent membrane with side-chain grafted olefins after cleaning;
[0027] The concentration of the solution containing the halogenated olefin is 0.05-0.5 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, deionized water, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0028] The halogenated olefin is selected from one or more of 3-bromopropylene, 3-chloropropylene, 4-bromobutylene, 4-chlorobutylene, 5-bromopentene and 5-chloropentene;
[0029] After the reaction is completed, the membrane material is cleaned with solvent and deionized water;
[0030] Step 5: The polybenzimidazole gel-type ion solvent membrane with side-chain grafted olefins obtained in step 4 is subjected to a free radical polymerization reaction at 60-80° C. for 20-30 hours under the action of an initiator, and then the membrane is cleaned and soaked in an alkaline solution to obtain the gel-state polybenzimidazole ion solvent membrane with a double cross-linked cationic network structure;
[0031] The concentration of the imidazole salt solution containing diene groups is 0.05-0.5 mol / L, and the solvent is one or more of ethanol, methanol, deionized water, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0032] The general structural formula of the imidazole salt containing a diene group is as follows:
[0033]
[0034] Wherein, X is Cl or Br; y=0-3, z=1-4;
[0035] Specifically, the imidazole salt containing a diene group is selected from: one or more of 1-allyl-3-vinylimidazole chloride, 1-allyl-3-vinylimidazole bromide, 1-allyl-3-allyl imidazole chloride, 1-allyl-3-allyl imidazole bromide, 1-allyl-hexyl-3-vinylimidazole chloride, 1-allyl-hexyl-3-vinylimidazole bromide, 1-allyl-3-vinylimidazole chloride, 1-allyl-3-vinylimidazole bromide, etc.;
[0036] The initiator is azobisisobutyronitrile, and its content is 1-4% based on the total mass of the reaction materials;
[0037] After the free radical polymerization reaction is completed, the membrane product is cleaned with N,N-dimethylacetamide, ethanol, and deionized water;
[0038] The alkali solution is one or more of potassium hydroxide solution and sodium hydroxide solution, and the concentration of the alkali solution is 0.5-6 mol / L; the immersion in the alkali solution is carried out at room temperature, and the immersion time is ≥48h; after immersion in the alkali solution, the halogen anions from the imidazole salt in the polymer membrane are exchanged into OH - .
[0039] The gel-state polybenzimidazole ion solvent membrane with a double-crosslinked cationic network structure of the present invention can be used for hydrogen production by alkaline water electrolysis.
[0040] The technical principles of the present invention include:
[0041] First, a gel-state PBI is prepared by a phase inversion process of a PPA solution-gel, and then nucleophilic substitution and in-situ free radical polymerization are performed on it, and then a PBI ion solvent membrane with a double cross-linked cationic network structure is prepared after being doped with an alkaline solution. The ion solvent membrane prepared by the present invention combines the advantages of the porous morphology of the three-dimensional network of the gel membrane with the imidazole cationic group to obtain additional transmission sites arranged continuously over a long range to improve the ion conductivity. In the case of low alkali solution, a relatively high ion conductivity is still maintained, the electrolysis performance is further improved, and it is beneficial to strengthen the dimensional stability of the membrane, and has good application prospects in the field of hydrogen production by alkaline water electrolysis.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The gel-state PBI ion solvent membrane (doped with alkali) with a double cross-linked cationic network structure obtained by the present invention has high ion conductivity and high performance, and has excellent water electrolysis performance under low concentration alkali solution, which is expected to contribute to the application of alkaline water electrolysis to produce hydrogen.
[0044] (2) The ionic conductivity of the ionic solvent membrane (doped with 1 M KOH) at 25° C. is increased from 0.137 S / cm to 0.146 S / cm.
[0045] (3) The ionic solvent membrane (doped with 1M KOH) also exhibited excellent performance in a water electrolysis hydrogen production cell. At 1M KOH and 60°C, the current density reached 1.96 A / cm 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 : Infrared analysis spectra of the gel-state PBI ion solvent membrane in the comparative example and the embodiment.
[0047] Figure 2 : Mechanical properties diagram of comparative example and example PBI ion solvent membrane; (right: 1M KOH solution doped, left: undoped).
[0048] Figure 3 : SEM images of PBI ion solvent membranes of comparative example and embodiment.
[0049] Figure 4 : Ionic conductivity of PBI ion solvent membrane (doped with 1M KOH solution) in comparative example and example.
[0050] Figure 5 : Ionic conductivity and current density at 2V of PBI ion solvent membrane (doped with 1M KOH solution) of comparative examples and examples.
[0051] Figure 6 : Polarization curves of hydrogen production by water electrolysis of gel-state PBI ion solvent membrane (doped with 1M KOH solution) at 60°C in comparative examples and embodiments; (electrode: anode nickel iron, cathode platinum carbon).
[0052] Figure 7 : Polarization curves of hydrogen production by water electrolysis of gel-state PBI ion solvent membrane (doped with 1M KOH solution) in comparative examples and embodiments at 60°C; (electrode: anode nickel-iron, cathode Raney nickel). DETAILED DESCRIPTION
[0053] For ease of understanding of the present invention, the present invention will be more fully described in conjunction with the following examples. However, the present invention can be implemented in many different forms, and protection scope is not limited to the embodiments described herein. In addition, for those skilled in the art, without departing from the essence and scope of the present invention, the various modifications or improvements of the material composition and the dosage in these embodiments all belong to the scope of protection claimed in the present invention.
[0054] Comparative Example 1:
[0055] The m-PBI (commercial membrane) provided by PBIPerformance, USA, was used to prepare the ion solvent membrane. The specific steps are as follows: the m-PBI (commercial membrane) was soaked in acid (such as 85% phosphoric acid) or alkali (such as 1M KOH) and treated at 25°C for 48 hours to prepare the m-PBI ion solvent membrane.
[0056] The m-PBI ion solvent membrane (doped with 1M KOH) obtained in Comparative Example 1 was analyzed and tested:
[0057] Alkali absorption rate: 10wt%; ion conductivity: 0.086S / cm@25℃.
[0058] Comparative Example 2:
[0059] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0060] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition, i.e., an initial PA / PBI gel membrane;
[0061] The gel-state PBI ion solvent membrane (doped with 1M KOH) obtained in Comparative Example 2 was analyzed and tested:
[0062] Alkali absorption rate: 110wt%; ion conductivity: 0.137S / cm@25℃.
[0063] Embodiment 1:
[0064] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0065] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0066] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a modified solution with a concentration of 0.1 mol / L (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 1M KOH for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0067] The gel-state PBI ion solvent membrane (doped with 1M KOH) having a double cross-linked cationic network structure obtained in Example 1 was analyzed and tested:
[0068] Alkali absorption rate: 61wt%; ion conductivity: 0.140S / cm@25℃.
[0069] Embodiment 2:
[0070] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0071] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0072] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L 3-bromopropylene solution (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.2 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 1M KOH for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0073] The gel-state PBI ion solvent membrane (doped with 1M KOH) having a double cross-linked cationic network structure obtained in Example 2 was analyzed and tested:
[0074] Alkali absorption rate: 53wt%; ion conductivity: 0.146S / cm@25℃.
[0075] The performance of water electrolysis and hydrogen production was tested on the gel-state PBI ion solvent membrane (doped with 1M KOH) having a double cross-linked cationic network structure obtained in Example 2:
[0076] In order to evaluate the performance of the ionic solvent membrane of Example 2 in an alkaline water electrolyzer, the obtained membrane was prepared into a membrane electrolyte assembly (MEAs, anode: nickel iron, cathode: Raney nickel / platinum carbon). A 1M KOH solution was used for electrolyte circulation and the performance test of hydrogen production by electrolysis of water was performed. Example 2 Based on the three-dimensional porous morphology of the gel-state ionic solvent membrane, imidazolium cations were introduced, which can form a cross-linked network by themselves and can also form a cross-linked network with the main chain of polybenzimidazole PBI. The constructed double cross-linked network increases the OH - The transport sites can achieve higher ion conductivity and better performance at lower alkali concentrations.
[0077] The results are as follows Figure 6 , Figure 7 As shown, at 60°C, 1M KOH (anode nickel iron and cathode platinum carbon), Example 2 can reach 1.96A / cm at 2.05V. 2 , the performance is improved by 19.6% compared with comparative example 2. At 60°C, 1M KOH (anode nickel iron and cathode Raney nickel), at 2V, example 2 can reach 0.65A / cm 2 , relative to Comparative Example 2 (0.53A / cm 2 ), the performance is improved by 22.6%. It can be seen that the performance of Example 2 is better than that of Comparative Example 2 under low alkali solution.
[0078] Embodiment 3:
[0079] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0080] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0081] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.3 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 1M KOH for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0082] The gel-state PBI ion solvent membrane (doped with 1M KOH) having a double cross-linked cationic network structure obtained in Example 3 was analyzed and tested:
[0083] Alkali absorption rate: 43wt%.
[0084] Embodiment 4:
[0085] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0086] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0087] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.4 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 1M KOH for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0088] Embodiment 5:
[0089] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0090] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0091] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.1 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 0.5-3 mol / L sulfuric acid for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0092] Embodiment 6:
[0093] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0094] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 mm. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0095] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L 3-bromopropylene solution (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.2 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 0.5-3 mol / L sulfuric acid for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0096] Embodiment 7:
[0097] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) into a three-necked reaction bottle equipped with a mechanical stirrer, use 160 mL of polyphosphoric acid as solvent, the monomer content is 3 wt%, and react at 190° C. for 24 h under the protection of nitrogen flow to obtain a polymer solution;
[0098] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, with a scraping thickness of 0.254 μm. Since polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a PA / PBI gel ion solvent membrane is prepared through a solution-gel phase transition;
[0099] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.3 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinking agent and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 0.5-3 mol / L sulfuric acid for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0100] Embodiment 8:
[0101] (1) Weigh 3,3'-diaminobenzidine, 2,5-dihydroxyterephthalic acid, and trimesic acid respectively, pour them into a three-mouth reaction kettle, and then add a solvent and a polycondensation agent, polyphosphoric acid, into the reaction kettle. The ratio of 2,5-dihydroxyterephthalic acid to trimesic acid monomers is 100 / 10, react under a nitrogen atmosphere, and use an oil bath heating method to program the temperature to 190°C for more than 15 hours.
[0102] (2) pouring the polymer solution onto a glass substrate, using a film scraping frame to scrape the film, and controlling the thickness of the cast film to be 250 μm. Since the polyphosphoric acid is naturally hydrolyzed into phosphoric acid, a functional branched high-temperature ionic solvent membrane is prepared through a solution-gel phase transition;
[0103] (3) The obtained membrane was soaked in deionized water for 3 days (the water was changed every 24 hours) to remove the phosphoric acid contained in the membrane, and then a 0.3 mol / L solution of 3-bromopropylene (the solvent was ethanol) was used for nucleophilic reaction at 70°C for 24 hours. After being cleaned with ethanol, a 0.3 mol / L modified solution (1-allyl-3-vinyl-imidazole chloride as a crosslinker and N,N-dimethylacetamide as a solvent) was used to heat the membrane to 60°C under nitrogen flow conditions, and then 4% initiator (azobisisobutyronitrile) was added, and the temperature was raised to 70°C and reacted for 24 hours. Finally, after the reaction was completed, the membrane was washed with N,N-dimethylacetamide, ethanol, and deionized water, and then soaked in 85% phosphoric acid for 48 hours to obtain a polybenzimidazole gel ion solvent membrane with a double cross-linked cationic network structure.
[0104] Table 1 Analysis of alkali absorption rate in some comparative examples and embodiments (doped with 1 mol / L potassium hydroxide)
[0105]
[0106] Anion exchange membrane (AEM) electrolysis of water has many advantages, but due to the fragility of its quaternary ammonium group, most AEMs have low alkali stability, which hinders its commercialization. Ion solvation membrane (ISM) can be a substitute, but high alkali concentration is required so far. The gel-state PBI ion solvent membrane with a double cross-linked cationic network structure provided by the present invention combines the advantages of the porous morphology of the three-dimensional network of the gel membrane with the cationic group to construct a double cross-linked network structure, and can obtain additional transmission sites for long-range continuous arrangement to improve ionic conductivity. In the case of low alkali concentration, it has higher ionic conductivity and electrolysis water performance. In addition, the introduction of imidazole cations can form a layer of cross-linked network by itself, and the imidazole cations can also form a cross-linked network with the polybenzimidazole PBI main chain. The formation of the double cross-linked network makes the embodiment have better dimensional stability than Comparative Example 2.
Claims
1. A gel-state polybenzimidazole ion solvent membrane having a double cross-linked cationic network structure, characterized in that: It is composed of polybenzimidazole with a double cross-linked cationic network structure, hydroxide ions, and ionic solvents; in, The structural formula of the double cross-linked cationic network polybenzimidazole is as follows: Wherein, x=1-3, y=0-3, z=1-4, n=350-400; The ionic solvent is an alkaline solution.
2. The gel-state polybenzimidazole ion solvent membrane having a double cross-linked cationic network structure as claimed in claim 1, characterized in that: The ionic solvent is one or more of potassium hydroxide solution and sodium hydroxide solution.
3. The method for preparing a gel-state polybenzimidazole ion solvent membrane having a double cross-linked cationic network structure according to claim 1, characterized in that: The following steps are involved: Step 1: Under an inert atmosphere, tetraamine, carboxylic acid monomer and polyphosphoric acid are mixed, stirred and heated to 120-200° C. for condensation reaction for 18-24 hours to obtain a polybenzimidazole solution; Tetramine is selected from one or more of 3,3-diaminobenzidine, 1,2,4,5-tetraaminobenzene, and 3,3',4,4'-tetraaminodiphenyl ether; The carboxylic acid monomer is selected from one or more of 2-hydroxyterephthalic acid, 2,5-dihydroxyterephthalic acid, 5-hydroxyisophthalic acid, 4,6-dihydroxyisophthalic acid, terephthalic acid, isophthalic acid, and trimesic acid; Step 2: Scrape the polybenzimidazole solution obtained in step 1 onto a glass substrate to complete the phase transformation from the solution to the gel state, thereby obtaining a phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane; Step 3: Soak the phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane obtained in step 2 in deionized water until it becomes neutral, so as to remove the phosphoric acid doped in the membrane; Step 4: Mix the polybenzimidazole gel ion solvent membrane treated in step 3 with a solution containing halogenated olefins, perform nucleophilic substitution reaction at 60-90° C. for 12-24 hours, and prepare a polybenzimidazole gel ion solvent membrane with side-chain grafted olefins after cleaning; The halogenated olefin is selected from one or more of 3-bromopropylene, 3-chloropropylene, 4-bromobutylene, 4-chlorobutylene, 5-bromopentene and 5-chloropentene; Step 5: The polybenzimidazole gel-type ion solvent membrane with side-chain grafted olefins obtained in step 4 is subjected to a free radical polymerization reaction at 60-80° C. for 20-30 hours under the action of an initiator, and then the membrane is cleaned and soaked in an alkaline solution to obtain the gel-state polybenzimidazole ion solvent membrane with a double cross-linked cationic network structure; The general structural formula of the imidazole salt containing a diene group is as follows: Wherein, X is Cl or Br; y=0-3, z=1-4; The initiator is azobisisobutyronitrile.
4. The preparation method according to claim 3, characterized in that: In step 1, polyphosphoric acid is used as a reaction solvent, and after tetraamine, carboxylic acid monomer and polyphosphoric acid are mixed, the total mass fraction of the monomers is 1 to 15 wt %.
5. The preparation method according to claim 3, characterized in that: In step 2, the temperature of the phase conversion process is 0-80° C. and the relative humidity is 40-100%.
6. The preparation method according to claim 3, characterized in that: In step 4, the concentration of the solution containing the halogenated olefin is 0.05-0.5 mol / L, and the solvent is one or more of ethanol, methanol, ether, carbon tetrachloride, chloroform, dichloromethane, deionized water, N,N-dimethylformamide, and N,N-dimethylacetamide.
7. The preparation method according to claim 3, characterized in that: In step 5, the concentration of the imidazole salt solution containing diene groups is 0.05-0.5 mol / L, and the solvent is one or more of ethanol, methanol, deionized water, N,N-dimethylformamide, and N,N-dimethylacetamide.
8. The preparation method according to claim 3, characterized in that: In step 5, the imidazole salt containing a diene group is selected from: one or more of 1-allyl-3-vinylimidazole chloride, 1-allyl-3-vinylimidazole bromide, 1-allyl-3-allyl imidazole chloride, 1-allyl-3-allyl imidazole bromide, 1-allylhexyl-3-vinylimidazole chloride, 1-allylhexyl-3-vinylimidazole bromide, 1-allyl-3-vinylimidazole chloride, 1-allyl-3-vinylimidazole bromide, etc.
9. The preparation method according to claim 3, characterized in that: In step 5, the alkali solution is one or more of potassium hydroxide solution and sodium hydroxide solution, and the concentration of the alkali solution is 0.5-6 mol / L; the immersion in the alkali solution is carried out at room temperature, and the immersion time is ≥48h.
10. Use of the gel-state polybenzimidazole ion solvent membrane having a double cross-linked cationic network structure as claimed in claim 1 in hydrogen production by alkaline water electrolysis.
Citation Information
Patent Citations
Physical phase-split dynamic polymer and application thereof
CN108342049A
Side chain type polyphenylene oxide containing benzimidazole structure, preparation method of side chain type polyphenylene oxide and homogeneous anion exchange membrane
CN112409593A
Quaternized polybenzimidazole gel type proton exchange membrane with high proton conductivity and stability and preparation method of quaternized polybenzimidazole gel type proton exchange membrane
CN115224333A
High-temperature proton exchange membrane for fuel cell and preparation method of high-temperature proton exchange membrane
CN118063709A
Combined material system for ion exchange membranes and their use in electrochemical processes
US20170114196A1
Cited By
Preparation method of low-salt permeable bipolar membrane
CN119258795A